High and low temperature resistant sealing ring rubber material for engine connecting pipe and preparation method thereof
Through the combination of materials such as ethylene acrylate rubber, polyphenylene sulfide and titanium oxygen network composite, the problem of unstable performance of sealing rings in high and low temperature environments is solved, and the improvement of high mechanical strength and bonding performance is achieved. Suitable for sealing applications of engine connection pipes.
Patent Information
- Application Number
- CN202411099753.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
AI Technical Summary
The existing sealing ring materials are unstable in high and low temperature environments, and are prone to aging, cracking or hardening, resulting in seal failure and cannot meet the strict working environment requirements of the engine connection pipe.
Using a combination formula of ethylene acrylate rubber, polyphenylene sulfide, titanium oxygen network composite, plasticizer, functional additive, anti-aging agent and vulcanizing agent, sealing ring materials are prepared through plasticizing and kneading processes to form stable network structure and chemical bonds improve mechanical strength and bonding properties.
It significantly improves the high and low temperature resistance, mechanical strength and adhesive properties of the sealing ring, ensuring good sealing performance and stability in extreme environments and extends service life.
Smart Images

Figure BDA0004989049840000061 
Figure BDA0004989049840000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealing ring preparation, in particular to a sealing ring rubber material for a high and low temperature resistant engine connecting pipe and a preparation method thereof. Background Art
[0002] In recent years, with the localization of engine technology and hybrid technology, the working environment of engine connecting pipes and their seals has become more and more severe, especially under high temperature and low temperature conditions, which puts higher requirements on the performance of sealing ring materials. At present, acrylate rubber, ethylene acrylate rubber or nitrile rubber are often used as the main materials for formula design, but the comprehensive performance of each material is insufficient, resulting in unstable sealing performance; mainly reflected in the following aspects:
[0003] Although ethylene acrylate rubber has high temperature resistance, its vulcanization speed is slow and its strength is low. In addition, its mechanical properties in high and low temperature environments are not ideal, and it is prone to aging, cracking and other problems, which can also easily lead to sealing failure.
[0004] Although nitrile rubber has excellent oil resistance, its low-temperature performance is poor. It is easy to harden and lose elasticity in low-temperature environments, thus affecting the sealing effect. Summary of the invention
[0005] Technical problem to be solved: In order to overcome the above-mentioned shortcomings, a sealing ring rubber material for a high and low temperature resistant engine connecting pipe and a preparation method thereof are provided.
[0006] The technical solution is: a sealing ring rubber material for a high and low temperature resistant engine connecting pipe, comprising the following components:
[0007] Ethylene acrylic rubber (AEM): 100-120 parts;
[0008] Polyphenylene sulfide (PPS): 5-10;
[0009] Titanium oxygen network complex: 10-15 parts;
[0010] Plasticizer: 5-8 parts;
[0011] Functional additives: 3-5 parts;
[0012] Anti-aging agent: 5-10 parts;
[0013] Vulcanizing agent: 3-5 parts.
[0014] Preferably, the method for preparing the titanium oxide network composite comprises the following steps:
[0015] Mix titanate polymer and titanium oxide in a ratio of 3:1 and stir evenly;
[0016] During the stirring process, the temperature is gradually raised to 80-100°C and the reaction is maintained for 1-2 hours to allow the titanate polymer to react with the titanium oxide to form a Ti-O-Ti bond;
[0017] After the reaction was completed, the mixture was cooled to room temperature to obtain a titanium oxide network composite (TONC).
[0018] Preferably, the titanate polymer is tetrabutyl titanate; and the titanium oxide is titanium dioxide (TiO2).
[0019] Preferably, the plasticizer is dioctyl phthalate (DOP) or dioctyl sebacate (DOS).
[0020] Preferably, the functional auxiliary agent is an organic silane coupling agent, including γ-methacryloxypropyltrimethoxysilane (MEMO) or γ-cyanoethyltriethoxysilane (CETES).
[0021] Preferably, the antioxidant is one or more combinations of KY845 and ZMTI.
[0022] Preferably, the vulcanizing agent is a peroxide vulcanizing agent, including one or more combinations of 1,3-di-tert-butyl diisopropylbenzene peroxide, 1,4-di-tert-butyl diisopropylbenzene peroxide, and 1,2-di-tert-butyl diisopropylbenzene peroxide.
