Friction damping vibration attenuation material with double-layer hollow structure as well as preparation method and application of friction damping vibration attenuation material

By preparing a double-layer hollow structure friction damping vibration reduction material, the energy dissipation of the interfacial friction between the middle hollow layer and the outer hollow sphere is utilized, which solves the shortcomings of composite materials in vibration reduction performance and achieves a highly efficient vibration control effect.

CN118931111AActive Publication Date: 2024-11-12NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411179750.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing composite materials have shortcomings in vibration reduction performance, making it difficult to effectively reduce the vibration impact on high-end precision instruments in vibration environments.

Method used

A friction damping vibration reduction material with a double-layer hollow structure increases the friction damping performance of the composite material by dissipating energy through interfacial friction between the middle hollow layer and the outer hollow sphere. The preparation method includes preparing a solid double-layer silica sphere, carbonizing and etching to form a double-layer hollow carbon sphere, and then compounding it with a resin material.

Benefits of technology

It improves the vibration reduction performance of composite materials, ensures lightweight and high-strength characteristics, and enhances the damping and vibration reduction effect, making it suitable for vibration control of high-end precision instruments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931111A_ABST
    Figure CN118931111A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of composite material vibration attenuation, in particular to a friction damping vibration attenuation material with a double-layer hollow structure as well as a preparation method and application thereof, and the preparation method of the material specifically comprises the following steps: S1, preparing solid double-layer silicon dioxide spheres, S2, preparing double-layer hollow carbon spheres, and S3, preparing a composite material with a double-layer hollow sphere structure. Scattering and diffraction energy consumption of mechanical waves occur in a middle hollow layer area, then the mechanical waves cause interface friction energy consumption between the middle hollow balls and the outer-layer hollow balls, the mechanical waves are further scattered for multiple times between the layers, friction energy consumption of the outer-layer hollow balls and the composite material interface is caused, and the composite material is obtained. The interface friction energy dissipation effect of the composite material is improved, and the vibration reduction performance of the composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite material vibration reduction, and in particular to a friction damping vibration reduction material with a double-layer hollow structure, a preparation method and application thereof. Background Art

[0002] With the development of technology, modern engineering systems are increasingly dependent on efficient vibration control to ensure their performance, reliability and life. For example, the aerospace field requires materials that can effectively reduce the vibration generated by aircraft at high speeds, thereby improving flight safety and passenger comfort. In the automotive industry, vibration-damping materials can significantly reduce the noise and vibration generated by vehicles at high speeds, improving driving experience and ride comfort.

[0003] Composite materials are gradually being widely used in aerospace, navigation and transportation fields due to their light weight and high strength. In the aerospace field, aircraft structures need to face the vibration and impact loads brought by high-speed flight and complex aerodynamic environments. Composite materials, with their high strength, low density and excellent vibration control characteristics, are an ideal choice for reducing structural weight, improving aircraft performance and passenger comfort. In the navigation field, composite materials can reduce the weight of the hull and protect the hull from corrosion in the hot and humid marine environment due to their light weight and corrosion resistance. In the field of transportation, composite materials can effectively reduce the impact of engine and road vibration on passengers in the car, improving driving comfort and safety.

[0004] To improve the damping performance of composite materials, micro-nano-sized fillers such as carbon nanotubes and graphene can be added to the composite materials to increase the contact area between the resin and the nanofillers and increase the interface friction effect of the mechanical waves during vibration.

[0005] The double-layer hollow structure is composed of a middle hollow region layer and an outer layer that wraps the middle hollow layer, forming a double-layer hollow structure with a gap between the two layers. Due to its unique double-layer hollow structure, compared with solid and single-layer hollow balls of the same size, when the vibration mechanical wave passes through the outer layer and enters the middle hollow layer, the mechanical wave first scatters and diffracts energy in the middle hollow layer area, and then the mechanical wave causes the interface friction energy consumption between the middle hollow ball and the outer hollow ball. The mechanical wave further forms multiple scatterings between the layers, causing friction energy consumption at the interface between the outer hollow ball and the composite material.

[0006] Based on the above description, the double-layer hollow structure can effectively increase the interface friction energy dissipation effect of the composite material, improve the friction damping performance of the composite material, and improve the vibration reduction performance of the composite material. It can provide a practical and effective solution for solving the vibration reduction control of high-end precision instruments, which ensures the light weight and high strength characteristics of the original structure and increases its damping vibration reduction performance. Summary of the invention

[0007] The present invention provides a friction damping vibration reduction material with a double-layer hollow structure, a preparation method and application thereof, so as to solve the problems raised in the above background technology.

