Thickening type vinyl resin as well as preparation method and application thereof

By adjusting the ratio of magnesium oxide and isocyanate, and using its synergistic effect, the problems of low thickening efficiency and high cost of vinyl resin are solved, rapid thickening and stability are achieved, the viscosity needs of sheet molding materials are met, and the viscosity of the sheet molding materials is improved. Production efficiency and material properties.

CN118931116AInactive Publication Date: 2024-11-12SHANDONG WANGLIN NEW MATERIALS CO LTD +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411406032.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has problems of low efficiency, high cost and difficulty in controlling viscosity in the thickening process of vinyl resins. Especially when magnesium oxide or isocyanate alone, it cannot meet the viscosity requirements of sheet molding materials.

Method used

By adjusting the ratio of magnesium oxide and isocyanate, the synergistic effect of oxidized magnesium oxide and isocyanate is used to achieve rapid thickening of vinyl resin, combining low-shrinkage additives and fillers to optimize the resin structure and performance.

Benefits of technology

The rapid thickening of vinyl resin is achieved, meeting the different viscosity requirements of sheet molding materials, improving production efficiency and material performance, and does not require complex thickening additives and promoters to regulate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a thickening vinyl resin and a preparation method and application thereof, and belongs to the technical field of composite materials. The thickening type vinyl resin is prepared from the following components in parts by mass: 95 to 105 parts of a commercially available vinyl resin raw material, 40 to 60 parts of a low-shrinkage additive, 200 to 300 parts of filler and 1 to 5 parts of a thickening agent, the thickening agent is composed of isocyanate and magnesium oxide, and the mass ratio of the magnesium oxide to the isocyanate is 1: (1-5). According to the invention, the synergistic effect of magnesium oxide and isocyanate is utilized, and the ratio of magnesium oxide to isocyanate is adjusted, so that rapid thickening of vinyl resin is realized, and different viscosity requirements of the particle size of the sheet molding compound are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to a thickening vinyl resin and a preparation method and application thereof. Background Art

[0002] The sheet molding compound molding process is an advanced composite material molding process, and the key link in the preparation is the thickening of the resin. Vinyl resin is an addition reaction product of an epoxy resin and an unsaturated monobasic acid containing an olefinic bond. The development of vinyl resin sheet molding compounds has attracted much attention from various countries. Due to the low initial viscosity of vinyl resin, the fiber content in its sheet molding compound can be increased to more than 50%. The products have the characteristics of light weight, high strength, and excellent corrosion resistance, and their performance is better than that of traditional unsaturated polyester sheet molding compounds.

[0003] In the prior art, there are three main methods for thickening vinyl resins; the first is to thicken unsaturated polyesters with magnesium oxide, and the carboxyl groups of the resin are coordinated with magnesium oxide to form a network structure, thereby increasing the viscosity of the system. Since vinyl resins have no terminal carboxyl groups, the viscosity requirements of sheet molding materials cannot be achieved by combining only the hydroxyl groups in the vinyl group with magnesium oxide. Therefore, the method of thickening vinyl resins using only magnesium oxide has major defects. The second is to introduce unsaturated dibasic acids during the synthesis of vinyl. Patent application CN103910855B discloses a vinyl ester resin and a preparation method thereof, which achieves the purpose of thickening by the carboxyl groups provided by the unsaturated dibasic acid, but the speed of this thickening is still limited. The third is to achieve the purpose of thickening by changing the thickener. Patent application CN105713173B discloses the use of toluene diisocyanate as a thickener, but the thickening method of this patent is to add thickening aids and thickening promoters to improve the thickening effect, which undoubtedly increases the manufacturing cost. Summary of the invention

[0004] The technical problem to be solved by the present invention is: to overcome the deficiencies of the prior art and provide a thickening vinyl resin and a preparation method and application thereof; the present invention utilizes the synergistic effect of magnesium oxide and isocyanate, and by adjusting the ratio of magnesium oxide and isocyanate, the rapid thickening of the vinyl resin is achieved, thereby meeting the different viscosity requirements of sheet molding compounds.