[0023] Based on the formula components of the sealing ring rubber material of the high and low temperature resistant engine connecting pipe, the present invention also provides a method for preparing the sealing ring rubber material of the high and low temperature resistant engine connecting pipe, comprising the following steps:
[0024] 1) Plasticizing: polyphenylene sulfide (PPS) and the titanium oxide network composite are weighed separately, mixed thoroughly and then plasticized to form ingredient A;
[0025] The ethylene acrylate rubber (AEM) is then plasticized to form ingredient B, so that ingredients A and B reach a plastic state suitable for further processing.
[0026] 2) First mixing: Put ingredients A and B into an internal mixer, start mixing, add plasticizer, functional additive, carbon black, antioxidant in sequence, continue mixing, and obtain rubber C;
[0027] The rubber compound C is discharged onto the open mixing mill for heat dissipation. After the thin pass is completed, the sheet is cooled.
[0028] 3) Second mixing: Put the rubber compound C and the vulcanizer into the internal mixer for mixing for 60-90 seconds, then continue mixing for 60-90 seconds after cleaning, and then discharge the material to the cutting machine for sheeting, thus completing the preparation of the final sealing ring rubber compound.
[0029] Beneficial effects: 1. AEM has excellent heat resistance, oil resistance and aging resistance, and is the main base material for sealing ring rubber; it provides basic elasticity and mechanical strength.
[0030] 2. PPS has high heat resistance and chemical stability, and can maintain good mechanical properties at high temperatures; the Ti-O-Ti bond formed by the reaction of titanate and titanium oxide constitutes a stable network skeleton structure; the molten polyphenylene sulfide (PPS) flows and fills into the holes and pores of this skeleton structure to form an interpenetrating polymer network; at the same time, the use of organic silane coupling agent as a functional additive can form a chemical bond between inorganic materials and organic materials, improve the bonding performance between polyphenylene sulfide and titanium oxide network composites; improve the flexibility and processing performance of the sealing ring, so that it can maintain good sealing plasticity in high and low temperature environments.
[0031] 3. The vulcanizer can form a cross-linked structure between rubber molecules, so that the mixing system of AEM, PPS and titanium oxide network compound is interwoven into a network structure. It significantly enhances the mechanical strength, heat resistance and bonding performance of the sealing ring, ensuring its stability in high and low temperature environments. DETAILED DESCRIPTION
[0032] The present invention is described in detail below with reference to specific embodiments, but is not intended to limit the present invention.
[0033] A sealing ring rubber material for a high and low temperature resistant engine connecting pipe comprises the following components:
[0034] Ethylene acrylic rubber (AEM): 100-120 parts;
[0035] Polyphenylene sulfide (PPS): 5-10;
[0036] Titanium oxygen network complex: 10-15 parts;
[0037] Plasticizer: 5-8 parts;
[0038] Functional additives: 3-5 parts;
[0039] Anti-aging agent: 5-10 parts;
[0040] Vulcanizing agent: 3-5 parts.
[0041] In a specific implementation process, the method for preparing the titanium oxide network composite comprises the following steps:
[0042] Mix titanate polymer and titanium oxide in a ratio of 3:1 and stir evenly;
[0043] During the stirring process, the temperature is gradually raised to 80-100°C and the reaction is maintained for 1-2 hours to allow the titanate polymer to react with the titanium oxide to form a Ti-O-Ti bond;
[0044] After the reaction was completed, the mixture was cooled to room temperature to obtain a titanium oxide network composite (TONC).
[0045] In a specific implementation process, the titanate polymer is tetrabutyl titanate; and the titanium oxide is titanium dioxide (TiO2).
[0046] Titanium-oxygen network composites are formed by the reaction of titanate (such as tetrabutyl titanate) and titanium oxide (such as TiO2) to form Ti-O-Ti bonds. This bonding structure is very stable at high temperatures, giving the material excellent heat resistance. Ti-O-Ti bonds form a network skeleton structure. Molten polyphenylene sulfide (PPS) flows and fills the holes and pores of this skeleton structure to form an interpenetrating polymer network.
[0047] In a specific implementation process, the plasticizer is dioctyl phthalate (DOP) or dioctyl sebacate (DOS).
