Preparation method of fluorodiene hyperbranched modified perfluoroether elastomer composition

Through the superbranching modification technology of non-conjugated fluorodiolefins and CO2 devolatilization and end group passivation methods, the problem of fluoropolymer molecular weight control and insufficient mechanical properties was solved, and perfluoroethers that are resistant to high-temperature superheated water vapor were prepared. Elastomer composition, suitable for semiconductor processes.

CN118931075APending Publication Date: 2024-11-12SHANGHAI MORISEAL NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411087661.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Due to the coupling termination of free radical polymerization reaction and high C-F bond energy, existing fluoropolymers have difficulty in controlling the molecular weight and molecular weight distribution, and the mechanical properties of peroxide vulcanized fluoroelastomers and the high temperature superheated water vapor resistance are insufficient. It cannot meet the harsh needs of semiconductor processes.

Method used

The perfluoroelastomer preparation method is prepared by the hyperbranched and modified non-conjugated fluorodiolefins. It is prepared by emulsion polymerization, co-aggregation, mixing thin-through and molding, combined with CO2 devolatilization and end group passivation technology. Perfluoroelastic elastomer composition with high temperature superheated water vapor and low compression permanent deformation.

Benefits of technology

The perfluoroelastic elastomer composition has achieved high temperature superheated water vapor resistance and low compression permanent deformation characteristics, solved the problem of poor stability of end groups, and is suitable for harsh semiconductor processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931075A_ABST
    Figure CN118931075A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a fluorodiene hyperbranched modified perfluoroether elastomer composition, and belongs to the field of fluoroelastomers. The preparation method specifically comprises the following steps: carrying out emulsion polymerization on tetrafluoroethylene, perfluoroalkyl vinyl ether, a chain transfer agent, a peroxide initiator and non-conjugated fluorine diene serving as a vulcanization point monomer to obtain hyperbranched perfluoroether elastomer emulsion; the perfluoroether elastomer emulsion and the PFA emulsion are subjected to coprecipitation condensation, washing, drying devolatilization and end group passivation, and perfluoroether elastomer micro powder is obtained; mixing and thin-passing the perfluoroether elastomer micro powder with a filling agent, an acid acceptor and a vulcanizing agent at 60-90 DEG C to obtain perfluoroether elastomer mixed rubber; and carrying out compression molding on the perfluoroether elastomer rubber compound, and carrying out secondary vulcanization to obtain the hyperbranched modified perfluoroether elastomer composition. The perfluoroether elastomer composition obtained by the treatment scheme of the application can resist high-temperature superheated water vapor (gas), and has low compression set and low gas permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluoroelastomers, and in particular to a method for preparing a fluorodiene hyperbranched modified perfluoroether elastomer composition. Background Art

[0002] Fluorine-containing polymers obtained by free radical polymerization are very difficult to control in terms of molecular weight and molecular weight distribution due to the coupling termination and disproportionation termination of free radicals. At the same time, the high CF bond energy prevents the branching reaction of the polymer chain, so fluorine-containing polymers with high fluorine content are basically linear. Although linear polymers can provide better fluidity and physical properties in many occasions, polymers with complex chain structures such as star and block copolymers are more competitive in the market because they can provide other excellent properties.

[0003] Previous peroxide-cured fluoroelastomers were obtained by introducing "vulcanization point" monomers that are susceptible to free radical attack into macromolecules. For example, for peroxide vulcanization systems, the bond energy of the CI bond is low, and the iodine at the end of the polymer chain can be used to vulcanize the elastomer. It is worth noting that the mechanical stability of the cross-linked network is related to the number of end groups on the macromolecule. The greater the number, the better the mechanical properties of the cross-linked network. When this type of "vulcanization point" monomer technology is used, the number of end groups on each macromolecule chain is less than 2, and the resulting vulcanized rubber is relatively poor in mechanical properties, compression permanent deformation, or tolerance to high-temperature superheated water steam (gas), which cannot meet the demanding requirements of semiconductor processes for the performance of fluoroelastomer vulcanized rubber.

[0004] Based on this, a new technical solution is needed. Summary of the invention

[0005] Therefore, in order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a method for preparing a hyperbranched fluorodiolefin modified perfluoroether elastomer composition, which has the properties of resistance to high-temperature superheated water vapor (gas), low compression set and low gas permeability.

