High-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material and preparation method thereof

By using aromatic polycarbonate, polyether etherketone and other materials in polycarbonate composite materials and combining components such as Elosite nanotubes and combined with extruder thermoforming process, the polycarbonate composite material is solved in the resistance of polycarbonate composite materials. The lack of combustion, antistatic and gloss is achieved, and high gloss, halogen-free flame retardant, permanent antistatic and superhydrophobic properties are suitable for a variety of application scenarios.

CN118931143APending Publication Date: 2024-11-12GUANGDONG GERUI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411006657.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing polycarbonate composite materials lack excellent flame retardancy, permanent antistatic properties and high gloss in the electronic and electrical fields, and it is difficult to achieve easy cleaning and superhydrophobicity.

Method used

Using aromatic polycarbonate, polyether ether ketone, polyaniline modified elolite nanotubes, hydroquinone bis(diphenyl phosphate), MBS core-shell graft copolymer, nanobarium sulfate powder and ABS The combination of high-gloss masterbatches combined with the thermoforming process of twin-screw extruders to form a high-gloss, halogen-free flame-retardant, permanent anti-static polycarbonate composite material.

Benefits of technology

It realizes the excellent mechanical properties, flame resistance, permanent anti-static properties and high gloss of polycarbonate composite materials, and gives it superhydrophobicity and easy cleaning, which is suitable for a variety of application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004963182550000091
    Figure BDA0004963182550000091
Patent Text Reader

Abstract

The invention discloses a high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material and a preparation method thereof. Comprising the following components in parts by weight: 90 to 120 parts of aromatic polycarbonate, 20 to 40 parts of polyether-ether-ketone, 5 to 15 parts of polyaniline modified halloysite nanotube, 5 to 10 parts of hydroquinone bis (phenyl diphenyl phosphate), 1 to 5 parts of MBS core-shell graft copolymer, 2 to 5 parts of nano barium sulfate powder, 1 to 3 parts of ABS highlight master batch, 0.1 to 0.5 part of antioxidant and 0.2 to 0.5 part of light stabilizer. On the premise of ensuring excellent mechanical properties, the flame-retardant antistatic plastic has excellent flame retardance, permanent antistatic property and high surface glossiness; meanwhile, the super-hydrophobicity is also endowed, and the good easy-to-clean property is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polycarbonate composite materials and relates to a high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material and a preparation method thereof. Background Art

[0002] Polycarbonate (PC) composite material is an engineering plastic with excellent performance. It is composed of polycarbonate resin and various reinforcing materials (such as glass fiber, carbon fiber, etc.). This material combines the transparency, impact resistance, and temperature resistance of polycarbonate with the high strength and rigidity of reinforcing materials, making it widely used in many fields, such as: automotive industry, electronics and electrical, construction industry, medical equipment, aerospace, sports equipment, etc. Due to its excellent comprehensive performance, polycarbonate composite materials are gradually replacing traditional glass materials and playing an increasingly important role in modern industry. With the advancement of materials science, its application areas are still expanding. Different application scenarios have different focuses on the performance of polycarbonate composite materials.

[0003] Patent CN 106674875 A discloses a high-gloss, easy-to-clean, flame-retardant PC / ABS composite material, characterized in that it is made of the following components in parts by weight: 80-85 parts of acrylonitrile-butadiene-styrene copolymer, 10-15 parts of polycarbonate-g-polystyrene copolymer, 4-8 parts of spray-free high-gloss functional masterbatch, 0.5-1 parts of toughening agent, 0.3-0.6 parts of graphene / nickel-iron double hydroxide, 0.5-1 parts of inorganic filler, 1-2 parts of light stabilizer, 0.5-1 parts of antistatic agent, 0.15-0.5 parts of dispersant, and 0.5-3 parts of colorant.

