Preparation process of high-toughness wear-resistant TPU composite material

The fluorine-containing diol and modified carbon fiber are generated by reactions such as indole to prepare high-toughness and wear-resistant TPU composite materials, which solves the problem of insufficient toughness and wear resistance of traditional TPU materials under high load and high friction environments, and realizes the The performance of the material is improved and is suitable for a variety of application fields.

CN118931159AInactive Publication Date: 2024-11-12JIANGSU ZENGQIANG NEW MATERIAL SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411064855.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional TPU materials lack toughness and wear resistance in high load and high friction environments, limiting their application range.

Method used

Indole, 3,5-bis(trifluoromethyl)iodine benzene, cuprous iodide and other chemical substances are used to produce intermediate products, and bromine atoms and alkyl groups are introduced through N-bromosuccinimide, ethanolamine and other reactions. Alcohol, forming fluorine-containing diol, combined with 4,4'-diphenylmethane diisocyanate and modified carbon fiber, prepare a high toughness, wear-resistant TPU composite material.

Benefits of technology

The surface hardness and self-lubricity of TPU materials are improved, the wear resistance is significantly improved, and the toughness is enhanced by the addition of carbon fibers, making it less likely to break during impact, and is suitable for high wear resistance and high toughness application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of TPU (thermoplastic polyurethane) materials, in particular to a preparation process of a high-toughness wear-resistant TPU composite material, which is used for solving the problem that the application range of a traditional TPU material is limited due to poor toughness and wear resistance of the traditional TPU material. According to the preparation process, the diol monomer is fluorine-containing diol, the molecular structure of the fluorine-containing diol contains an indole structure, the stability is high, the fluorine-containing diol contains a large number of fluorine atoms, and the fluorine atoms have small atomic radius and high electronegativity, so that the fluorine atoms can form tight and stable chemical bonds in resin molecules; the stable chemical bond structure enables the prepared TPU to be high in surface hardness and very good in self-lubricating property, so that the TPU can resist friction and abrasion of external objects and has excellent abrasion resistance, then carbon fibers are added into the TPU to form the TPU composite material, the toughness of the TPU composite material is improved, and the abrasion resistance is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of TPU materials, and in particular to a preparation process of a high-toughness and wear-resistant TPU composite material. Background Art

[0002] With the advancement of science and technology and the development of industry, the requirements for material performance are also increasing. As a high-performance polymer material, TPU (thermoplastic polyurethane) has been widely used in the fields of shoes, pipes, cable sheaths, etc. due to its excellent wear resistance, high elasticity and processability. However, the toughness and wear resistance of traditional TPU materials still need to be improved, especially in high-load and high-friction environments, where its performance decreases rapidly, limiting its application range. Therefore, the development of a high-toughness and wear-resistant TPU composite material has important practical significance and application value. Summary of the invention

[0003] In order to overcome the above technical problems, the purpose of the present invention is to provide a preparation process of a high-toughness and wear-resistant TPU composite material, which solves the problem that traditional TPU materials have poor toughness and wear resistance, which limits their application range.