[0005] The technical solution adopted by the present invention to solve the technical problem is: the thickening vinyl resin, in parts by mass, includes the following components: 95-105 parts of commercially available vinyl resin raw materials, 40-60 parts of low shrinkage additives, 200-300 parts of fillers, and 1-5 parts of thickeners; the thickener is composed of isocyanate and magnesium oxide, and the mass ratio of magnesium oxide to isocyanate is 1:1-5. When the ratio of the two is less than this range, the thickening effect will not meet the requirements of sheet molding compounds, and when the ratio of the two is greater than this range, excessive thickening will result; the particle size of the magnesium oxide is 800 mesh, and the magnesium oxide of this particle size has a fast reaction speed, which can significantly improve production efficiency. The ability of magnesium oxide to combine with hydroxyl groups in vinyl is limited. If magnesium oxide is added alone as a thickener, the viscosity cannot meet the viscosity requirements of sheet molding compounds; isocyanate combines quickly with hydroxyl groups in vinyl. If isocyanate is added alone as a thickener, it often leads to excessively high thickening viscosity and is difficult to control. The invention utilizes the synergistic effect of magnesium oxide and isocyanate and adjusts the ratio of magnesium oxide and isocyanate to achieve rapid thickening of the vinyl resin and meet the different viscosity requirements of the sheet molding compound.

[0006] Preferably, the mass ratio of magnesium oxide to isocyanate is 1:1.5-2.5; the thickening viscosity can reach 268000-611200P, and the thickening system is stable without phase separation.

[0007] The isocyanate is toluene diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate. The three isocyanates can significantly accelerate the thickening speed of the vinyl resin, so that the resin can reach the required viscosity in a short time and improve work efficiency; the addition of isocyanate can also optimize the molecular structure of the vinyl resin, improve its toughening effect, reduce side reactions, be safe and environmentally friendly, and ensure quality stability. The vinyl resin is a bisphenol A epoxy vinyl resin, a novolac epoxy vinyl resin or a brominated bisphenol A epoxy vinyl ester resin. The bisphenol A epoxy vinyl resin, the novolac epoxy vinyl resin or the brominated bisphenol A epoxy vinyl ester resin can form good wettability with the filler, which helps to improve the overall performance of the material and ensure stability and reliability during the thickening process.

[0008] The viscosity of the commercially available vinyl resin raw material is 6-10P; the commercially available vinyl resin raw material has a lower viscosity in the initial stage, which is convenient for construction and mixing, and can quickly thicken to reach the required consistency, which is crucial to ensuring construction quality and efficiency.

[0009] The low shrinkage additive is polystyrene, polymethyl methacrylate or polyvinyl acetate; the main function of the low shrinkage additive is to release internal stress through local relaxation and compensate for polymerization shrinkage, thereby achieving the effect of reducing shrinkage. The low shrinkage additive can delay the resin curing process, thereby proving its effectiveness in controlling material shrinkage; in addition, the low shrinkage additive can also optimize the processing performance of the material, improve production efficiency and product quality.

[0010] The filler is calcium carbonate or quartz sand, the particle size of the calcium carbonate is 400 meshes, and calcium carbonate can reduce the shrinkage rate of the resin, improve the rheological state, and control the viscosity, thereby improving the stability of the vinyl resin. The particle size of the quartz sand is 325 meshes, and this particle size can ensure that the quartz sand is evenly distributed in the resin, thereby enhancing the fluidity of the resin, improving the thickening effect, and optimizing the performance of the resin.

[0011] According to another aspect of the present invention, there is also provided a method for thickening a vinyl resin, comprising the following steps: (1) uniformly mixing a commercially available vinyl resin raw material and a low shrinkage additive to obtain component A; (2) Mix the filler and component A evenly to obtain component B; (3) The thickener and component B are mixed evenly, and baked to obtain a thickening vinyl resin.

[0012] The baking temperature in step (3) is 40-50°C and the time is 20-30 hours; preferably, the baking temperature is 45°C and the time is 24 hours; the preferred baking temperature can ensure that the resin is uniformly cured during the baking process, while avoiding excessively high temperature causing the resin to cure too quickly or performance degradation; the preferred baking temperature and time can fully cure the thickened resin system to achieve the best performance state, and a viscosity test can more accurately reflect the actual performance of the cured resin.