[0004] Patent CN 109627735 A discloses an antistatic and antibacterial PC / ASA material, a preparation method and an application thereof. The antistatic and antibacterial PC / ASA material comprises the following components in parts by weight: PC resin: 30-55 parts, ASA resin: 15-30 parts, antistatic agent: 10-25 parts, calcium carbonate: 5-15 parts, methyl methacrylate-butadiene-styrene terpolymer: 3-10 parts, antibacterial agent: 1-3.5 parts, light stabilizer: 0.3-

[0005] 1.5 parts, processing aids: 0.5-1.5 parts.

[0006] Patent CN102964796A discloses a high-gloss, anti-aging polycarbonate composite material, including polycarbonate and an additive, characterized in that the additive includes at least an anti-aging agent and a lubricant, and based on 100 parts by weight of the polycarbonate, the content of the anti-aging agent is 0.25-10 parts by weight, and the content of the lubricant is 0.25-3 parts by weight.

[0007] In the field of electronics and electrical appliances, polycarbonate materials require excellent flame retardancy to prevent fires, excellent antistatic properties to ensure the electrical safety of equipment, and high gloss to improve aesthetics. Summary of the invention

[0008] Based on the needs and deficiencies of the prior art, the present invention provides a high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material and a preparation method thereof, which has excellent flame retardancy, permanent antistatic performance, and high surface gloss while ensuring excellent mechanical properties; at the same time, it also imparts super-hydrophobicity and obtains good easy-to-clean performance.

[0009] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0010] A high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material, calculated by weight, comprises the following components:

[0011] 90-120 parts of aromatic polycarbonate,

[0012] 20-40 parts of polyetheretherketone,

[0013] 5-15 parts of polyaniline modified halloysite nanotubes,

[0014] 5-10 parts of hydroquinone bis(diphenyl phosphate),

[0015] MBS core-shell graft copolymer 1-5 parts,

[0016] 2-5 parts of nano barium sulfate powder,

[0017] ABS high gloss masterbatch 1-3 parts,

[0018] 0.1-0.5 parts of antioxidants,

[0019] Light stabilizer 0.2-0.5 parts.

[0020] Furthermore, the polycarbonate composite material comprises the following components, calculated in parts by weight:

[0021] 100-110 parts of aromatic polycarbonate,

[0022] 25-35 parts of polyetheretherketone,

[0023] 8-10 parts of polyaniline modified halloysite nanotubes,

[0024] 7-8 parts of hydroquinone bis(diphenyl phosphate),

[0025] MBS core-shell graft copolymer 3-4 parts,

[0026] 3-4 parts of nano barium sulfate powder,

[0027] ABS high gloss masterbatch 2-3 parts,

[0028] 0.2-0.4 parts of antioxidants,

[0029] Light stabilizer 0.3-0.4 parts.

[0030] Furthermore, the polycarbonate composite material is composed of the following components, calculated by weight: 100 to 110 parts of aromatic polycarbonate,

[0031] 25-35 parts of polyetheretherketone,

[0032] 8-10 parts of polyaniline modified halloysite nanotubes,

[0033] 7-8 parts of hydroquinone bis(diphenyl phosphate),

[0034] MBS core-shell graft copolymer 3-4 parts,

[0035] 3-4 parts of nano barium sulfate powder,

[0036] ABS high gloss masterbatch 2-3 parts,

[0037] 0.2-0.4 parts of antioxidants,

[0038] Light stabilizer 0.3-0.4 parts.

[0039] Furthermore, the aromatic polycarbonate is bisphenol A type polycarbonate resin.

[0040] Furthermore, the antioxidant is at least one of antioxidant 1076 or antioxidant 168.

[0041] Furthermore, the light stabilizer is one or more of bisphenol A salicylate, 2-hydroxy-4-n-octyloxy-benzophenone, and 2,4-dihydroxybenzophenone.

[0042] Furthermore, the particle size of the nano-barium sulfate powder is 200-300 nm.

[0043] The present application adopts a combination of nano barium sulfate powder and ABS high gloss masterbatch to improve the gloss of polycarbonate composite materials.