[0006] In order to achieve the above-mentioned object, the present invention provides a method for preparing a fluorodienes hyperbranched modified perfluoroether elastomer composition, comprising: S1, subjecting 43-68% by mass of tetrafluoroethylene, 30-55% of perfluoroalkyl vinyl ether, 0.05-0.85% of chain transfer agent, 0.3-0.5% of peroxy initiator and 1-2% of non-conjugated fluorodienes as vulcanization point monomers to emulsion polymerization to obtain a hyperbranched perfluoroether elastomer emulsion; the non-conjugated fluorodienes are added continuously in stages during the polymerization process; S2, co-condensing the perfluoroether elastomer emulsion with a PFA emulsion having a solid content of 30-60%, washing, drying and devolatilizing, and end group passivation to obtain a perfluoroether elastomer micropowder; wherein the drying and devolatilization is low-temperature drying or vacuum drying followed by liquid or supercritical CO2 devolatilization treatment; S3, at 60-90 ℃, mixing 100-80% of the perfluoroether elastomer powder with 0-20% of the filler, 0-10% of the acid absorber, and 0-2% of the vulcanizer to obtain a perfluoroether elastomer rubber mix; S4, molding the perfluoroether elastomer rubber mix and performing secondary vulcanization to obtain a hyperbranched modified perfluoroether elastomer composition.

[0007] Optionally, the non-conjugated fluorodiene structure is CH2=CH-(CF2) n -CH=CH2, where n is a positive integer not less than 2.

[0008] Optionally, the chain transfer agent is at least one of CF2I2, I(CF2)6I, I(CF2)4I, CF2ClI, CF3CFICF2I.

[0009] Optionally, the perfluoroalkyl vinyl ether includes at least one of perfluoromethyl vinyl ether, perfluoroethyl vinyl ether and perfluoropropyl vinyl ether.

[0010] Optionally, in S2, the end groups are passivated by using 10% F2 in a balance gas at 30-100°C for 1-5 hours, and the balance gas is N2.

[0011] Optionally, the PFA emulsion contains 90-99 wt% tetrafluoroethylene and 1-10 wt% perfluoropropyl vinyl ether.

[0012] Optionally, the filler is at least one of PTFE micropowder, PFA micropowder, fluorinated PI powder, carbon black, or silica.

[0013] Optionally, the acid absorber is at least one of MgO, CaO, ZnO, PbO, and dibasic lead phosphite.

[0014] Optionally, the vulcanizing agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

[0015] Compared with the prior art, the advantages of the present invention are: a perfluoroether elastomer is obtained by applying a non-conjugated fluorodiolefin hyperbranching modification technology, and the prepared perfluoroether elastomer composition has the characteristics of resistance to high-temperature superheated water vapor (gas) and low compression permanent deformation; at the same time, CO2 devolatilization and end group passivation methods are further used to solve the problem of poor end group stability of the perfluoroether elastomer composition, so as to be applied to demanding semiconductor processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 The figure is a simplified flow chart of the preparation method of the fluorodiene hyperbranched modified perfluoroether elastomer composition in the embodiment of the present invention. DETAILED DESCRIPTION

[0018] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0019] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0020] It should be noted that various aspects of the embodiments within the scope of protection of the present invention are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0021] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0022] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0023] like Figure 1 As shown, the present invention provides a method for preparing a fluorodiolefin hyperbranched modified perfluoroether elastomer composition, comprising: S1. Emulsion polymerization is performed on 43-68% by mass of tetrafluoroethylene, 30-55% by mass of perfluoroalkyl vinyl ether, 0.05-0.85% by mass of chain transfer agent, 0.3-0.5% by mass of peroxide initiator and 1-2% by mass of non-conjugated fluorodiene as a vulcanization point monomer to obtain a hyperbranched perfluoroether elastomer emulsion.

[0024] Hyperbranched perfluoroether elastomer emulsion refers to the perfluoroether elastomer in the emulsion having a large number of end groups, and the end groups are easy to be chemically modified. The properties of the end groups largely determine the physical and chemical properties of the hyperbranched perfluoroether elastomer. Hyperbranched perfluoroether elastomers with different branching degrees and a large number of end groups are obtained through S1, and finally combined with devolatilization and end group passivation in S2, which can be applied in different fields.

[0025] The temperature of emulsion polymerization is 50~90 ℃.

