White composite material as well as preparation method and application thereof

By using transparent resin, inorganic filler and curing agent, the problem of difficulty in taking into account the transparency and reflectivity of traditional resin materials in LED and IC packaging is solved, and the high transmittance and high reflectivity are achieved. It improves optical performance in semi-transparent LED and IC packaging materials.

CN118931105APending Publication Date: 2024-11-12BEIJING SHOUKEHUA MICRO ELECTRONICS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410967989.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional resin materials are difficult to take into account both transparency and reflectivity in LED and IC packaging, resulting in poor optical performance and affecting the transmission and utilization efficiency of light.

Method used

A white composite material composed of transparent resin, inorganic filler and curing agent is prepared by mixing and mixing at a certain temperature to ensure that it has a light transmittance of more than 20% and a light reflectance of more than 40% at a specific wavelength. .

Benefits of technology

It achieves the improvement of light reflectivity while ensuring light transmittance. It is suitable as a semi-transmissive LED bracket packaging material, a semi-transmissive IC packaging material or an optical semiconductor packaging material, significantly improving the overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004952281040000121
    Figure BDA0004952281040000121
  • Figure BDA0004952281040000131
    Figure BDA0004952281040000131
  • Figure BDA0004952281040000141
    Figure BDA0004952281040000141
Patent Text Reader

Abstract

The invention relates to the field of electronic packaging materials, and discloses a white composite material and a preparation method and application thereof. The white composite material is made of a resin composition containing a transparent resin, an inorganic filler and a curing agent, and has a light transmittance of 20% or more and a light reflectance of 40% or more at a wavelength of 420-450 nm for a 1 mm sheet. The white composite material disclosed by the invention has relatively high light transmittance and relatively high light reflectivity, and has relatively good overall performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of LED and IC packaging materials, and in particular to a white composite material and a preparation method and application thereof, and more particularly to a preparation method and application of a white composite material having both light transmittance and reflectivity. Background Art

[0002] With the rapid development of electronic technology, LED (light emitting diode) and IC (integrated circuit) are more and more widely used in modern electronic devices. As a key packaging material for electronic devices, resin has been widely used in the packaging of LED and IC due to its excellent mechanical properties, insulation properties and chemical corrosion resistance.

[0003] However, traditional resin materials focus more on mechanical properties such as heat resistance, moisture resistance, and thermal stability during application, and still have some shortcomings in terms of optical properties. For example, it is difficult to balance transparency and reflectivity, resulting in unsatisfactory optical properties of packaging materials. In LED packaging applications, packaging materials not only need to have a certain degree of transparency to ensure light transmission, but also need to have a high reflectivity to improve light utilization efficiency. Summary of the invention

[0004] The purpose of the present invention is to overcome the problem that the transparency and reflectivity of packaging materials in the prior art are difficult to balance, and to provide a white composite material and a preparation method and application thereof. The white composite material of the present invention has a higher light reflectivity while ensuring light transmittance, and is particularly suitable for use as a semi-transparent LED bracket packaging material, a semi-transparent IC packaging material or an optical semiconductor packaging material.

[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a white composite material, which is made of a resin composition containing a transparent resin, an inorganic filler and a curing agent. At a wavelength of 420-450nm, the light transmittance of a 1mm sheet of the white composite material is more than 20%, and the light reflectivity is more than 40%.

[0006] Preferably, at a wavelength of 420-450 nm, the light transmittance of a 1 mm sheet of the white composite material is 30-70%, and the light reflectivity is 50-90%.

[0007] Preferably, the resin composition further contains a curing accelerator, a coupling agent and an antioxidant.

[0008] Preferably, based on the total weight of the resin composition, the content of the transparent resin is 4-45wt%, the content of the inorganic filler is 10-90wt%, the content of the curing agent is 4-45wt%, the content of the accelerator is 0.01-1wt%, the content of the coupling agent is 0.1-1wt%, and the content of the antioxidant is 0.05-1wt%.

[0009] More preferably, based on the total weight of the resin composition, the content of the transparent resin is 15-40wt%, the content of the inorganic filler is 30-70wt%, the content of the curing agent is 10-40wt%, the content of the accelerator is 0.05-0.2wt%, the content of the coupling agent is 0.2-0.8wt%, and the content of the antioxidant is 0.1-0.5wt%.

[0010] Preferably, the transparent resin is at least one of transparent epoxy resin, silicone resin and silicone epoxy resin.