[0044] When styrene-maleic anhydride is used as a compatibilizer, its anhydride functional group may react with the end group of polycarbonate to form PC-g-SMA grafts. Since the styrene segments in styrene-maleic anhydride have good compatibility with polycarbonate, the compatibility of PC / ABS blends is improved. The notched impact strength of PC / ABS alloys compatibilized with this type of compatibilizer can be increased by more than 2 times, and the elongation at break can be increased by more than 3 times.

[0045] Halloysite is an effective inorganic flame retardant widely used to improve the flame retardant properties of materials. When heated, it expands and forms a protective barrier that isolates oxygen and heat, slowing down the combustion reaction inside the material. Halloysite has high thermal and chemical stability, can maintain its structure at high temperatures, and does not produce flammable gases, thereby reducing the combustion rate. In addition, halloysite absorbs heat during heating, which helps to reduce the temperature on the surface and inside of the material and slow down the combustion process. Halloysite nanotubes are compounded with halogen-free flame retardant bisphenol A-bis(diphenyl phosphate) as a flame retardant system for polycarbonate composites.

[0046] The prior art also studies that halloysite grafted with conductive polymers can play an antistatic role; the present invention pre-grafts the conductive polymer polyaniline on the halloysite nanotubes, which not only utilizes the flame retardancy of halloysite, but also exerts its antistatic property, without the need to add an additional antistatic agent. In addition, after the grafting of polyaniline, the dispersibility problem of the halloysite nanotubes in the polycarbonate matrix is ​​also solved.

[0047] Furthermore, the preparation method of the polyaniline modified halloysite nanotubes is:

[0048] (1) Add 100 parts of water to a reaction container, then add 1.5 to 3.5 parts of dodecyldimethylsulfonyl betaine, turn on the stirring device to mix evenly; turn on the heater to raise the solution temperature to 50 to 60° C., then add 20 to 30 parts of halloysite nanotubes, and continue stirring for 10 to 20 minutes;

[0049] (2) Add dilute hydrochloric acid to the reactor, stop adding when the pH reaches 4.6 to 4.7, and place the reactor in an ice bath at -5 to 0°C to wait for the solution temperature to stabilize;

[0050] (3) adding 5 to 10 parts of aniline monomer to the reactor, controlling the stirring rate to 10 to 15 rpm, and applying ultrasound during the stirring process; then dripping 3 to 5 parts of ammonium persulfate solution into the reactor, wherein the dripping time is controlled to be 20 to 30 minutes;

[0051] (4) The reaction solution of step (3) is filtered and washed with anhydrous ethanol and deionized water for 2 to 3 times, and the solid component is placed in a drying oven for drying to obtain polyaniline-modified halloysite nanotubes.

[0052] Furthermore, the polycarbonate composite material has a glossiness greater than 85° and a surface water contact angle greater than 130°.

[0053] A method for preparing a high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material comprises the following steps:

[0054] (1) Weigh the components in proportion for later use;

[0055] (2) Pour aromatic polycarbonate, polyetheretherketone, polyaniline modified halloysite nanotubes, hydroquinone bis(diphenyl phosphate), and MBS core-shell graft copolymer according to weight parts into a stirring device and stir evenly to form material group A; pour nano barium sulfate powder, ABS high gloss masterbatch, antioxidant, and light stabilizer according to weight parts into a stirring device and stir evenly to form material group B;

[0056] (3) Material group A is fed from the main feed of a twin-screw extruder, and material group B is fed from the side feed of the twin-screw extruder, and the mixture is melted, mixed, and extruded through the twin-screw extruder to obtain a polycarbonate composite material.

[0057] Furthermore, the set temperature of the twin-screw extruder is: section one: 210-230°C, section two: 215-235°C, section three: 220-240°C, section four: 225-245°C, section five: 210-230°C, section six: 210-230°C, section seven: 215-235°C, section eight: 215-235°C, section nine: 220-240°C, and die head: 225-245°C.

[0058] Furthermore, the rotation speed of the twin-screw extruder is 200-250 rpm.