[0026] The general mechanism of fluorinated monomer and free radical polymerization is

[0027] Hyperbranched perfluoroether elastomer emulsion polymerization is achieved by controlling the branching of the polymer chain. A very small amount of highly active fluorodiolefin is used in the reaction medium to react with the polymer chain to form a multifunctional molecule. By strictly controlling its reaction, the reaction proceeds in the desired direction. Because the fluorodiolefin is active, it can quickly and completely connect with the growing chain once added. Therefore, the number of crosslinks in the polymer depends on the number of fluorodiolefins introduced into the reaction. Preferably, the degree of branching reaction is controlled by adding in stages.

[0028] Peroxide initiators are compounds containing peroxy groups (-OO-). When heated, the -OO- bond breaks and splits into two corresponding free radicals, thereby initiating monomer polymerization. Peroxide initiators are divided into two categories: inorganic peroxides and organic peroxides. Inorganic peroxide initiators include ammonium persulfate or potassium persulfate, and organic peroxide initiators include benzoyl peroxide, tert-butyl benzoyl peroxide, methyl ethyl ketone peroxide, etc.

[0029] Non-conjugated fluorodienes refer to fluorodienes that do not have a conjugated structure, with two double bonds separated by multiple single bonds, i.e. containing -C=C-(C) n -C=C- system fluorodienes (n≥2).

[0030] S2. Co-precipitate and condense the perfluoroether elastomer emulsion with a PFA emulsion having a solid content of 30-60%, wash, dry and devolatilize, and passivate the end groups to obtain perfluoroether elastomer micropowder; wherein the drying and devolatilization is low-temperature drying or vacuum drying followed by liquid or supercritical CO2 devolatilization treatment.

[0031] PFA is a copolymer of tetrafluoroethylene and perfluoropropyl vinyl ether monomers, and the solid content of the emulsion is 30-60%. PFA emulsion can be synthesized in situ with a solid content of 25-35% or commercially available with a solid content of 40-60%. The ratio of tetrafluoroethylene to perfluoropropyl vinyl ether is 90-99:10-1 (mass fraction).

[0032] The principle of co-precipitation and coagulation of perfluoroether elastomer emulsion and PFA emulsion is as follows: Apply high shear force (mechanical stirring coagulation) to the coagulated perfluoroether elastomer emulsion and PFA emulsion or add inorganic acid such as HCl or HNO3 and stir vigorously to make the emulsion to be coagulated coprecipitate and coagulate into particles. The coagulated granulated product can also be thoroughly washed with deionized water and vacuum dried at 50-100 ℃.

[0033] There are generally two methods for end group passivation: (1) end capping with short chains or small organic molecules; (2) end capping by active polymerization grafting. When short chains or small organic molecules are used for end capping, the -COF group of the end group can react with the amine group; when active polymerization grafting is used for end capping, -COOH or -CH2OH and the -COF of the end group can react with the amine group. The present invention uses fluorination technology to achieve end group passivation. Hyperbranched perfluoroether elastomers with different branching degrees and a large number of end groups are obtained through S1, and finally combined with devolatilization and end group passivation in S2, which can be applied in different fields.

[0034] S3. Mix 100-80% by mass of perfluoroether elastomer powder, 0-20% by mass of filler, 0-10% by mass of acid absorber, and 0-2% by mass of vulcanizing agent at 60-90 °C to obtain a perfluoroether elastomer compound rubber.

[0035] Thin-pass mixing is to adjust the roller gap of the open mixing mill to 1.2-3.5 mm, allow the rubber components with the above weight percentage to pass through the roller gap, and let them fall into the receiving tray. After all the rubber has passed through the roller gap, the rubber on the tray is folded twice and then thin-passed. After a period of time, such as 40 minutes, fillers, acid absorbers and vulcanizers are added, and thin-pass mixing is continued until the surface of the mixed rubber is flat and free of particles. The total time for thin-pass mixing is about 1 hour.

[0036] S4, molding the perfluoroether elastomer mixed rubber and performing secondary vulcanization to obtain a hyperbranched modified perfluoroether elastomer composition.

[0037] The above-mentioned specific processes of emulsion polymerization, mixing and thinning, compression molding, secondary vulcanization and added vulcanizing agent are conventional processes in the industry.