[0011] Preferably, the transparent resin is a transparent epoxy resin, selected from at least one of bisphenol A type resin, hydrogenated bisphenol A type resin, alicyclic epoxy resin, and triglycidyl isocyanurate.

[0012] Preferably, the inorganic filler is at least one of spherical silicon oxide, aluminum oxide and aluminum hydroxide.

[0013] Preferably, the particles of the inorganic filler are solid particles and / or hollow particles.

[0014] Preferably, the curing agent is a monofunctional alicyclic anhydride, preferably at least one of tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride and methylhexahydrophthalic anhydride.

[0015] Preferably, the curing accelerator is selected from at least one of organic phosphorus compounds, tertiary amine compounds and imidazole compounds.

[0016] Preferably, the coupling agent is a silane coupling agent, preferably at least one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane, γ-2,3-aminopropyltriethoxysilane and γ-mercaptoaminopropyltrimethoxysilane.

[0017] Preferably, the antioxidant is a phenolic antioxidant, preferably at least one of 2,6-di-tert-butyl-p-cresol, 2,2-methylenebis(4-ethyl-6-tert-butylphenol), 4,4-thiobis(3-methyl-6-tert-butylphenol) and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0018] The second aspect of the present invention provides a method for preparing the white composite material described above, the method comprising: mixing a resin composition containing a transparent resin, an inorganic filler, a curing agent and an optional curing accelerator, a coupling agent and an antioxidant, and kneading the obtained mixture.

[0019] Preferably, the mixing conditions include: temperature of 60-100° C. and time of 10-30 minutes.

[0020] The third aspect of the present invention provides the use of the white composite material described above as a semi-transparent LED bracket packaging material, a semi-transparent IC packaging material or an optical semiconductor packaging material.

[0021] The white composite material of the present invention adopts a transparent resin and an inorganic filler with a certain light transmittance, has both high light transmittance and high light reflectivity, has good overall performance, and is particularly suitable for use as a semi-transparent LED bracket packaging material, a semi-transparent IC packaging material or an optical semiconductor packaging material. DETAILED DESCRIPTION

[0022] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0023] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0024] The white composite material of the present invention is made of a resin composition containing a transparent resin, an inorganic filler and a curing agent. At a wavelength of 420-450nm, the light transmittance of a 1 mm sheet of the white composite material is more than 20%, and the light reflectivity is more than 40%. The white composite material of the present invention has both high light transmittance and high light reflectivity.

[0025] Preferably, the light transmittance of a 1 mm sheet of the white composite material is 25-90%, more preferably 30-70%, and further preferably 35-60%; the light reflectivity is 45-95%, more preferably 50-90%, and further preferably 55-80%.

[0026] In the present invention, the light transmittance and light reflectance of the white composite material are measured using an integrating sphere spectrophotometer UV2600.

[0027] In the white composite material of the present invention, in a preferred case, in addition to the transparent resin, the inorganic filler and the curing agent, the resin composition also contains a curing accelerator, a coupling agent and an antioxidant. Further preferably, in the resin composition, based on the total weight of the resin composition, the content of the transparent resin is 4-45wt%, the content of the inorganic filler is 10-90wt%, the content of the curing agent is 4-45wt%, the content of the accelerator is 0.01-1wt%, the content of the coupling agent is 0.1-1wt%, and the content of the antioxidant is 0.05-1wt%. More preferably, based on the total weight of the resin composition, the content of the transparent resin is 15-40wt%, the content of the inorganic filler is 30-70wt%, the content of the curing agent is 10-40wt%, the content of the accelerator is 0.05-0.2wt%, the content of the coupling agent is 0.2-0.8wt%, and the content of the antioxidant is 0.1-0.5wt%. More preferably, based on the total weight of the resin composition, the content of the transparent resin is 20-35wt%, the content of the inorganic filler is 30-60wt%, the content of the curing agent is 12-35wt%, the content of the accelerator is 0.08-0.15wt%, the content of the coupling agent is 0.4-0.7wt%, and the content of the antioxidant is 0.2-0.4wt%. The white composite material prepared by the resin composition according to the above preferred components and content ranges has both high light transmittance and light reflectivity, and has good overall performance.

[0028] In the present invention, the transparent resin may be a resin with high transparency conventionally used in the art. Preferably, the transparent resin is at least one of a transparent epoxy resin, a silicone resin and a silicone epoxy resin. In a further preferred embodiment, the transparent resin is a transparent epoxy resin selected from at least one of bisphenol A type resin, hydrogenated bisphenol A type resin, alicyclic epoxy resin and triglycidyl isocyanurate. More preferably, the transparent resin is triglycidyl isocyanurate.