[0059] The high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material and the preparation method thereof provided by the present invention have the following beneficial effects compared with the prior art:

[0060] (1) The present application uses aromatic polycarbonate and polyetheretherketone as main raw materials to form a blended alloy system, which greatly improves the mechanical properties and compatibility of polycarbonate materials and provides a basic guarantee for the application of composite materials.

[0061] (2) The present application forms a composite material with high gloss, halogen-free flame retardancy and long-term antistatic properties by compounding polyaniline-modified halloysite nanotubes, hydroquinone bis(diphenyl phosphate), MBS core-shell graft copolymer, nano-barium sulfate powder and ABS high-gloss masterbatch with polycarbonate. The composite material has a wide range of applications. DETAILED DESCRIPTION

[0062] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0063] Main raw materials: Aromatic polycarbonate is bisphenol A type polycarbonate resin, a product of Luxi Chemical Group Co., Ltd., brand: LXTY1920-01; polyetheretherketone is a product of Victrex, UK, brand: 450GL30; MBS core-shell graft copolymer is a product of Mitsubishi Chemical, Japan, brand: S-2001.

[0064] The preparation method of polyaniline modified halloysite nanotubes is as follows:

[0065] (1) Add 100 parts of water to a reaction container, then add 2 parts of dodecyldimethylsulfonyl betaine, turn on the stirring device to mix evenly; turn on the heater to raise the solution temperature to 53° C., then add 25 parts of halloysite nanotubes, and continue stirring for 15 minutes;

[0066] (2) Add dilute hydrochloric acid to the reactor, stop adding when the pH reaches 4.6, and place the reactor in an ice bath at -5°C until the solution temperature stabilizes;

[0067] (3) adding 7 parts of aniline monomer to the reactor, controlling the stirring rate at 10 rpm, and applying ultrasound during the stirring process; then dropping 4 parts of ammonium persulfate solution into the reactor, wherein the dropping time is controlled to be 25 min;

[0068] (4) The reaction solution of step (3) is filtered and washed with anhydrous ethanol and deionized water for three times, and the solid component is placed in a drying oven for drying to obtain polyaniline-modified halloysite nanotubes.

[0069] In the following examples and comparative examples, the raw materials used were those mentioned above unless otherwise specified.

[0070] Example 1

[0071] A high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material, calculated by weight, consists of the following components:

[0072] 100 parts of aromatic polycarbonate,

[0073] 25 parts of polyetheretherketone,

[0074] 8 parts of polyaniline modified halloysite nanotubes,

[0075] 7 parts of hydroquinone bis(diphenyl phosphate),

[0076] MBS core-shell graft copolymer 3 parts,

[0077] 3 parts of nano barium sulfate powder,

[0078] ABS high gloss masterbatch 2 parts,

[0079] 0.2 parts of antioxidant,

[0080] 0.3 parts of light stabilizer.

[0081] Wherein, the antioxidant is antioxidant 1076;

[0082] Wherein, the light stabilizer is bisphenol A salicylate;

[0083] Wherein, the particle size of the nano barium sulfate powder is 200nm.

[0084] A method for preparing a high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material comprises the following steps:

[0085] (1) Weigh the components in proportion for later use;

[0086] (2) Pour aromatic polycarbonate, polyetheretherketone, polyaniline modified halloysite nanotubes, hydroquinone bis(diphenyl phosphate), and MBS core-shell graft copolymer according to weight parts into a stirring device and stir evenly to form material group A; pour nano barium sulfate powder, ABS high gloss masterbatch, antioxidant, and light stabilizer according to weight parts into a stirring device and stir evenly to form material group B;

[0087] (3) adding material group A from the main feed of a twin-screw extruder and adding material group B from the side feed of the twin-screw extruder, melting, mixing and extruding through the twin-screw extruder to obtain a polycarbonate composite material;

[0088] The set temperatures of the twin-screw extruder are: first section: 210°C, second section: 215°C, third section: 220°C, fourth section: 225°C, fifth section: 210°C, sixth section: 210°C, seventh section: 215°C, eighth section: 215°C, ninth section: 220°C, die head: 225°C.