[0048] In the specific implementation process, the functional additive is an organic silane coupling agent, including γ-methacryloxypropyltrimethoxysilane (MEMO) or γ-cyanoethyltriethoxysilane (CETES). These organic silane coupling agents can significantly improve the performance of the sealing ring rubber, so that it maintains excellent adhesion and stability in high and low temperature environments.
[0049] In the specific implementation process, the antioxidant is one or more combinations of KY845 and ZMTI.
[0050] In a specific implementation process, the vulcanizing agent is a peroxide vulcanizing agent, including one or more combinations of 1,3-di-tert-butyl diisopropylbenzene peroxide, 1,4-di-tert-butyl diisopropylbenzene peroxide, and 1,2-di-tert-butyl diisopropylbenzene peroxide.
[0051] Based on the formula components of the sealing ring rubber material of the high and low temperature resistant engine connecting pipe, the present invention also provides a method for preparing the sealing ring rubber material of the high and low temperature resistant engine connecting pipe, comprising the following steps:
[0052] 1) Plasticizing: polyphenylene sulfide (PPS) and the titanium oxide network composite are weighed separately, mixed thoroughly and then plasticized to form ingredient A;
[0053] The ethylene acrylate rubber (AEM) is then plasticized to form ingredient B, so that ingredients A and B reach a plastic state suitable for further processing.
[0054] 2) First mixing: Put ingredients A and B into an internal mixer, start mixing, add plasticizer, functional additive, carbon black, antioxidant in sequence, continue mixing, and obtain rubber C;
[0055] The rubber compound C is discharged onto the open mixing mill for heat dissipation. After the thin pass is completed, the sheet is cooled.
[0056] 3) Second mixing: Put the rubber compound C and the vulcanizer into the internal mixer for mixing for 60-90 seconds, then continue mixing for 60-90 seconds after cleaning, and then discharge the material to the cutting machine for sheeting, thus completing the preparation of the final sealing ring rubber compound.
[0057] Example 1
[0058] A sealing ring rubber material for a high and low temperature resistant engine connecting pipe, the raw material composition ratio of which is shown in Table 1.
[0059] Example 2
[0060] A sealing ring rubber material for a high and low temperature resistant engine connecting pipe, the raw material composition ratio of which is shown in Table 1.
[0061] Example 3
[0062] A sealing ring rubber material for a high and low temperature resistant engine connecting pipe, the raw material composition ratio of which is shown in Table 1.
[0063] Example 4
[0064] A sealing ring rubber material for a high and low temperature resistant engine connecting pipe, the raw material composition ratio of which is shown in Table 1.
[0065] Comparative Example 1
[0066] A sealing ring rubber material for a high and low temperature resistant engine connecting pipe, the raw material composition ratio of which is shown in Table 1. The only difference from Example 2 is that no titanium oxide network composite is added.
[0067] Comparative Example 2
[0068] A sealing ring rubber material for a high and low temperature resistant engine connecting pipe, the raw material composition ratio of which is shown in Table 1.
[0069] The only difference from Example 2 is that no PPS is added.
[0070]
[0071] Trial plan
[0072] According to the schemes of Examples 1-4 and Comparative Examples 1-2 shown in Table 1 above, the schemes for testing and evaluating the physical properties of the rubber material for the engine hose prepared are as follows:
[0073] Hardness test: Use ShoreA hardness tester to measure the hardness of the rubber, the range is between 70-80ShoreA.
[0074] Tensile strength and elongation at break test: The tensile test was carried out under standard conditions to measure the tensile strength (≥8MPa) and elongation at break (≥250%).
[0075] Hot air aging test: Aging at 135°C for 168 hours, measuring the change rate of tensile strength and elongation, and the change rate is required to be within ±25%.
[0076] Low temperature brittleness test: Keep at -40℃ for 3 minutes and check whether the sample has cracks. No cracks are required.
[0077] Table 2 Physical performance parameters of the sealing ring rubber obtained in Examples 1-4 and Comparative Examples 1-2
[0078]
[0079] Combined with the data analysis in Table 2 above, it can be seen that the sealing ring rubber materials of Examples 1-4 have higher hardness and tensile strength, and can maintain stable performance under high stress and high load environments.
[0080] The high elongation at break indicates that the sealing ring rubber materials of Examples 1-4 have better ductility and flexibility and can adapt to complex deformation environments.