[0004] The purpose of the present invention can be achieved through the following technical solutions: A preparation process of a high-toughness wear-resistant TPU composite material comprises the following steps: Step 1: Indole, 3,5-bis(trifluoromethyl)iodobenzene, cuprous iodide, anhydrous potassium carbonate and anhydrous ether are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction for 15-20 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, and then the mixture is heated to reflux and stirred for reaction for 8-10 hours. After the reaction is completed, the reaction product is cooled to room temperature, poured into distilled water, and extracted with ethyl acetate for 2-3 times. The extracts are combined and dried over anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A. Step 2: Add the intermediate product A, N-bromosuccinimide and N,N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, introduce nitrogen protection, stir and react for 8-10 hours at a temperature of 40-45°C and a stirring rate of 300-400r / min. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation to obtain an intermediate product B; Step 3: Add the intermediate product B, ethanolamine, anhydrous potassium carbonate and N,N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction for 15-20 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat the mixture to reflux and continue stirring the reaction for 8-10 hours. After the reaction is completed, cool the reaction product to room temperature, pour it into distilled water, extract it with dichloromethane 2-3 times, combine the extracts and dry them with anhydrous sodium sulfate, then vacuum filter, and rotary evaporate the filtrate to remove the solvent to obtain a fluorinated diol; Step 4: Add carbon fiber and anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to reflux and continue stirring and reacting for 3-4 hours. After the reaction is completed, cool the reaction product to room temperature, then vacuum filter, wash the filter cake with distilled water 3-5 times, and then place it in a vacuum drying oven and dry it at a temperature of 50-55°C for 3-5 hours to obtain pretreated carbon fiber; Step 5: Add the pretreated carbon fiber and anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and ultrasonically disperse for 30-40 minutes at a temperature of 25-30°C and an ultrasonic frequency of 40-50kHz, then add 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate and continue ultrasonic dispersion for 10-15 minutes, then stir the reaction for 4-5 hours at a temperature of 60-65°C and a stirring rate of 300-400r / min under nitrogen protection, and after the reaction, cool the reaction product to room temperature, and then vacuum filter, wash the filter cake with ethanol solution 3-5 times, and then place it in a vacuum drying oven, and dry it for 10-15 hours at a temperature of 45-50°C to obtain modified carbon fiber; Step six: Add 4,4'-diphenylmethane diisocyanate, fluorinated diol, dibutyltin dilaurate and N-methylpyrrolidone to a three-necked flask equipped with an agitator, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 15-20 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to reflux and continue stirring and reacting for 3-5 hours, then add 1,4-butanediol and modified carbon fiber and continue stirring and reacting for 1-2 hours. After the reaction, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 80-85°C for 3-5 hours to obtain a high-toughness and wear-resistant TPU composite material.

[0005] As a further scheme of the present invention: the usage ratio of the indole, 3,5-bis(trifluoromethyl)iodobenzene, cuprous iodide, anhydrous potassium carbonate and anhydrous ether in step 1 is 0.1 mol: 0.11-0.13 mol: 0.05-0.07 mol: 0.11-0.13 mol: 100-120 mL.

[0006] As a further solution of the present invention: the usage ratio of the intermediate product A, N-bromosuccinimide and N,N-dimethylformamide in step 2 is 0.1 mol: 0.22-0.25 mol: 100-120 mL.

[0007] As a further scheme of the present invention: the usage ratio of the intermediate product B, ethanolamine, anhydrous potassium carbonate and N,N-dimethylformamide in step three is 0.1 mol: 0.22-0.25 mol: 0.25-0.3 mol: 120-150 mL.

[0008] As a further solution of the present invention: the usage ratio of the carbon fiber and anhydrous acetone in step 4 is 5g:50-60mL.

[0009] As a further solution of the present invention: the model of the carbon fiber in step 4 is T700SC-12000-50C.

[0010] As a further solution of the present invention: the usage ratio of the pretreated carbon fiber, anhydrous toluene, 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate in step five is 5g: 60-65mL: 2.5-5.5g: 0.2-0.3g.

[0011] As a further solution of the present invention: the volume fraction of the ethanol solution in step five is 50-60%.

[0012] As a further scheme of the present invention: the usage ratio of the 4,4'-diphenylmethane diisocyanate, fluorinated diol, dibutyltin dilaurate, N-methylpyrrolidone, 1,4-butanediol and modified carbon fiber in step six is ​​20-25g: 60-80g: 0.4-0.8g: 100-120g: 4-8g: 5-11g.