[0089] Wherein, the rotation speed of the twin-screw extruder is 200 rpm.

[0090] Example 2

[0091] A high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material, calculated by weight, consists of the following components:

[0092] 110 parts of aromatic polycarbonate,

[0093] 35 parts of polyetheretherketone,

[0094] 10 parts of polyaniline modified halloysite nanotubes,

[0095] 8 parts of hydroquinone bis(diphenyl phosphate),

[0096] MBS core-shell graft copolymer 4 parts,

[0097] 4 parts of nano barium sulfate powder,

[0098] ABS high gloss masterbatch 3 parts,

[0099] 0.4 parts of antioxidant,

[0100] Light stabilizer 0.4 parts

[0101] Wherein, the antioxidant is antioxidant 168;

[0102] Wherein, the light stabilizer is 2-hydroxy-4-n-octyloxy-benzophenone;

[0103] Wherein, the particle size of the nano barium sulfate powder is 300nm.

[0104] A method for preparing a high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material comprises the following steps:

[0105] (1) Weigh the components in proportion for later use;

[0106] (2) Pour aromatic polycarbonate, polyetheretherketone, polyaniline modified halloysite nanotubes, hydroquinone bis(diphenyl phosphate), and MBS core-shell graft copolymer according to weight parts into a stirring device and stir evenly to form material group A; pour nano barium sulfate powder, ABS high gloss masterbatch, antioxidant, and light stabilizer according to weight parts into a stirring device and stir evenly to form material group B;

[0107] (3) adding material group A from the main feed of a twin-screw extruder and adding material group B from the side feed of the twin-screw extruder, melting, mixing and extruding through the twin-screw extruder to obtain a polycarbonate composite material;

[0108] The set temperatures of the twin-screw extruder are: first section: 230°C, second section: 235°C, third section: 240°C, fourth section: 245°C, fifth section: 230°C, sixth section: 230°C, seventh section: 235°C, eighth section: 235°C, ninth section: 240°C, die head: 245°C.

[0109] Wherein, the rotation speed of the twin-screw extruder is 250 rpm.

[0110] Example 3

[0111] A high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material, calculated by weight, consists of the following components:

[0112] 105 parts of aromatic polycarbonate,

[0113] 30 parts of polyetheretherketone,

[0114] 9 parts of polyaniline modified halloysite nanotubes,

[0115] 8 parts of hydroquinone bis(diphenyl phosphate),

[0116] MBS core-shell graft copolymer 3 parts,

[0117] 3.5 parts of nano barium sulfate powder,

[0118] ABS high gloss masterbatch 2 parts,

[0119] 0.3 parts of antioxidant,

[0120] Light stabilizer 0.4 parts

[0121] Wherein, the antioxidant is antioxidant 168;

[0122] Wherein, the light stabilizer is 2,4-dihydroxybenzophenone;

[0123] Wherein, the particle size of the nano barium sulfate powder is 250nm.

[0124] A method for preparing a high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material comprises the following steps:

[0125] (1) Weigh the components in proportion for later use;

[0126] (2) Pour aromatic polycarbonate, polyetheretherketone, polyaniline modified halloysite nanotubes, hydroquinone bis(diphenyl phosphate), and MBS core-shell graft copolymer according to weight parts into a stirring device and stir evenly to form material group A; pour nano barium sulfate powder, ABS high gloss masterbatch, antioxidant, and light stabilizer according to weight parts into a stirring device and stir evenly to form material group B;

[0127] (3) adding material group A from the main feed of a twin-screw extruder and adding material group B from the side feed of the twin-screw extruder, melting, mixing and extruding through the twin-screw extruder to obtain a polycarbonate composite material;

[0128] The set temperatures of the twin-screw extruder are: first section: 220°C, second section: 225°C, third section: 230°C, fourth section: 235°C, fifth section: 230°C, sixth section: 230°C, seventh section: 235°C, eighth section: 235°C, ninth section: 230°C, die head: 235°C;

[0129] Wherein, the rotation speed of the twin-screw extruder is 230rmp.