[0038] The above method obtains a perfluoroether elastomer by applying a non-conjugated fluorodiolefin hyperbranching modification technology. The prepared perfluoroether elastomer composition has the characteristics of resistance to high-temperature superheated water vapor (gas) and low compression permanent deformation. At the same time, CO2 devolatilization and end group passivation methods are further used to solve the problem of poor end group stability of the perfluoroether elastomer composition, so as to be applied to demanding semiconductor processes.

[0039] In one embodiment, the non-conjugated fluorodiene structure is CH2=CH-(CF2) n -CH=CH2, where n is a positive integer not less than 2. The molecular formula is CH2=CH-(CF2) n The electron-rich double bond in -CH=CH2 ensures rapid reaction with the electron-deficient fluoropolymer growth chain, among which 1,6-divinylperfluorohexane is particularly effective in the polymerization of fluoromonomers and is easier to control.

[0040] In one embodiment, the chain transfer agent is at least one of CF2I2, I(CF2)6I, I(CF2)4I, CF2ClI, CF3CFICF2I.

[0041] In one embodiment, the perfluoroalkyl vinyl ether includes at least one of perfluoromethyl vinyl ether, perfluoroethyl vinyl ether and perfluoropropyl vinyl ether.

[0042] In one embodiment, in S2, the end group is passivated at 30-100° C. for 1-5 hr using 10% F2 in the balance gas, and the balance gas is N2. The volume ratio of F2 to the balance gas N2 is 10:90, so the volume ratio of F2 in the total gas is 10%.

[0043] In one embodiment, the content of tetrafluoroethylene in the PFA emulsion is 90-99 wt %, and the content of perfluoropropyl vinyl ether is 1-10 wt %.

[0044] In one embodiment, the filler is at least one of PTFE micropowder, PFA micropowder, fluorinated PI powder, carbon black, or silica.

[0045] In one embodiment, the acid absorber is at least one of MgO, CaO, ZnO, PbO, and dibasic lead phosphite.

[0046] In one embodiment, the vulcanizing agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane (DBPH).

[0047] Example 1 S1. 650 g (about 6.5 mol; mass fraction 54.3%) tetrafluoroethylene (MW 100.01), 520 g (about 3.1 mol; mass fraction 43.4%) perfluoromethyl vinyl ether (MW 166.02), 7.5 g (about 0.017 mol; mass fraction 0.6%) chain transfer agent 1,4-diiodooctafluorobutane I(CF2)4I (MW 453.84), 5.0 g initiator ammonium persulfate (APS, MW228.201), and 15 g (about 0.059 mol; mass fraction 1.25%) non-conjugated fluorodienes CH2=CH-(CF2)4-CH=CH2 (MW254.12) were emulsion polymerized to obtain a hyperbranched perfluoroether elastomer emulsion; the non-conjugated fluorodienes can be added in batches by a metering pump from the beginning to the end of the reaction, 1.5 g each time, for a total of 10 times. MW is molecular weight.

[0048] S2, co-precipitation and condensation with 300 ml of PFA emulsion with a solid content of about 32% (containing about 110 g of PFA), washing, drying, devolatilization and end group passivation to obtain about 895 g of perfluoroether elastomer powder.

[0049] The product was dried and devolatilized with supercritical CO2 for 4 h, and the end groups were passivated with 10% F2 (N2 as the balance gas).

[0050] S3. Mix the perfluoroether elastomer powder with 40 g of dipentadienyl vulcanizing agent at 60-90 °C to obtain a perfluoroether elastomer mixed rubber.

[0051] S4, molding the mixed rubber, performing secondary vulcanization to obtain a hyperbranched modified perfluoroether elastomer composition, and preparing it into an O-ring.

[0052] Example 2 S1, 600 g (about 6.0 mol; mass fraction 51.15%) tetrafluoroethylene (MW 100.01), 540 g (about 3.25 mol; mass fraction 46.04%) perfluoromethyl vinyl ether (MW 166.02), 10 g (about 0.022 mol; mass fraction 0.85%) chain transfer agent 1,4-diiodooctafluorobutane I(CF2)4I (MW 453.84), 5.0 g initiator ammonium persulfate (APS, MW228.201, mass fraction 0.43%), 18 g (about 0.071 mol; mass fraction 1.53%) non-conjugated fluorodiolefin CH2=CH-(CF2)4-CH=CH2 (MW 254.12) was subjected to emulsion polymerization to obtain a hyperbranched perfluoroether elastomer emulsion; non-conjugated fluorodiolefin was added in batches by a metering pump from the beginning to the end of the reaction, 1.8 g each time, for a total of 10 times.