[0013] Beneficial effects of the present invention: The invention discloses a preparation process of a high-toughness wear-resistant TPU composite material. First, indole and 3,5-bis(trifluoromethyl)iodobenzene are reacted, and the iodine atom on the 3,5-bis(trifluoromethyl)iodobenzene reacts with the secondary amino group on the indole, thereby introducing two trifluoromethyl groups into the indole to obtain an intermediate product A. Then, the intermediate product A is reacted with N-bromosuccinimide, and the N-bromosuccinimide brominates the intermediate product A, and at least two bromine atoms are introduced into the benzene ring in the indole structure of the intermediate product A to obtain an intermediate product B. Then, the intermediate product B is reacted with ethanolamine, and the bromine atom on the intermediate product B is The method comprises the following steps: reacting with the amino group on ethanolamine to introduce at least two alkyl alcohols to obtain a fluorinated diol, and then treating the carbon fiber with anhydrous acetone to fully remove impurities on the surface of the carbon fiber to obtain a pretreated carbon fiber, and then treating the pretreated carbon fiber with 4,4'-diphenylmethane diisocyanate to introduce a large number of isocyanate groups on the surface of the pretreated carbon fiber to obtain a modified carbon fiber, and finally using the fluorinated diol as a diol monomer, 4,4'-diphenylmethane diisocyanate as a diisocyanate monomer, 1,4-butanediol as a chain extender, and the modified carbon fiber as a modifier to prepare a high-toughness carbon fiber. Wear-resistant TPU composite material; the diol monomer of the preparation process is a fluorinated diol, the molecular structure of the fluorinated diol contains an indole structure, high stability, and contains a large number of fluorine atoms, which have a small atomic radius and a high electronegativity, so that the fluorine atoms can form a tight and stable chemical bond in the resin molecule. This stable chemical bond structure makes the surface hardness of the prepared TPU high, and its self-lubricating property is particularly good, which makes it able to resist friction and wear of external objects, so that it has excellent wear resistance. Then, carbon fiber is added to form a TPU composite material. Carbon fiber is a high-performance The material has the advantages of light weight, high strength, high stiffness, etc. Therefore, the addition of carbon fiber significantly improves the toughness of the TPU composite material, making it less likely to break when impacted, and the wear resistance is further improved. Among them, after the carbon fiber is modified, it contains a large number of isocyanate groups, which can be doped into the TPU composite material in the form of chemical bonds, so that it has the best reinforcement effect; since the TPU composite material of the present invention has high toughness and wear resistance, it can be widely used in the fields of shoe materials, pipes, cable sheaths, etc., especially in application scenarios requiring high wear resistance and high toughness. It has significant advantages. DETAILED DESCRIPTION

[0014] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] Embodiment 1:

[0016] This embodiment is a preparation process of a high-toughness and wear-resistant TPU composite material, comprising the following steps: Step 1: 0.1 mol of indole, 0.11 mol of 3,5-bis(trifluoromethyl)iodobenzene, 0.05 mol of cuprous iodide, 0.11 mol of anhydrous potassium carbonate and 100 mL of anhydrous ether are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at 25°C and a stirring rate of 300 r / min for 15 minutes, and then the mixture is heated to reflux and stirred for reaction for 8 hours. After the reaction is completed, the reaction product is cooled to room temperature, poured into distilled water, extracted twice with ethyl acetate, the extracts are combined and dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A; Step 2: 0.1 mol of intermediate product A, 0.22 mol of N-bromosuccinimide and 100 mL of N, N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer and a gas duct, and nitrogen was introduced for protection. The reaction was stirred at a temperature of 40° C. and a stirring rate of 300 r / min for 8 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate product B; Step 3: Add 0.1 mol of intermediate product B, 0.22 mol of ethanolamine, 0.25 mol of anhydrous potassium carbonate and 120 mL of N, N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction for 15 minutes at a temperature of 25°C and a stirring rate of 300 r / min, then heat the temperature to reflux and continue stirring the reaction for 8 hours. After the reaction is completed, the reaction product is cooled to room temperature, then poured into distilled water, and then extracted twice with dichloromethane, the extracts are combined and dried over anhydrous sodium sulfate, then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a fluorinated diol; Step 4: Add 5g of carbon fiber model T700SC-12000-50C and 50mL of anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 20 minutes at a temperature of 25°C and a stirring rate of 300r / min, then heat to reflux and continue stirring and reacting for 3 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filter cake is washed 3 times with distilled water, and then placed in a vacuum drying oven and dried at a temperature of 50°C for 3 hours to obtain pretreated carbon fiber; Step 5: Add 5g of pretreated carbon fiber and 60mL of anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and ultrasonically disperse for 30min at a temperature of 25°C and an ultrasonic frequency of 40kHz, then add 2.5g of 4,4'-diphenylmethane diisocyanate and 0.2g of dibutyltin dilaurate to continue ultrasonic dispersion for 10min, and then stir the reaction for 4h at a temperature of 60°C, a stirring rate of 300r / min, and nitrogen protection. After the reaction, the reaction product is cooled to room temperature, and then vacuum filtered, and the filter cake is washed 3 times with a volume fraction of 50% ethanol solution, and then placed in a vacuum drying oven and dried at a temperature of 45°C for 10h to obtain modified carbon fiber; Step six: Add 20g 4,4'-diphenylmethane diisocyanate, 60g fluorinated diol, 0.4g dibutyltin dilaurate and 100g N-methylpyrrolidone to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 15min at a temperature of 25°C and a stirring rate of 300r / min, then heat to reflux and continue stirring and reacting for 3h, then add 4g 1,4-butanediol and 5g modified carbon fiber and continue stirring and reacting for 1h. After the reaction, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 80°C for 3h to obtain a high-toughness and wear-resistant TPU composite material.