[0130] Comparative Example 1

[0131] Comparative Example 1 is substantially the same as Example 3, except that only halloysite nanotubes are used in Comparative Example 1.

[0132] Comparative Example 2

[0133] Comparative Example 2 is substantially the same as Example 3, except that hydroquinone bis(diphenyl phosphate) is not added in Comparative Example 2.

[0134] Comparative Example 3

[0135] Comparative Example 3 is substantially the same as Example 3, except that in Comparative Example 3, neither polyaniline-modified halloysite nanotubes nor halloysite nanotubes are added.

[0136] The polycarbonate composite materials prepared in Examples 1-3 and Comparative Examples 1-3 were measured.

[0137] (1) Tensile strength: According to the standard GB / T 1040 “Test method for tensile properties of plastics”, the tensile properties of the specimens were tested using a universal material testing machine at a tensile rate of 60 mm / min.

[0138] (2) Izod notched impact strength: The specimens were prepared in accordance with the standard GB / T1043.1-2008. The specimens were made into a B-type notch using a notch making machine. The notch depth was 3 mm and the pendulum impact energy was 4 J. The Izod notched impact strength was measured on a pendulum impact tester.

[0139] (3) Gloss: Use a surface gloss tester to test at 60° in accordance with GB88072-1988. Clean the surface of the sample and lay it flat. Place the gloss tester on it, press it tightly and select a suitable angle for testing. The reading obtained is the gloss.

[0140] (4) Surface resistance: Use a resistance meter to measure the resistance of the sample surface.

[0141] (5) Flame retardancy: According to the UL94 standard "Plastic combustion performance test method horizontal method and vertical method", the combustion level of the sample is tested using a horizontal and vertical combustion tester.

[0142] (6) Contact angle: Drop a drop of water on the surface of a polycarbonate sample and measure its contact angle.

[0143] The specific data of the above tests are recorded in Table 1.

[0144] Table 1

[0145]

[0146] It can be seen from the data in Table 1 that the polycarbonate composite material prepared by the present invention has excellent mechanical properties, and its tensile strength exceeds 60 MPa; it has high gloss plating, excellent antistatic properties, and flame retardancy, and the contact angle data can show that the surface of the polycarbonate composite material has super hydrophobicity.

[0147] In particular, the flame retardancy levels of Example 3 and Comparative Examples 1-3 indicate that the halloysite nanotubes and hydroquinone bis(diphenyl phosphate) have a synergistic flame retardancy effect.

[0148] In addition, whether the halloysite nanotubes are modified with polyaniline also determines the antistatic performance of the composite material. Generally speaking, the lower the surface resistance, the better the antistatic effect. 5 Ω increased to 6.6×10 7 Ω, the surface resistance spans two orders of magnitude, which shows that the antistatic performance of Example 3 is far better than that of Comparative Example 1.

[0149] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A high gloss halogen-free flame retardant permanent antistatic polycarbonate composite material, It is characterized in that Calculated by weight, it includes the following components: 90-120 parts of aromatic polycarbonate, 20-40 parts of polyetheretherketone, 5-15 parts of polyaniline modified halloysite nanotubes, 5-10 parts of hydroquinone bis(diphenyl phosphate), MBS core-shell graft copolymer 1-5 parts, 2-5 parts of nano barium sulfate powder, ABS high gloss masterbatch 1-3 parts, 0.1-0.5 parts of antioxidants, Light stabilizer 0.2-0.5 parts.

2. A high gloss halogen-free flame retardant permanent antistatic polycarbonate composite material according to claim 1, It is characterized in that Calculated by weight, it includes the following components: 100-110 parts of aromatic polycarbonate, 25-35 parts of polyetheretherketone, 8-10 parts of polyaniline modified halloysite nanotubes, 7-8 parts of hydroquinone bis(diphenyl phosphate), MBS core-shell graft copolymer 3-4 parts, 3-4 parts of nano barium sulfate powder, ABS high gloss masterbatch 2-3 parts, 0.2-0.4 parts of antioxidants, Light stabilizer 0.3-0.4 parts.