[0013] The mixing in step (1), step (2) and step (3) is all carried out under closed conditions. This is because the temperature rises during the stirring process and the closed conditions can minimize the volatilization of styrene.

[0014] In step (1), the vinyl resin and the low shrinkage additive are mixed and stirred at a speed of 400-800 r / min for 3-8 min; in step (2), the filler and component A are mixed and stirred at a speed of 800-1200 r / min for 8-12 min; in step (3), the thickener and component B are mixed until a homogeneous phase without stratification or agglomeration is formed at a speed of 1000-1400 r / min for 1-5 min; According to another aspect of the present invention, the present invention also provides use of the thickened vinyl resin in sheet molding compounds.

[0015] Compared with the prior art, the present invention has the following beneficial effects: (1) The ability of magnesium oxide to bind to the hydroxyl groups in vinyl is limited, which is the key factor affecting the thickening viscosity. Isocyanate binds to the hydroxyl groups in vinyl quickly, which often leads to excessively high thickening viscosity and difficulty in control. The present invention utilizes the synergistic effect of magnesium oxide and isocyanate, and by adjusting the ratio of magnesium oxide and isocyanate, the rapid thickening of the vinyl resin is achieved, thereby meeting the different viscosity requirements of sheet molding compounds.

[0016] (2) The present invention adopts two thickeners, magnesium oxide and isocyanate, for the first time, and realizes the rapid thickening of the vinyl resin by utilizing the chain extension reaction between the hydroxyl groups in the vinyl resin and isocyanate and magnesium oxide.

[0017] (3) The present invention does not require complicated regulation of thickening aids and thickening promoters, and achieves thickening of the vinyl resin through a simple process flow without changing the vinyl resin formula. DETAILED DESCRIPTION

[0018] Embodiment 6 is the best embodiment of the present invention. The present invention will be further described below in conjunction with specific embodiments and comparative examples.

[0019] The chemical additives used in the examples and comparative examples of the present invention are all commercially available, and their specific information is as follows: Bisphenol A epoxy vinyl resin: industrial grade, brand WL-9001, purchased from Zibo Wanglin New Material Technology Co., Ltd.; phenolic epoxy vinyl resin: industrial grade, purchased from Dacheng County Shengxing Anticorrosive Materials Business Department; brominated bisphenol A epoxy vinyl ester resin: industrial grade, Hubei Dali Chemical Co., Ltd.; polystyrene: industrial grade, brand WL-3803, purchased from Zibo Wanglin New Material Technology Co., Ltd.; polymethyl methacrylate: industrial grade, purchased from Dongguan Baojia Plastic Co., Ltd.; polyvinyl acetate: industrial grade, Purchased from Jiangsu Bosite Chemical Technology Co., Ltd.; isophorone diisocyanate: industrial grade, purchased from Shanghai Hongzhuang Chemical Technology Co., Ltd.; diphenylmethane diisocyanate: industrial grade, purchased from Jinan Hongwang Chemical Co., Ltd.; toluene diisocyanate: industrial grade, purchased from Wanhua Chemical Group Co., Ltd.; quartz sand: industrial grade, Lingshou County Chengnuo Mineral Products Co., Ltd.; calcium carbonate: industrial grade, model GY-106, purchased from Jiangxi Guangyuan Chemical Co., Ltd.; magnesium oxide: industrial grade, purchased from Shandong Shengwolun Chemical Technology Co., Ltd.

[0020] Example 1 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of bisphenol A epoxy resin and 50 parts of polystyrene were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 1 part of magnesium oxide and 3 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 min to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 45°C for 24 h.

[0021] Example 2 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of bisphenol A epoxy resin and 50 parts of polystyrene were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 1 part of magnesium oxide and 4 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 min to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 45° C. for 24 h.

[0022] Example 3 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of bisphenol A epoxy resin and 50 parts of polystyrene were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 1 part of magnesium oxide and 5 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 min to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 45° C. for 24 h.

[0023] Example 4 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of bisphenol A epoxy resin and 50 parts of polystyrene were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 2 parts of magnesium oxide and 3 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 minutes to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 45° C. for 24 hours.