[0017] Embodiment 2:

[0018] This embodiment is a preparation process of a high-toughness and wear-resistant TPU composite material, comprising the following steps: Step 1: 0.1 mol of indole, 0.12 mol of 3,5-bis(trifluoromethyl)iodobenzene, 0.06 mol of cuprous iodide, 0.12 mol of anhydrous potassium carbonate and 110 mL of anhydrous ether were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at 28°C and a stirring rate of 350 r / min for 18 min, and then the mixture was heated to reflux and continued to stir for 9 h. After the reaction, the reaction product was cooled to room temperature, and then poured into distilled water, and then extracted twice with ethyl acetate, the extracts were combined and dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate product A; Step 2: 0.1 mol of intermediate product A, 0.24 mol of N-bromosuccinimide and 110 mL of N, N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and nitrogen was introduced for protection. The reaction was stirred at a temperature of 42° C. and a stirring rate of 350 r / min for 9 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate product B; Step 3: Add 0.1 mol of intermediate product B, 0.24 mol of ethanolamine, 0.28 mol of anhydrous potassium carbonate and 135 mL of N, N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, introduce nitrogen protection, stir the reaction for 18 minutes at a temperature of 28°C and a stirring rate of 350 r / min, then heat the temperature to reflux and continue stirring the reaction for 9 hours. After the reaction is completed, the reaction product is cooled to room temperature, then poured into distilled water, and then extracted twice with dichloromethane, the extracts are combined and dried over anhydrous sodium sulfate, then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a fluorinated diol; Step 4: Add 5g of carbon fiber model T700SC-12000-50C and 55mL of anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 25min at a temperature of 28°C and a stirring rate of 350r / min, then heat to reflux and continue stirring and reacting for 3.5h. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filter cake is washed 4 times with distilled water, and then placed in a vacuum drying oven and dried at a temperature of 52°C for 4h to obtain pretreated carbon fiber; Step 5: Add 5g of pretreated carbon fiber and 62mL of anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and ultrasonically disperse for 35min at a temperature of 28°C and an ultrasonic frequency of 45kHz, then add 4g of 4,4'-diphenylmethane diisocyanate and 0.25g of dibutyltin dilaurate and continue ultrasonic dispersion for 12min, then stir the reaction for 4.5h at a temperature of 62°C, a stirring rate of 350r / min, and nitrogen protection. After the reaction, the reaction product is cooled to room temperature, and then vacuum filtered. The filter cake is washed 4 times with an ethanol solution with a volume fraction of 55%, and then placed in a vacuum drying oven and dried at a temperature of 48°C for 12h to obtain modified carbon fiber; Step six: Add 22g 4,4'-diphenylmethane diisocyanate, 70g fluorinated diol, 0.6g dibutyltin dilaurate and 110g N-methylpyrrolidone into a three-necked flask equipped with an agitator, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 18min at a temperature of 28°C and a stirring rate of 350r / min, then heat to reflux and continue stirring and reacting for 4h, then add 6g 1,4-butanediol and 8g modified carbon fiber and continue stirring and reacting for 1.5h. After the reaction, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 82°C for 4h to obtain a high-toughness and wear-resistant TPU composite material.