[0008] A method for preparing a friction damping and vibration reduction material with a double-layer hollow structure, the preparation method specifically comprising the following steps:

[0009] S1. Preparation of solid double-layer silica spheres:

[0010] Anhydrous ethanol, ammonia water and deionized water are mixed and stirred in a glass beaker for 15 minutes to obtain an alkaline ethanol / water mixed solution, and then tetrabutyl silicate, resorcinol and formaldehyde are quickly added to the above solution in sequence, and the mixture is sealed and stirred for a period of time to obtain a microsphere solution with silicon dioxide as the core and carbide as the shell, and then tetrabutyl silicate is added to the solution for a second time, and the mixture is stirred for a period of time, and then the solution is added to the reactor to react for a period of time, and finally the mixture is repeatedly washed and dried with an ethanol solution and deionized water to obtain a solid double-layer silica sphere;

[0011] S2. Preparation of double-layer hollow carbon spheres:

[0012] The solid double-layer silica sphere obtained in step S1 is carbonized in an inert gas to obtain a carbonized solid double-layer silica sphere, and then SiO2 is etched with hydrofluoric acid to obtain a double-layer hollow carbon sphere solution, and finally washed with deionized water and dried to obtain a double-layer hollow carbon sphere;

[0013] S3. Preparation of a composite material having a double-layer hollow sphere structure:

[0014] The double-layer hollow carbon spheres prepared in step S2 are reacted with a silane coupling agent solution, and then vacuum filtered and dried. The double-layer hollow carbon spheres are then dispersed in an organic solution. Finally, the double-layer hollow carbon sphere organic solution is mixed and stirred with a composite material resin, and allowed to stand and dry to obtain a friction damping vibration reduction material with a double-layer hollow structure.

[0015] Furthermore, in step S1, the volume ratio of formaldehyde, tetrabutyl silicate, deionized water, ammonia water and anhydrous ethanol is 1:(3-7):(11-26):(3-8):(83-187), and the mass ratio of resorcinol to deionized water in step S1 is 1:(20-35).

[0016] Furthermore, in step S1, after adding tetrabutyl silicate, resorcinol and formaldehyde to the solution, the sealed stirring time is 6-10 hours, the second addition of tetrabutyl silicate in step S1 and the stirring time is 24-30 hours, the solution in step S1 reacts in the reactor for 12-24 hours, and the reaction temperature is 180°C.

[0017] Furthermore, in step S2, the inert gas is nitrogen or argon, and the carbonization temperature is 500-700°C.

[0018] Furthermore, the step of etching SiO2 with hydrofluoric acid in step S2 is as follows:

[0019] The carbonized solid double-layer silica spheres were first statically etched for 6 h and then ultrasonically etched for 2 h.

[0020] Furthermore, the organic solution in which the double-layer hollow carbon spheres are dispersed in step S3 is an ethanol or acetone solution.

[0021] Furthermore, the composite material resin in step S3 is a pure resin composite material or a fiber-reinforced resin-based composite material.

[0022] A friction damping vibration reduction material with a double-layer hollow structure is prepared by the method for preparing the friction damping vibration reduction material with a double-layer hollow structure.

[0023] The friction damping vibration reduction material with a double-layer hollow structure prepared by the above preparation method is applied to industrial vibration reduction materials.

[0024] The advantages and beneficial effects of the present invention are:

[0025] The present invention synthesizes SiO2@CP@SiO2@CP in a solution, then obtains SiO2@C@SiO2@C by carbonization, and finally obtains C@C by etching with hydrofluoric acid, and then compounds C@C with a resin material, and scatters and diffracts mechanical waves through the middle hollow layer area, and then mechanical waves cause interface friction energy consumption between the middle hollow sphere and the outer hollow sphere, and the mechanical waves further form multiple scatterings between the layers, causing friction energy consumption between the outer hollow sphere and the composite material interface, increasing the interface friction energy consumption effect of the composite material, and improving the vibration reduction performance of the composite material. It can provide a practical and effective solution to solve the vibration reduction control of high-end precision instruments, that is, it ensures the light weight and high strength characteristics of the original structure, and increases its damping vibration reduction performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1 This is a microscopic morphology of the double-layer hollow carbon sphere (C@C) of the present invention.