[0024] Example 5 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of bisphenol A epoxy resin and 50 parts of polystyrene were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 2 parts of magnesium oxide and 4 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 minutes to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 45° C. for 24 hours.

[0025] Example 6 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of bisphenol A epoxy resin and 50 parts of polystyrene were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 2 parts of magnesium oxide and 5 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 minutes to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 45° C. for 24 hours.

[0026] Example 7 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of bisphenol A epoxy resin and 50 parts of polystyrene were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 1 part of magnesium oxide and 1 part of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 min to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 45° C. for 24 h.

[0027] Example 8 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of bisphenol A epoxy resin and 50 parts of polystyrene were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 2 parts of magnesium oxide and 5 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 minutes to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 40° C. for 30 hours.

[0028] Example 9 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of bisphenol A epoxy resin and 50 parts of polystyrene were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 2 parts of magnesium oxide and 5 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 minutes to obtain a vinyl resin thickening system, which was baked at 50° C. for 20 hours and then its viscosity was measured.

[0029] Example 10 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of phenolic epoxy vinyl resin and 50 parts of polymethyl methacrylate were stirred in a closed container at a speed of 600 r / min for 5 minutes to obtain component A; (2) 250 parts of quartz sand and component A were stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 2 parts of magnesium oxide and 5 parts of isophorone diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 minutes to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 45°C for 24 hours.

[0030] Embodiment 11 A method for preparing a thickening vinyl resin comprises the following steps: (1) 100 parts of brominated bisphenol A epoxy resin and 50 parts of polyvinyl acetate were stirred at a speed of 600 r / min for 5 minutes in a closed container to obtain component A; (2) 250 parts of quartz sand and component A were stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 2 parts of magnesium oxide and 5 parts of diphenylmethane diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1200 r / min for 3 minutes to obtain a vinyl resin thickening system, and its viscosity was measured after baking at 45° C. for 24 hours.

[0031] Example 12 A method for preparing a thickening vinyl resin comprises the following steps: (1) 95 parts of bisphenol A epoxy resin and 40 parts of polystyrene were stirred at a speed of 400 r / min for 3 minutes in a closed container to obtain component A; (2) 200 parts of calcium carbonate and component A are stirred in a closed container in step (1) at a speed of 800 r / min for 8 minutes to obtain component B; (3) 2 parts of magnesium oxide and 5 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1000 r / min for 1 min to obtain a vinyl resin thickening system, which was baked at 45° C. for 24 h and then its viscosity was measured.

[0032] Embodiment 13 A method for preparing a thickening vinyl resin comprises the following steps: (1) 105 parts of brominated bisphenol A epoxy resin and 60 parts of polystyrene were stirred at a speed of 800 r / min for 8 minutes in a closed container to obtain component A; (2) 300 parts of calcium carbonate and component A were stirred in a closed container in step (1) at a speed of 1000 r / min for 10 min to obtain component B; (3) 2 parts of magnesium oxide and 5 parts of toluene diisocyanate were stirred with component B in a sealed container in step (1) at a speed of 1400 r / min for 5 minutes to obtain a vinyl resin thickening system, which was baked at 45° C. for 24 hours and then its viscosity was measured.

[0033] Comparative Example 1 The preparation method of a thickening vinyl resin described in this comparative example is the same as that in Example 6, except that the magnesium oxide powder in step (3) is 2 parts and toluene diisocyanate is not added.

[0034] Comparative Example 2 The preparation method of a thickening vinyl resin described in this comparative example is the same as that in Example 6, the only difference is that in step (3), 5 parts of toluene diisocyanate are added and magnesium oxide is not added.

[0035] Comparative Example 3 The preparation method of a thickening vinyl resin described in this comparative example is the same as that of Example 6, except that 2 parts of magnesium oxide and 12 parts of toluene diisocyanate are added in step (3).

[0036] Comparative Example 4 The preparation method of a thickening vinyl resin described in this comparative example is the same as that of Example 6, except that 1 part of magnesium oxide and 0.5 part of toluene diisocyanate are added in step (3).

[0037] Performance Testing The performance of the thickening vinyl resin prepared in the examples and comparative examples was tested. The specific test results are shown in Table 1.