[0019] Embodiment 3:

[0020] This embodiment is a preparation process of a high-toughness and wear-resistant TPU composite material, comprising the following steps: Step 1: 0.1 mol of indole, 0.13 mol of 3,5-bis(trifluoromethyl)iodobenzene, 0.07 mol of cuprous iodide, 0.13 mol of anhydrous potassium carbonate and 120 mL of anhydrous ether are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 30°C and a stirring rate of 400 r / min for 20 minutes, and then the mixture is heated to reflux and stirred for reaction for 10 hours. After the reaction is completed, the reaction product is cooled to room temperature, poured into distilled water, extracted with ethyl acetate for 3 times, the extracts are combined and dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A; Step 2: 0.1 mol of intermediate product A, 0.25 mol of N-bromosuccinimide and 120 mL of N, N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and nitrogen was introduced for protection. The reaction was stirred at a temperature of 45° C. and a stirring rate of 400 r / min for 10 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain an intermediate product B; Step 3: Add 0.1 mol of intermediate product B, 0.25 mol of ethanolamine, 0.3 mol of anhydrous potassium carbonate and 150 mL of N, N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, introduce nitrogen protection, stir and react for 20 minutes at a temperature of 30°C and a stirring rate of 400 r / min, then heat to reflux and continue stirring and reacting for 10 hours. After the reaction is completed, the reaction product is cooled to room temperature, then poured into distilled water, and then extracted with dichloromethane 3 times, the extracts are combined and dried over anhydrous sodium sulfate, then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a fluorinated diol; Step 4: Add 5g of carbon fiber model T700SC-12000-50C and 60mL of anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 30 minutes at a temperature of 30°C and a stirring rate of 400r / min, then heat to reflux and continue stirring and reacting for 4 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filter cake is washed with distilled water 5 times, and then placed in a vacuum drying oven and dried at a temperature of 55°C for 5 hours to obtain pretreated carbon fiber; Step 5: Add 5g of pretreated carbon fiber and 65mL of anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and ultrasonically disperse for 40min at a temperature of 30°C and an ultrasonic frequency of 50kHz, then add 5.5g of 4,4'-diphenylmethane diisocyanate and 0.3g of dibutyltin dilaurate to continue ultrasonic dispersion for 15min, and then stir the reaction for 5h at a temperature of 65°C, a stirring rate of 400r / min, and nitrogen protection. After the reaction, the reaction product is cooled to room temperature, and then vacuum filtered, and the filter cake is washed 5 times with a volume fraction of 60% ethanol solution, and then placed in a vacuum drying oven, and dried at a temperature of 50°C for 15h to obtain modified carbon fiber; Step six: Add 25g 4,4'-diphenylmethane diisocyanate, 80g fluorinated diol, 0.8g dibutyltin dilaurate and 120g N-methylpyrrolidone to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 20min at a temperature of 30°C and a stirring rate of 400r / min, then heat to reflux and continue stirring and reacting for 5h, then add 8g 1,4-butanediol and 11g modified carbon fiber and continue stirring and reacting for 2h. After the reaction, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 85°C for 5h to obtain a high-toughness and wear-resistant TPU composite material.