[0029] In the present invention, the inorganic filler can be an inorganic filler with high light transmittance conventionally used in the art. In a preferred case, the inorganic filler is at least one of spherical silicon oxide, aluminum oxide and aluminum hydroxide. In a preferred embodiment, the particles of the inorganic filler are solid particles and / or hollow particles. In a more preferred embodiment, the inorganic filler is solid silicon dioxide particles.

[0030] In the present invention, the curing agent can be a monofunctional alicyclic anhydride. In a preferred embodiment, the curing agent is at least one of tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride and methylhexahydrophthalic anhydride. In a more preferred embodiment, the curing agent is hexahydrophthalic anhydride and / or methylhexahydrophthalic anhydride.

[0031] In the present invention, the curing accelerator may be selected from at least one of an organophosphorus compound, a tertiary amine compound and an imidazole compound. Examples of the organophosphorus compound may be methyl tributyl phosphonium dimethyl phosphate, benzyl triphenyl phosphonium bromide, and the like. Examples of the tertiary amine compound may be 2,4,6-tris(dimethylaminomethyl)phenol, benzyl dimethylamine, o-hydroxybenzyl dimethylamine, and the like. Examples of the imidazole compound may be 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, and the like. In a preferred embodiment, the curing accelerator is methyl tributyl phosphonium dimethyl phosphate.

[0032] In the present invention, the coupling agent may be a silane coupling agent. In a preferred embodiment, the coupling agent is at least one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane, γ-2,3-aminopropyltriethoxysilane and γ-thiolaminopropyltrimethoxysilane. In a more preferred embodiment, the coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane.

[0033] In the present invention, the antioxidant may be a phenolic antioxidant. In a preferred embodiment, the antioxidant is at least one of 2,6-di-tert-butyl-p-cresol, 2,2-methylenebis(4-ethyl-6-tert-butylphenol), 4,4-thiobis(3-methyl-6-tert-butylphenol) and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate. In a more preferred embodiment, the antioxidant is 2,6-di-tert-butyl-p-cresol.

[0034] In a more preferred embodiment, the resin composition contains 20-35wt% of a transparent resin, 30-60wt% of an inorganic filler, 12-35wt% of a curing agent, 0.08-0.15wt% of an accelerator, 0.4-0.7wt% of a coupling agent, and 0.2-0.4wt% of an antioxidant, wherein the transparent resin is triglycidyl isocyanurate, the inorganic filler is solid silica particles, the curing agent is hexahydrophthalic anhydride and / or methyl hexahydrophthalic anhydride, the curing accelerator is methyl tributylphosphine dimethyl phosphate, the coupling agent is γ(2,3 epoxypropoxy)propyltrimethoxysilane, and the antioxidant is 2,6-di-tert-butyl-p-cresol. The white composite material prepared according to the resin composition of this preferred embodiment has significantly better overall performance.

[0035] The white composite material of the present invention can be prepared by a combination of conventional technical means in the art. In some embodiments, the preparation method of the white composite material comprises: mixing a resin composition containing a transparent resin, an inorganic filler, a curing agent, and an optional curing accelerator, a coupling agent, and an antioxidant, and kneading the obtained mixture.

[0036] In the above preparation method, "optional" means that the resin composition may or may not contain one or more components of a curing accelerator, a coupling agent and an antioxidant. In a preferred case, the resin composition contains a transparent resin, an inorganic filler, a curing agent, a curing accelerator, a coupling agent and an antioxidant.

[0037] In the above preparation method, the types and contents of the transparent resin, the inorganic filler, the curing agent, the curing accelerator, the coupling agent and the antioxidant are the same as those described above and will not be repeated here.

[0038] In the above preparation method, the mixing conditions may include: temperature of 60-100° C., preferably 70-90° C.; time of 10-30 minutes, preferably 15-25 minutes.

[0039] The present invention also provides the use of the white composite material as a semi-transparent LED bracket packaging material, a semi-transparent IC packaging material or a light semiconductor packaging material. The white composite material of the present invention is used as a semi-transparent LED bracket packaging material, a semi-transparent IC packaging material or a light semiconductor packaging material, and exhibits a higher light transmittance and a higher light reflectance, and has better overall performance.

[0040] The white composite material and its preparation and application described in the present invention are further described by examples. The examples are implemented based on the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following examples.

[0041] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are all commercially available.