3. A high gloss halogen-free flame retardant permanent antistatic polycarbonate composite material according to any one of claims 1 to 2, It is characterized in that Calculated by weight, it is composed of the following components: 100-110 parts of aromatic polycarbonate, 25-35 parts of polyetheretherketone, 8-10 parts of polyaniline modified halloysite nanotubes, 7-8 parts of hydroquinone bis(diphenyl phosphate), MBS core-shell graft copolymer 3-4 parts, 3-4 parts of nano barium sulfate powder, ABS high gloss masterbatch 2-3 parts, 0.2-0.4 parts of antioxidants, Light stabilizer 0.3-0.4 parts.

4. A high gloss halogen-free flame retardant permanent antistatic polycarbonate composite material according to any one of claims 1 to 3, It is characterized in that The preparation method of the polyaniline modified halloysite nanotubes is: (1) Add 100 parts of water to a reaction container, then add 1.5 to 3.5 parts of dodecyldimethylsulfonyl betaine, turn on the stirring device to mix evenly; turn on the heater to raise the solution temperature to 50 to 60° C., then add 20 to 30 parts of halloysite nanotubes, and continue stirring for 10 to 20 minutes; (2) Add dilute hydrochloric acid to the reactor, stop adding when the pH reaches 4.6 to 4.7, and place the reactor in an ice bath at -5 to 0°C to wait for the solution temperature to stabilize; (3) adding 5 to 10 parts of aniline monomer to the reactor, controlling the stirring rate to 10 to 15 rpm, and applying ultrasound during the stirring process; then dripping 3 to 5 parts of ammonium persulfate solution into the reactor, wherein the dripping time is controlled to be 20 to 30 minutes; (4) The reaction solution of step (3) is filtered and washed with anhydrous ethanol and deionized water for 2 to 3 times, and the solid component is placed in a drying oven for drying to obtain polyaniline-modified halloysite nanotubes.

5. A high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material according to any one of claims 1 to 3, It is characterized in that The aromatic polycarbonate is bisphenol A type polycarbonate resin.

6. A high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material according to any one of claims 1 to 3, It is characterized in that The antioxidant is at least one of antioxidant 1076 and antioxidant 168.

7. A high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material according to any one of claims 1 to 3, It is characterized in that The light stabilizer is one or more of bisphenol A salicylate, 2-hydroxy-4-n-octyloxy-benzophenone, and 2,4-dihydroxybenzophenone.

8. A high gloss halogen-free flame retardant permanent antistatic polycarbonate composite material according to any one of claims 1 to 3, It is characterized in that The particle size of the nano barium sulfate powder is 200-300 nm.

9. A method for preparing the high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material as claimed in any one of claims 1 to 8, It is characterized in that The following steps are involved: (1) Weigh the components in proportion for later use; (2) Pour aromatic polycarbonate, polyetheretherketone, polyaniline modified halloysite nanotubes, hydroquinone bis(diphenyl phosphate), and MBS core-shell graft copolymer according to weight parts into a stirring device and stir evenly to form material group A; pour nano barium sulfate powder, ABS high gloss masterbatch, antioxidant, and light stabilizer according to weight parts into a stirring device and stir evenly to form material group B; (3) Material group A is fed from the main feed of a twin-screw extruder, and material group B is fed from the side feed of the twin-screw extruder, and the mixture is melted, mixed, and extruded through the twin-screw extruder to obtain a polycarbonate composite material.

10. The method for preparing the high-gloss halogen-free flame-retardant permanent antistatic polycarbonate composite material according to claim 9, It is characterized in that The set temperatures of the twin-screw extruder are: section one: 210-230°C, section two: 215-235°C, section three: 220-240°C, section four: 225-245°C, section five: 210-230°C, section six: 210-230°C, section seven: 215-235°C, section eight: 215-235°C, section nine: 220-240°C, and die head: 225-245°C; the rotation speed of the twin-screw extruder is 200-250rmp.