[0021] Comparative Example 1: This comparative example is a preparation process of a high-toughness and wear-resistant TPU composite material, comprising the following steps: Step 1: Add 5g of carbon fiber model T700SC-12000-50C and 60mL of anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 30 minutes at a temperature of 30°C and a stirring rate of 400r / min, then heat to reflux and continue stirring and reacting for 4 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filter cake is washed with distilled water 5 times, and then placed in a vacuum drying oven and dried at a temperature of 55°C for 5 hours to obtain pretreated carbon fiber; Step 2: Add 5g of pretreated carbon fiber and 65mL of anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and ultrasonically disperse for 40min at a temperature of 30°C and an ultrasonic frequency of 50kHz, then add 5.5g of 4,4'-diphenylmethane diisocyanate and 0.3g of dibutyltin dilaurate and continue ultrasonic dispersion for 15min, then stir and react for 5h at a temperature of 65°C, a stirring rate of 400r / min, and nitrogen protection. After the reaction, the reaction product is cooled to room temperature, and then vacuum filtered, and the filter cake is washed 5 times with a volume fraction of 60% ethanol solution, and then placed in a vacuum drying oven and dried at a temperature of 50°C for 15h to obtain modified carbon fiber; Step 3: Add 25g 4,4'-diphenylmethane diisocyanate, 80g 2-(trifluoromethyl)benzene-1,3-diol, 0.8g dibutyltin dilaurate and 120g N-methylpyrrolidone to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 20min at a temperature of 30°C and a stirring rate of 400r / min, then heat to reflux and continue stirring and reacting for 5h, then add 8g 1,4-butanediol and 11g modified carbon fiber and continue stirring and reacting for 2h. After the reaction, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 85°C for 5h to obtain a high-toughness and wear-resistant TPU composite material.

[0022] Comparative Example 2: This comparative example is a preparation process of a high-toughness and wear-resistant TPU composite material, comprising the following steps: Step 1: 0.1 mol of indole, 0.13 mol of 3,5-bis(trifluoromethyl)iodobenzene, 0.07 mol of cuprous iodide, 0.13 mol of anhydrous potassium carbonate and 120 mL of anhydrous ether are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 30°C and a stirring rate of 400 r / min for 20 minutes, and then the mixture is heated to reflux and stirred for reaction for 10 hours. After the reaction is completed, the reaction product is cooled to room temperature, poured into distilled water, extracted with ethyl acetate for 3 times, the extracts are combined and dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A; Step 2: 0.1 mol of intermediate product A, 0.25 mol of N-bromosuccinimide and 120 mL of N, N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and nitrogen was introduced for protection. The reaction was stirred at a temperature of 45° C. and a stirring rate of 400 r / min for 10 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain an intermediate product B; Step 3: Add 0.1 mol of intermediate product B, 0.25 mol of ethanolamine, 0.3 mol of anhydrous potassium carbonate and 150 mL of N, N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, introduce nitrogen protection, stir and react for 20 minutes at a temperature of 30°C and a stirring rate of 400 r / min, then heat to reflux and continue stirring and reacting for 10 hours. After the reaction is completed, the reaction product is cooled to room temperature, then poured into distilled water, and then extracted with dichloromethane 3 times, the extracts are combined and dried over anhydrous sodium sulfate, then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a fluorinated diol; Step 4: Add 25g 4,4'-diphenylmethane diisocyanate, 80g fluorinated diol, 0.8g dibutyltin dilaurate and 120g N-methylpyrrolidone into a three-necked flask equipped with an agitator, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 20min at a temperature of 30°C and a stirring rate of 400r / min, then heat to reflux and continue stirring and reacting for 5h, then add 8g 1,4-butanediol and continue stirring and reacting for 2h. After the reaction, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 85°C for 5h to obtain a high-toughness and wear-resistant TPU composite material.