[0081] Under high temperature aging conditions, the sealing ring rubber materials of Examples 1-4 exhibit lower tensile strength and elongation change rate, extending the service life. Under low temperature conditions, the sealing ring rubber materials of Examples 1-4 have no cracks, showing excellent brittleness resistance.
[0082] In summary, the formula components of the sealing ring rubber material for the engine connecting pipe of the present invention significantly improve the high and low temperature resistance, mechanical strength and bonding performance of the sealing ring rubber material through the synergistic effect of the mixing system of AEM, PPS, and titanium oxide network composite, and the (functional auxiliary agent) of the organic silane coupling agent; the sealing ring rubber material is able to maintain excellent sealing performance in extreme environments, and is suitable for the application of sealing rings of engine connecting pipes in various environments.
[0083] The above embodiments are provided for persons familiar with the art to implement or use the present invention. Personnel familiar with the art can make various modifications or changes to the above embodiments without departing from the inventive concept of the present invention. Therefore, the protection scope of the present invention is not limited to the above embodiments, but should be the maximum scope of the innovative features mentioned in the claims.
Claims
1. A sealing ring rubber material for a high and low temperature resistant engine connecting pipe, characterized in that: The invention comprises the following components: ethylene acrylate rubber (AEM): 100-120 parts; Polyphenylene sulfide (PPS): 5-10; Titanium oxygen network complex: 10-15 parts; Plasticizer: 5-8 parts; Functional additives: 3-5 parts; Anti-aging agent: 5-10 parts; Vulcanizing agent: 3-5 parts.
2. The sealing ring rubber material for a high and low temperature resistant engine connecting pipe according to claim 1, characterized in that: The preparation method of the titanium oxide network composite comprises the following steps: Mix titanate polymer and titanium oxide in a ratio of 3:1 and stir evenly; During the stirring process, the temperature is gradually raised to 80-100°C and the reaction is maintained for 1-2 hours to allow the titanate polymer to react with the titanium oxide to form a Ti-O-Ti bond; After the reaction was completed, the mixture was cooled to room temperature to obtain a titanium oxide network composite (TONC).
3. The sealing ring rubber material for a high and low temperature resistant engine connecting pipe according to claim 2, characterized in that: The titanate polymer is tetrabutyl titanate; and the titanium oxide is titanium dioxide (TiO2).
4. The sealing ring rubber material for a high and low temperature resistant engine connecting pipe according to claim 1, characterized in that: The plasticizer is dioctyl phthalate (DOP) or dioctyl sebacate (DOS).
5. The sealing ring rubber material for a high and low temperature resistant engine connecting pipe according to claim 1, characterized in that: The functional auxiliary agent is an organic silane coupling agent, including γ-methacryloxypropyltrimethoxysilane (MEMO) or γ-cyanoethyltriethoxysilane (CETES).
6. The sealing ring rubber material for a high and low temperature resistant engine connecting pipe according to claim 1, characterized in that: The antioxidant is one or more combinations of KY845 and ZMTI.
7. The sealing ring rubber material for a high and low temperature resistant engine connecting pipe according to claim 1, characterized in that: The vulcanizing agent is a peroxide vulcanizing agent, including one or more combinations of 1,3-di-tert-butyl diisopropylbenzene peroxide, 1,4-di-tert-butyl diisopropylbenzene peroxide, and 1,2-di-tert-butyl diisopropylbenzene peroxide.
8. The method for preparing a sealing ring rubber compound for a high and low temperature resistant engine connecting pipe according to any one of claims 1 to 7, characterized in that: The following steps are involved: 1) Plasticizing: polyphenylene sulfide (PPS) and the titanium oxide network composite are weighed separately, mixed thoroughly and then plasticized to form ingredient A; Then, the ethylene acrylate rubber (AEM) is plasticized to form ingredient B, so that ingredients A and B reach a plastic state suitable for further processing; 2) First mixing: Put ingredients A and B into an internal mixer, start mixing, add plasticizer, functional additive, carbon black, antioxidant in sequence, continue mixing, and obtain rubber C; The rubber compound C is discharged onto the open mixing mill for heat dissipation. After the thin pass is completed, the sheet is cooled; 3) Second mixing: Put the rubber compound C and the vulcanizer into the internal mixer for mixing for 60-90 seconds, then continue mixing for 60-90 seconds after cleaning, and then discharge the material to the cutting machine for sheeting, thus completing the preparation of the final sealing ring rubber compound.