[0053] S2, co-precipitation and condensation with 300 ml of PFA emulsion with a solid content of about 32% (containing about 110 g of PFA), washing, drying, devolatilization and end group passivation to obtain about 910 g of perfluoroether elastomer powder.

[0054] The product was dried and devolatilized by supercritical CO2 for 4 h, and the end groups were passivated by using 10% F2 (N2 as the balance gas).

[0055] S3. Mix the perfluoroether elastomer powder with 40 g of dipentadienyl vulcanizing agent at 60-90 °C to obtain a perfluoroether elastomer mixed rubber.

[0056] S4, molding the mixed rubber, performing secondary vulcanization to obtain a hyperbranched modified perfluoroether elastomer composition, and preparing it into an O-ring.

[0057] Comparative Example 1 620 g (about 6.2 mol; mass fraction 51.2%) tetrafluoroethylene (MW 100.01), 560 g (about 3.37 mol; mass fraction 46.25%) perfluoromethyl vinyl ether (MW 166.02), 12.8 g (about 0.028 mol; mass fraction 1.06%) chain transfer agent 1,4-diiodooctafluorobutane I(CF2)4I (MW 453.84), 5.0 g initiator ammonium persulfate (APS, MW 228.201), and 13 g (about 0.051 mol; mass fraction 1.07%) iodine-containing curing point monomer 3,3,4,4-tetrafluoro-4-iodobut-1-ene (MW253.92) were emulsion polymerized to obtain a perfluoroether elastomer emulsion; the curing point monomer was added in batches by a metering pump at the beginning and end of the reaction, 1.3 g each time, for a total of 10 times.

[0058] S2, co-condensed with 300 ml of PFA emulsion with a solid content of about 32% (containing about 110 g of PFA), washed, dried, devolatilized and end-group passivated to obtain about 872 g of perfluoroether elastomer powder.

[0059] The product was dried and devolatilized by supercritical CO2 for 4 h, and the end groups were passivated by using 10% F2 (N2 as the balance gas).

[0060] S3. Mix the perfluoroether elastomer powder with 40 g of dipentadienyl vulcanizing agent at 60-90 °C to obtain a perfluoroether elastomer mixed rubber.

[0061] S4, molding the mixed rubber, performing secondary vulcanization to obtain a perfluoroether elastomer composition, and preparing it into an O-ring.

[0062] Comparative Example 2 617 g (about 6.17 mol; mass fraction 51.8%) tetrafluoroethylene (MW 100.01), 543 g (about 3.27 mol; mass fraction 45.56%) perfluoromethyl vinyl ether (MW 166.02), 12.6 g (about 0.028 mol; mass fraction 1.06%) chain transfer agent 1,4-diiodooctafluorobutane I(CF2)4I (MW 453.84), 5.0 g initiator ammonium persulfate (APS, MW228.201), 14.2 g (about 0.056 mol; mass fraction 1.19%) iodine-containing curing point monomer 3,3,4,4-tetrafluoro-4-iodobut-1-ene (MW 253.92) were emulsion polymerized to obtain a perfluoroether elastomer emulsion; the curing point monomer was added in batches by a metering pump at the beginning and end of the reaction, and 1.42 g was added each time. g, 10 times in total.

[0063] S2, co-precipitation and condensation with 300 ml of PFA emulsion with a solid content of about 32% (containing about 110 g of PFA), washing, drying, devolatilization and end group passivation to obtain about 902 g of perfluoroether elastomer.

[0064] The product was dried and devolatilized by supercritical CO2 for 4 h, and the end groups were passivated by using 10% F2 (N2 as the balance gas).

[0065] S3. Mix the perfluoroether elastomer powder with 40 g of dipentadienyl vulcanizing agent at 60-90° C. to obtain a perfluoroether elastomer mixed rubber.

[0066] S4, molding the mixed rubber, performing secondary vulcanization to obtain a perfluoroether elastomer composition, and preparing it into an O-ring.

[0067] Table 1 Main test results of the examples and comparative examples of this application

[0068] *The enterprise standard is Q / SMS 004-2024 Semiconductor Equipment Perfluorinated Seals Helium Mass Spectrometry Vacuum Leak Detection Test Method, which can be obtained through the National Standard Information Public Service Platform.