[0038] The viscosity was tested using an RVTV-2H high temperature rotary viscometer; Viscosity requirements for sheet molding compounds: 45°C thickening for 24 hours to reach a viscosity of 200,000p; Stability is determined by observing whether stratification and precipitation occur during baking.

[0039] Table 1 Performance data of vinyl resin in examples and comparative examples .

[0040] As shown in Table 1, the thickening viscosity of the embodiments is above 200000P, and the thickening system is stable without phase separation and precipitation. The present invention does not require complex regulation of thickening aids and thickening promoters, and achieves thickening of the vinyl resin through a simple process without changing the vinyl resin formula.

[0041] It can be seen from the results of Comparative Example 1 that when magnesium oxide is added alone as a thickener, the viscosity cannot meet the viscosity requirements of sheet molding compound due to the limited ability of magnesium oxide to bind to the hydroxyl groups in the vinyl group; it can be seen from the results of Comparative Example 2 that when isocyanate is added alone as a thickener, the isocyanate binds to the hydroxyl groups in the vinyl group quickly, resulting in difficulty in controlling the thickening viscosity. The present invention uses two thickeners, magnesium oxide and isocyanate, for the first time, and utilizes the chain extension reaction of the hydroxyl groups in the vinyl resin with isocyanate and magnesium oxide; it achieves rapid thickening of the vinyl resin. It can be seen from the results of Comparative Examples 3 and 4 that when the mass ratio of magnesium oxide to isocyanate in the thickener exceeds the range of the present invention, the thickening viscosity cannot meet the requirements of the sheet molding compound.

[0042] In summary, the present invention utilizes the synergistic effect of magnesium oxide and isocyanate and adjusts the ratio of magnesium oxide to isocyanate to achieve rapid thickening of the vinyl resin and meet the different viscosity requirements of the sheet molding compound.

[0043] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A thickening vinyl resin, characterized in that: The invention comprises the following components in parts by mass: 95-105 parts of commercially available vinyl resin raw materials, 40-60 parts of low shrinkage additives, 200-300 parts of fillers, and 1-5 parts of thickeners; the thickeners are composed of isocyanate and magnesium oxide, and the mass ratio of magnesium oxide to isocyanate is 1:1-5.

2. A thickening vinyl resin according to claim 1, characterized in that: The mass ratio of the magnesium oxide to the isocyanate is 1:1.5-2.

5.

3. A thickening vinyl resin according to claim 1, characterized in that: The isocyanate is toluene diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate.

4. A thickening vinyl resin according to claim 1, characterized in that: The vinyl resin is bisphenol A epoxy vinyl resin, novolac epoxy vinyl resin or brominated bisphenol A epoxy vinyl ester resin.

5. A thickening vinyl resin according to claim 1, characterized in that: The viscosity of the commercially available vinyl resin raw material is 6-10P.

6. A thickening vinyl resin according to claim 1, characterized in that: The low shrinkage additive is polystyrene, polymethyl methacrylate or polyvinyl acetate.

7. A thickening vinyl resin according to claim 1, characterized in that: The filler is calcium carbonate or quartz sand.

8. A method for preparing the thickening vinyl resin according to any one of claims 1 to 7, characterized in that it comprises the following steps: (1) uniformly mixing a commercially available vinyl resin raw material and a low shrinkage additive to obtain component A; (2) Mix the filler and component A evenly to obtain component B; (3) The thickener and component B are mixed evenly, and baked to obtain a thickening vinyl resin.

9. The method for preparing a thickening vinyl resin according to claim 8, characterized in that: The baking temperature in step (3) is 40-50°C and the baking time is 20-30h.

10. Use of the thickening vinyl resin according to any one of claims 1 to 7 in sheet molding compounds.

Citation Information

Patent Citations

  • A kind of vinyl ester resin and preparation method thereof

    CN103910855B

  • A thickening formulation and thickening method for a vinyl ester resin matrix.

    CN105713173B

  • Carbon fiber reinforced vinyl ester resin SMC (Sheet Molding Compound) prepreg as well as preparation method and use method thereof

    CN106750444A