[0028] Figure 2 This is a diagram of the damping performance of the double-layer hollow carbon sphere (C@C) filled with IN2 epoxy flow-guiding resin and pure IN2 epoxy flow-guiding resin. DETAILED DESCRIPTION

[0029] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.

[0030] like Figure 1-2 As shown, the present invention provides a friction damping vibration reduction material with a double-layer hollow structure, and the specific preparation steps are shown in the following Example 1;

[0031] Example 1

[0032] S1. Preparation of SiO2@CP@SiO2@CP:

[0033] 70 mL of anhydrous ethanol, 3 mL of ammonia water and 10 mL of deionized water were sealed and stirred in a glass beaker for 15 min to obtain an alkaline ethanol / water mixed solution, and then 2.8 mL of tetrabutyl silicate, 0.4 g of resorcinol and 0.56 mL of formaldehyde were added to the above solution in sequence, and the mixture was sealed and stirred for 6 h to obtain a SiO2@CP solution with silicon dioxide as the core and carbide as the shell;

[0034] Then, 1.5 mL of tetrabutyl silicate was added to the solution for a second time and stirring was continued for 24 h. Subsequently, the solution was added to the reactor and reacted at 180°C for 12 h. Finally, it was repeatedly washed with anhydrous ethanol solution and deionized water for 5 times and dried to obtain SiO2@CP@SiO2@CP.

[0035] S2. Preparation of C@C:

[0036] The SiO2@CP@SiO2@CP obtained in step S1 is placed in a tubular furnace and carbonized in nitrogen for 3 hours at a carbonization temperature of 700°C to obtain SiO2@C@SiO2@C;

[0037] Then SiO2@C@SiO2@C was placed in 60 mL of a 40 wt% hydrofluoric acid solution, left to etch for 6 h, and then ultrasonically etched for 2 h in an ultrasonic machine with a power of 180 W;

[0038] Finally, the microspheres were washed three times with deionized water to obtain C@C with a size of about 500 nm. Figure 1 As shown;

[0039] S3. Preparation of a composite material having a double-layer hollow sphere structure:

[0040] Prepare 60 mL of 7.5 wt% silane solution, add the C@C prepared in step S2 to the 7.5 wt% silane solution, select KH-560 silane coupling agent as the silane coupling agent, stir at room temperature for 5 h, and then wash with deionized water for 3 times to obtain silanized C@C;

[0041] The silanized C@C was dispersed in 30 mL of acetone and stirred for 15 min to be evenly dispersed, thereby obtaining a C@C acetone solution with a concentration of 15 wt%.

[0042] Next, 26 mL of the acetone solution in which C@C is dispersed is taken, and 100 g of a resin material is added. The resin material is selected as epoxy resin, and stirred for 15 min. Then, the mixture is vacuum dried at 90°C for 12 h to completely volatilize the acetone. Finally, 30 g of a curing agent is added. The curing agent and the epoxy resin form a composite resin material, and stirred for another 15 min to ensure that the epoxy resin and the curing agent are evenly mixed. The model of the curing agent is AT30. The composite resin material formed is IN2 epoxy flow-guiding resin.

[0043] The IN2 epoxy flow-conducting resin in this embodiment is a pure resin composite material. Adding fiber materials such as carbon fiber, glass fiber, and aramid fiber to the pure resin composite material can form a fiber-reinforced resin-based composite material, and the C@C in this application can also be added to form a friction damping and vibration reduction material;

[0044] Finally, IN2 epoxy flow-inducting resin mixed with C@C was poured into the mold and cured in a drying oven at 60°C. The addition amount of C@C was 3wt%, and finally a friction damping and vibration reduction material with a double-layer hollow structure was obtained.

[0045] In the present invention, the epoxy resin and curing agent used are both commercially available low-viscosity slow-curing epoxy resins.

[0046] Figure 2 The damping properties of pure epoxy resin and epoxy resin composites with double-layer hollow carbon spheres (C@C) are shown in Figure 2. The damping coefficient of pure epoxy resin is 0.9, and the damping coefficient of epoxy resin composites with double-layer hollow carbon spheres (C@C) is 0.96.

[0047] The friction damping and vibration reduction material with a double-layer hollow structure prepared by the above-mentioned preparation method has a double-layer hollow structure; the size is at the micro-nano level; the main component of the double-layer hollow structure is carbon; there is a gap between the inner layer and the outer layer of the double-layer hollow structure; the double-layer hollow structure is filled, dispersed and mixed in the resin to improve the damping and vibration reduction performance of the composite material.