[0023] Comparative Example 3: This comparative example is a preparation process of a high-toughness and wear-resistant TPU composite material, comprising the following steps: Step 1: 0.1 mol of indole, 0.13 mol of 3,5-bis(trifluoromethyl)iodobenzene, 0.07 mol of cuprous iodide, 0.13 mol of anhydrous potassium carbonate and 120 mL of anhydrous ether are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 30°C and a stirring rate of 400 r / min for 20 minutes, and then the mixture is heated to reflux and stirred for reaction for 10 hours. After the reaction is completed, the reaction product is cooled to room temperature, poured into distilled water, extracted with ethyl acetate for 3 times, the extracts are combined and dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A; Step 2: 0.1 mol of intermediate product A, 0.25 mol of N-bromosuccinimide and 120 mL of N, N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and nitrogen was introduced for protection. The reaction was stirred at a temperature of 45° C. and a stirring rate of 400 r / min for 10 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain an intermediate product B; Step 3: Add 0.1 mol of intermediate product B, 0.25 mol of ethanolamine, 0.3 mol of anhydrous potassium carbonate and 150 mL of N, N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, introduce nitrogen protection, stir and react for 20 minutes at a temperature of 30°C and a stirring rate of 400 r / min, then heat to reflux and continue stirring and reacting for 10 hours. After the reaction is completed, the reaction product is cooled to room temperature, then poured into distilled water, and then extracted with dichloromethane 3 times, the extracts are combined and dried over anhydrous sodium sulfate, then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a fluorinated diol; Step 4: Add 25g 4,4'-diphenylmethane diisocyanate, 80g fluorinated diol, 0.8g dibutyltin dilaurate and 120g N-methylpyrrolidone to a three-necked flask equipped with an agitator, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 20min at a temperature of 30°C and a stirring rate of 400r / min, then heat to reflux and continue stirring and reacting for 5h, then add 8g 1,4-butanediol and 11g carbon fiber and continue stirring and reacting for 2h. After the reaction, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 85°C for 5h to obtain a high-toughness and wear-resistant TPU composite material.

[0024] Comparative Example 4: This comparative example is a preparation process of a high-toughness and wear-resistant TPU composite material, comprising the following steps: Step 1: Add 5g of carbon fiber model T700SC-12000-50C and 60mL of anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 30 minutes at a temperature of 30°C and a stirring rate of 400r / min, then heat to reflux and continue stirring and reacting for 4 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filter cake is washed with distilled water 5 times, and then placed in a vacuum drying oven and dried at a temperature of 55°C for 5 hours to obtain pretreated carbon fiber; Step 2: Add 5g of pretreated carbon fiber and 65mL of anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and ultrasonically disperse for 40min at a temperature of 30°C and an ultrasonic frequency of 50kHz, then add 5.5g of 4,4'-diphenylmethane diisocyanate and 0.3g of dibutyltin dilaurate and continue ultrasonic dispersion for 15min, then stir and react for 5h at a temperature of 65°C, a stirring rate of 400r / min, and nitrogen protection. After the reaction, the reaction product is cooled to room temperature, and then vacuum filtered, and the filter cake is washed 5 times with a volume fraction of 60% ethanol solution, and then placed in a vacuum drying oven and dried at a temperature of 50°C for 15h to obtain modified carbon fiber; Step 3: Add 25g 4,4'-diphenylmethane diisocyanate, 80g polycarbonate diol (PCD-2000), 0.8g dibutyltin dilaurate and 120g N-methylpyrrolidone to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 20min at a temperature of 30°C and a stirring rate of 400r / min, then heat to reflux and continue stirring and reacting for 5h, then add 8g 1,4-butanediol and 11g modified carbon fiber and continue stirring and reacting for 2h. After the reaction, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 85°C for 5h to obtain a high-toughness and wear-resistant TPU composite material.

[0025] The performance of the high-toughness and wear-resistant TPU composite materials of Examples 1-3 and Comparative Examples 1-4 was tested under the following test conditions: Mechanical properties: The tensile strength and breaking strength were measured in tensile mode using a universal material testing machine provided by an electronic universal testing machine (VWN-20, High-speed rail). The sample was cut into a dumbbell shape (4 mm × 50 mm) with a thickness of 0.3 mm and tested at a speed of 100 mm / min at room temperature. Each sample was measured five times and the average value was recorded.

[0026] Friction and wear performance: According to GB / T3960-1983, the ring-block sliding dry friction test was carried out using an MMS-2A friction and wear testing machine. The test was carried out on a 6mm×30mm sample at a temperature of 23-25°C in an indoor environment. The load was 196N, the steel wheel speed was 200r / min (linear speed was 0.42m / s), the test theoretical distance was 3024m, and the friction coefficient was directly displayed and saved after analysis by a computer.