[0042] Example 1

[0043] The sources of materials used in this embodiment are as follows:

[0044] Transparent resin: triglycidyl isocyanurate A1, purchased from Nissan Chemical Materials Technology (Suzhou) Co., Ltd., brand TEPIC-S;

[0045] Inorganic filler: solid silica, purchased from Jiangsu Lianrui New Materials Co., Ltd., brand NQ101;

[0046] Curing agent: methyl hexahydrophthalic anhydride, purchased from Puyang Huicheng Electronic Materials Co., Ltd.;

[0047] Curing accelerator: methyl tributylphosphonium dimethyl phosphate, purchased from Nippon Chemical Industry Co., Ltd., brand name PX-4MP;

[0048] Coupling agent: γ-(2,3-epoxypropoxy)propyltrimethoxysilane, commercially available KH560;

[0049] Antioxidant: 2,6-di-tert-butyl-p-cresol, purchased from Jiangsu Maida New Materials Co., Ltd., brand name Antioxidant 264.

[0050] 35g of transparent resin, 30g of inorganic filler, 34g of curing agent, 0.1g of curing accelerator, 0.6g of coupling agent and 0.3g of antioxidant were put into a high-speed mixer and mixed to obtain an epoxy molding compound mixture. The obtained mixture was kneaded at 80°C for 20 minutes, cooled and crushed after kneading to obtain the white composite material L1 of the present invention.

[0051] Example 2

[0052] The transparent resin, inorganic filler, curing agent, curing accelerator, coupling agent and antioxidant used in this example are all from the same sources as those in Example 1.

[0053] 20g of transparent resin, 59.12g of inorganic filler, 20g of curing agent, 0.08g of curing accelerator, 0.4g of coupling agent and 0.4g of antioxidant were put into a high-speed mixer and mixed to obtain an epoxy molding compound mixture. The obtained mixture was kneaded at 90°C for 15 minutes, cooled and crushed after kneading to obtain the white composite material L2 of the present invention.

[0054] Example 3

[0055] The transparent resin, inorganic filler, curing agent, curing accelerator, coupling agent and antioxidant used in this example are all from the same sources as those in Example 1.

[0056] 30g of transparent resin, 56.95g of inorganic filler, 12g of curing agent, 0.15g of curing accelerator, 0.7g of coupling agent and 0.2g of antioxidant were put into a high-speed mixer and mixed to obtain an epoxy molding compound mixture. The obtained mixture was kneaded at 70°C for 25 minutes, cooled and crushed after kneading to obtain the white composite material L3 of the present invention.

[0057] Example 4

[0058] The transparent resin, inorganic filler, curing agent, curing accelerator, coupling agent and antioxidant used in this example are all from the same sources as those in Example 1.

[0059] 15g of transparent resin, 70g of inorganic filler, 14g of curing agent, 0.1g of curing accelerator, 0.6g of coupling agent and 0.3g of antioxidant were put into a high-speed mixer and mixed to obtain an epoxy molding compound mixture. The obtained mixture was kneaded at 80°C for 20 minutes, cooled and crushed after kneading to obtain the white composite material L4 of the present invention.

[0060] Example 5

[0061] The transparent resin, inorganic filler, curing accelerator, coupling agent and antioxidant used in this example are all from the same sources as those in Example 1.

[0062] The curing agent used was hexahydrophthalic anhydride, which was purchased from Puyang Huicheng Electronic Materials Co., Ltd.

[0063] 25g of transparent resin, 50g of inorganic filler, 24g of curing agent, 0.1g of curing accelerator, 0.6g of coupling agent and 0.3g of antioxidant were put into a high-speed mixer and mixed to obtain an epoxy molding compound mixture. The obtained mixture was kneaded at 80°C for 20 minutes, cooled and crushed after kneading to obtain the white composite material L5 of the present invention.

[0064] Example 6

[0065] The transparent resin, inorganic filler, curing accelerator, coupling agent and antioxidant used in this example are all from the same sources as those in Example 1.

[0066] There are two types of curing agents used, curing agent 1 is hexahydrophthalic anhydride, and curing agent 2 is methyl hexahydrophthalic anhydride, both of which are purchased from Puyang Huicheng Electronic Materials Co., Ltd.

[0067] 45g of transparent resin, 10g of inorganic filler, 22g of curing agent 1, 22g of curing agent 2, 0.1g of curing accelerator, 0.6g of coupling agent and 0.3g of antioxidant were put into a high-speed mixer for mixing, and the epoxy molding compound mixture was obtained. The obtained mixture was kneaded at 80°C for 20 minutes, cooled and crushed after kneading to obtain the white composite material L6 of the present invention.