[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a friction damping and vibration reduction material with a double-layer hollow structure, It is characterized in that The preparation method specifically comprises the following steps: S1. Preparation of solid double-layer silica spheres: Anhydrous ethanol, ammonia water and deionized water are mixed and stirred in a glass beaker for 15 minutes to obtain an alkaline ethanol / water mixed solution, and then tetrabutyl silicate, resorcinol and formaldehyde are quickly added to the above solution in sequence, and the mixture is sealed and stirred for a period of time to obtain a microsphere solution with silicon dioxide as the core and carbide as the shell, and then tetrabutyl silicate is added to the solution for a second time, and the mixture is stirred for a period of time, and then the solution is added to the reactor to react for a period of time, and finally the mixture is repeatedly washed and dried with an ethanol solution and deionized water to obtain a solid double-layer silica sphere; S2. Preparation of double-layer hollow carbon spheres: The solid double-layer silica sphere obtained in step S1 is carbonized in an inert gas to obtain a carbonized solid double-layer silica sphere, and then SiO is etched with hydrofluoric acid. 2 A double-layer hollow carbon sphere solution is obtained, and finally washed with deionized water and dried to obtain a double-layer hollow carbon sphere; S3. Preparation of a composite material having a double-layer hollow sphere structure: The double-layer hollow carbon spheres prepared in step S2 are reacted with a silane coupling agent solution, and then vacuum filtered and dried. The double-layer hollow carbon spheres are then dispersed in an organic solution. Finally, the double-layer hollow carbon sphere organic solution is mixed and stirred with a composite material resin, and allowed to stand and dry to obtain a friction damping vibration reduction material with a double-layer hollow structure.

2. The method for preparing the friction damping and vibration reduction material having a double-layer hollow structure according to claim 1, It is characterized in that In the step S1, the volume ratio of formaldehyde, tetrabutyl silicate, deionized water, ammonia water and anhydrous ethanol is 1:(3-7):(11-26):(3-8):(83-187), and the mass ratio of resorcinol to deionized water in the step S1 is 1:(20-35).

3. The method for preparing the friction damping and vibration reduction material having a double-layer hollow structure according to claim 1, It is characterized in that In the step S1, after adding tetrabutyl silicate, resorcinol and formaldehyde to the solution, the sealed stirring time is 6-10 hours, the second addition of tetrabutyl silicate in the step S1 is continued for stirring for 24-30 hours, the solution in the step S1 reacts in the reactor for 12-24 hours, and the reaction temperature is 180°C.

4. The method for preparing the friction damping and vibration reduction material having a double-layer hollow structure according to claim 1, It is characterized in that In step S2, the inert gas is nitrogen or argon, and the carbonization temperature is 500-700°C.

5. The method for preparing the friction damping and vibration reduction material having a double-layer hollow structure according to claim 1, It is characterized in that In step S2, hydrofluoric acid etches SiO 2 The steps are: The carbonized solid double-layer silica spheres were first statically etched for 6 h and then ultrasonically etched for 2 h.

6. The method for preparing the friction damping and vibration reduction material having a double-layer hollow structure according to claim 1, It is characterized in that The organic solution for dispersing the double-layer hollow carbon spheres in step S3 is ethanol or acetone solution.

7. The method for preparing the friction damping and vibration reduction material having a double-layer hollow structure according to claim 1, It is characterized in that The composite material resin in step S3 is a pure resin composite material or a fiber-reinforced resin-based composite material.

8. A friction damping and vibration reduction material with a double-layer hollow structure, It is characterized in that The friction damping and vibration reduction material with a double-layer hollow structure is prepared according to the preparation method of any one of claims 1 to 7.

9. The friction damping vibration reduction material prepared by the method for preparing the friction damping vibration reduction material with a double-layer hollow structure according to any one of claims 1 to 7 or the friction damping vibration reduction material according to claim 8, It is characterized in that The friction damping vibration reduction material is applied to industrial vibration reduction materials.

Citation Information

Patent Citations

  • Polymer-matrix composite material and preparation method thereof

    CN104725778A

  • Carbon-based material with bowl-in-ball structure and preparation method of carbon-based material

    CN117735528A

  • Nonaqueous vibration damper composition

    JP2016044234A