[0069] The heat resistance (superheated water steam) experiment was carried out in a 500 ml PTFE-lined hydrothermal reactor, filled with 300 ml of deionized water, heated to about 95 °C, and sealed in an oven after the air was removed. The temperature was adjusted to the set temperature and kept constant for 70 h. After cooling to room temperature, the performance test was carried out.

[0070] Table 2 Heat resistance (superheated water steam) Example and comparative example test results

[0071] *Senhuan Enterprise Standard Q / SMS 002-2024 Immersion and Liquid Resistance Test Method for Perfluoroether Elastomers and Rubber Seals. This enterprise standard can be obtained through the National Standard Information Public Service Platform.

[0072] By comparing Examples 1-2 and Comparative Examples 1-2 in Tables 1 and 2, it can be seen that the present application applies the non-conjugated fluorodiolefin hyperbranching modification technology to perfluoroether elastomers, and further adopts an end group passivation method to solve the problem of poor end group stability of the perfluoroether elastomer composition. The prepared perfluoroether elastomer composition has the characteristics of resistance to high-temperature superheated water vapor (gas) and low compression permanent set, and can be applied to demanding semiconductor processes.

[0073] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a fluorodiene hyperbranched modified perfluoroether elastomer composition, characterized in that: include: S1. Emulsion polymerize 43-68% by mass of tetrafluoroethylene, 30-55% by mass of perfluoroalkyl vinyl ether, 0.05-0.85% by mass of chain transfer agent, 0.3-0.5% by mass of peroxy initiator and 1-2% by mass of non-conjugated fluorodiolefin as a vulcanization point monomer to obtain a hyperbranched perfluoroether elastomer emulsion; the non-conjugated fluorodiolefin is added continuously in stages during the polymerization process; S2, co-precipitating and condensing the perfluoroether elastomer emulsion and a PFA emulsion with a solid content of 30-60%, washing, drying and devolatilizing, and end group passivation to obtain a perfluoroether elastomer powder; wherein the drying and devolatilization is low-temperature drying or vacuum drying followed by liquid or supercritical CO2 devolatilization treatment; S3, mixing 80-100% by mass of the perfluoroether elastomer powder, 0-20% by mass of a filler, 0-10% by mass of an acid absorber, and 0-2% by mass of a vulcanizing agent at 60-90° C. to obtain a perfluoroether elastomer mixed rubber; S4, molding the perfluoroether elastomer mixed rubber and performing secondary vulcanization to obtain a hyperbranched modified perfluoroether elastomer composition.

2. The preparation method according to claim 1, characterized in that: The non-conjugated fluorodiene structure is CH2=CH-(CF2) n -CH=CH2, where n is a positive integer not less than 2.

3. The preparation method according to claim 1, characterized in that: The chain transfer agent is at least one of CF2I2, I(CF2)6I, I(CF2)4I, CF2ClI, and CF3CFICF2I.

4. The preparation method according to claim 1, characterized in that: The perfluoroalkyl vinyl ether includes at least one of perfluoromethyl vinyl ether, perfluoroethyl vinyl ether and perfluoropropyl vinyl ether.

5. The preparation method according to claim 1, characterized in that: In S2, the end groups are passivated by using 10% F2 in a balance gas at 30-100° C. for 1-5 hr, and the balance gas is N2.

6. The preparation method according to claim 1, characterized in that: The PFA emulsion has a tetrafluoroethylene content of 90-99 wt %, and a perfluoropropyl vinyl ether content of 1-10 wt %.

7. The preparation method according to claim 1, characterized in that: The filler is at least one of PTFE micropowder, PFA micropowder, fluorinated PI powder, carbon black, or silicon dioxide.

8. The preparation method according to claim 1, characterized in that: The acid absorber is at least one of MgO, CaO, ZnO, PbO and dibasic lead phosphite.

9. The preparation method according to claim 1, characterized in that: The vulcanizing agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.

Citation Information

Cited By

  • Metal plate frame and fluororubber sealing assembly and preparation method thereof

    CN119639036A

  • High-temperature-resistant perfluoroether elastomer composition and preparation method thereof

    CN120607780A

  • Fluorodiene modified perfluoroether elastomer with in-situ embedded fluorinated nano-silica and preparation method of fluorodiene modified perfluoroether elastomer

    CN120623388A

  • A fluorinated diene-modified perfluoroether elastomer with in-situ embedded fluorinated nano-silica and its preparation method