[0068] Example 7

[0069] A white composite material was prepared according to the method of Example 1, except that the transparent resin used was bisphenol A resin (purchased from Nan Ya Company, brand E-20), and finally a white composite material L7 was prepared.

[0070] Example 8

[0071] A white composite material was prepared according to the method of Example 1, except that the transparent resin used was hydrogenated bisphenol A resin (purchased from Guodu Chemical Company, brand ST3000), and finally a white composite material L8 was prepared.

[0072] Example 9

[0073] A white composite material was prepared according to the method of Example 1, except that the transparent resin used was an alicyclic epoxy resin (purchased from Daicel Corporation, brand 2021P), and finally a white composite material L9 was prepared.

[0074] Example 10

[0075] A white composite material was prepared according to the method of Example 1, except that the transparent resin used was an organic silicon epoxy resin (purchased from Xinyue Chemical Company, brand KR470), and finally a white composite material L10 was prepared.

[0076] Embodiment 11

[0077] A white composite material was prepared according to the method of Example 1, except that the inorganic filler used was hollow silica particles (purchased from 3M Company, brand S60SH), and finally a white composite material L11 was prepared.

[0078] Example 12

[0079] A white composite material was prepared according to the method of Example 1, except that the inorganic filler used was solid alumina particles (purchased from Lianrui Company, brand NA1250W), and finally a white composite material L12 was prepared.

[0080] Example 13

[0081] A white composite material was prepared according to the method of Example 1, except that the inorganic filler used was solid aluminum hydroxide particles (purchased from Albemarle Corporation, USA, brand 104LEO), and finally a white composite material L13 was prepared.

[0082] Embodiment 14

[0083] The transparent resin, inorganic filler, curing accelerator, coupling agent and antioxidant used in this example are all from the same sources as those in Example 1.

[0084] 5 g of transparent resin, 90 g of inorganic filler, 4 g of curing agent, 0.1 g of curing accelerator, 0.6 g of coupling agent and 0.3 g of antioxidant were put into a high-speed mixer and mixed to obtain an epoxy molding compound mixture. The obtained mixture was kneaded at 80° C. for 20 minutes, cooled and crushed after kneading to obtain the white composite material L14 of the present invention.

[0085] Embodiment 15

[0086] The transparent resin, inorganic filler, curing accelerator, coupling agent and antioxidant used in this example are all from the same sources as those in Example 1.

[0087] 90g of transparent resin, 5g of inorganic filler, 4g of curing agent, 0.1g of curing accelerator, 0.6g of coupling agent and 0.3g of antioxidant were put into a high-speed mixer for mixing, and the epoxy molding compound mixture was obtained. The obtained mixture was kneaded at 80°C for 20 minutes, cooled and crushed after kneading, and the white composite material L15 of the present invention was obtained.

[0088] Comparative Example 1

[0089] A white composite material was prepared according to the method of Example 1, except that the resin used was o-cresol epoxy resin (purchased from Baling Petrochemical Co., Ltd., brand CYDCN-200H), and finally a composite material D1 was prepared.

[0090] Comparative Example 2

[0091] A white composite material was prepared according to the method of Example 1, except that the inorganic filler used was titanium oxide (purchased from Yibin Tianyuan Group Co., Ltd., brand TYR566), and finally a composite material D2 was prepared.

[0092] The proportions of various raw materials in Examples 1-15 and Comparative Examples 1-2 are shown in Table 1 below.

[0093] Table 1

[0094]

[0095] Test Case

[0096] The light transmittance and reflectivity of the white composite materials prepared in Examples 1-15 and Comparative Examples 1-2 at each stage were measured and tested, and the test method was as follows:

[0097] (1) The prepared resin composition was cured at a mold temperature of 175° C. for 120 seconds, and was transferred into a specific mold by a molding machine for injection molding to be cured and formed into a 1 mm thick sheet.

[0098] (2) Transmittance and reflectance after curing: After the thin film of step (1) was cured at 150° C. for 2 h, the transmittance and reflectance at a wavelength of 420 nm were tested using an ultraviolet spectrophotometer UV2600; wherein the ultraviolet spectrophotometer UV2600 was purchased from Shimadzu.

[0099] (3) Transmittance and reflectance after high-temperature aging at 180°C for 2 h: The thin film obtained in step (2) was baked in an oven at 180°C for 2 h, and the transmittance and reflectance at a wavelength of 420 nm were tested using an integrating sphere spectrophotometer UV2600.

[0100] (4) Transmittance and reflectance after aging at 260° C. for 5 min: The thin film obtained in step (3) was baked in an oven at 260° C. for 5 min, and the transmittance and reflectance at a wavelength of 420 nm were tested using an integrating sphere spectrophotometer UV2600.

[0101] The test results of light transmittance and reflectivity of the white composite materials prepared in Examples 1-15 and Comparative Examples 1-2 at each stage are shown in Table 2.

[0102] Table 2

[0103]

[0104]

[0105] It can be seen from the data in Table 2 that the white composite material according to the present invention has both high light transmittance and high light reflectance, and has good overall performance. Specifically, the white composite materials described in Examples 1-3 of the present invention have a reflectance of 60% or more while also having a transmittance of more than 35%. The transmittance of the white composite materials described in Examples 4-15 also reaches more than 25%, and the optical properties can still be maintained after high-temperature aging, and have good thermal stability; while the composite materials prepared in Comparative Examples 1-2 do not use the transparent resin or the inorganic filler described in the present invention, even if the reflectance is still 40% or more, the transmittance is low, and both cannot be taken into account.

[0106] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A white composite material, characterized in that: The white composite material is made of a resin composition containing a transparent resin, an inorganic filler and a curing agent. At a wavelength of 420-450nm, the light transmittance of a 1mm sheet of the white composite material is more than 20%, and the light reflectivity is more than 40%.

2. The white composite material according to claim 1, characterized in that: At a wavelength of 420-450 nm, a 1 mm sheet of the white composite material has a light transmittance of 30-70% and a light reflectivity of 50-90%.

3. The white composite material according to claim 1 or 2, characterized in that: The resin composition also contains a curing accelerator, a coupling agent and an antioxidant.

4. The white composite material according to claim 3, characterized in that: Based on the total weight of the resin composition, the content of the transparent resin is 4-45wt%, the content of the inorganic filler is 10-90wt%, the content of the curing agent is 4-45wt%, the content of the accelerator is 0.01-1wt%, the content of the coupling agent is 0.1-1wt%, and the content of the antioxidant is 0.05-1wt%.

5. The white composite material according to claim 4, characterized in that: Based on the total weight of the resin composition, the content of the transparent resin is 15-40wt%, the content of the inorganic filler is 30-70wt%, the content of the curing agent is 10-40wt%, the content of the accelerator is 0.05-0.2wt%, the content of the coupling agent is 0.2-0.8wt%, and the content of the antioxidant is 0.1-0.5wt%.

6. The white composite material according to any one of claims 1 to 5, characterized in that: The transparent resin is at least one of a transparent epoxy resin, a silicone resin and a silicone epoxy resin; Preferably, the transparent resin is a transparent epoxy resin, selected from at least one of bisphenol A type resin, hydrogenated bisphenol A type resin, alicyclic epoxy resin, and triglycidyl isocyanurate.

7. The white composite material according to any one of claims 1 to 5, characterized in that: The inorganic filler is at least one of spherical silicon oxide, aluminum oxide and aluminum hydroxide; Preferably, the particles of the inorganic filler are solid particles and / or hollow particles.

8. The white composite material according to any one of claims 3 to 5, characterized in that: The curing agent is a monofunctional alicyclic anhydride, preferably at least one of tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride and methylhexahydrophthalic anhydride; Preferably, the curing accelerator is selected from at least one of an organic phosphorus compound, a tertiary amine compound and an imidazole compound; Preferably, the coupling agent is a silane coupling agent, preferably at least one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane, γ-2,3-aminopropyltriethoxysilane and γ-mercaptoaminopropyltrimethoxysilane; Preferably, the antioxidant is a phenolic antioxidant, preferably at least one of 2,6-di-tert-butyl-p-cresol, 2,2-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-thiobis(6-tert-butyl-3-methylphenol) and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

9. A method for preparing the white composite material according to any one of claims 1 to 8, characterized in that: The method comprises: mixing a resin composition containing a transparent resin, an inorganic filler, a curing agent, and optionally a curing accelerator, a coupling agent, and an antioxidant, and kneading the obtained mixture; Preferably, the mixing conditions include: temperature of 60-100° C. and time of 10-30 minutes.

10. Use of the white composite material according to any one of claims 1 to 8 as a semi-transparent LED bracket packaging material, a semi-transparent IC packaging material or an optical semiconductor packaging material.