[0027] The test results are as follows:

[0028] Referring to the data in the above table, according to the comparison between Examples 1-3 and Comparative Examples 1-4, it can be known that the TPU composite material with fluorinated diol as the main raw material and modified carbon fiber added can give it excellent properties, making it have high toughness and high wear resistance.

[0029] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0030] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A preparation process of a high-toughness wear-resistant TPU composite material, characterized in that: The following steps are involved: Step 1: Indole, 3,5-bis(trifluoromethyl)iodobenzene, cuprous iodide, anhydrous potassium carbonate and anhydrous ether are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction for 15-20 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, and then the mixture is heated to reflux and stirred for reaction for 8-10 hours. After the reaction is completed, the reaction product is cooled to room temperature, poured into distilled water, and extracted with ethyl acetate for 2-3 times. The extracts are combined and dried over anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A. Step 2: Add the intermediate product A, N-bromosuccinimide and N,N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, introduce nitrogen protection, stir and react for 8-10 hours at a temperature of 40-45°C and a stirring rate of 300-400r / min. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation to obtain an intermediate product B; Step 3: Add the intermediate product B, ethanolamine, anhydrous potassium carbonate and N,N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction for 15-20 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat the mixture to reflux and continue stirring the reaction for 8-10 hours. After the reaction is completed, cool the reaction product to room temperature, pour it into distilled water, extract it with dichloromethane 2-3 times, combine the extracts and dry them with anhydrous sodium sulfate, then vacuum filter, and rotary evaporate the filtrate to remove the solvent to obtain a fluorinated diol; Step 4: Add carbon fiber and anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to reflux and continue stirring and reacting for 3-4 hours. After the reaction is completed, cool the reaction product to room temperature, then vacuum filter, wash the filter cake with distilled water 3-5 times, and then place it in a vacuum drying oven and dry it at a temperature of 50-55°C for 3-5 hours to obtain pretreated carbon fiber; Step 5: Add the pretreated carbon fiber and anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and ultrasonically disperse for 30-40 minutes at a temperature of 25-30°C and an ultrasonic frequency of 40-50kHz, then add 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate and continue ultrasonic dispersion for 10-15 minutes, then stir the reaction for 4-5 hours at a temperature of 60-65°C and a stirring rate of 300-400r / min under nitrogen protection, and after the reaction, cool the reaction product to room temperature, and then vacuum filter, wash the filter cake with ethanol solution 3-5 times, and then place it in a vacuum drying oven, and dry it for 10-15 hours at a temperature of 45-50°C to obtain modified carbon fiber; Step six: Add 4,4'-diphenylmethane diisocyanate, fluorinated diol, dibutyltin dilaurate and N-methylpyrrolidone to a three-necked flask equipped with an agitator, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 15-20 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to reflux and continue stirring and reacting for 3-5 hours, then add 1,4-butanediol and modified carbon fiber and continue stirring and reacting for 1-2 hours. After the reaction, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 80-85°C for 3-5 hours to obtain a high-toughness and wear-resistant TPU composite material.

2. The preparation process of a high-toughness wear-resistant TPU composite material according to claim 1, characterized in that: The usage ratio of the indole, 3,5-bis(trifluoromethyl)iodobenzene, cuprous iodide, anhydrous potassium carbonate and anhydrous ether in step 1 is 0.1 mol: 0.11-0.13 mol: 0.05-0.07 mol: 0.11-0.13 mol: 100-120 mL.

3. The preparation process of a high-toughness wear-resistant TPU composite material according to claim 1, characterized in that: The usage ratio of the intermediate product A, N-bromosuccinimide and N,N-dimethylformamide in step 2 is 0.1 mol: 0.22-0.25 mol: 100-120 mL.

4. The preparation process of a high-toughness wear-resistant TPU composite material according to claim 1, characterized in that: The usage ratio of the intermediate product B, ethanolamine, anhydrous potassium carbonate and N,N-dimethylformamide in step 3 is 0.1 mol: 0.22-0.25 mol: 0.25-0.3 mol: 120-150 mL.

5. The preparation process of a high-toughness wear-resistant TPU composite material according to claim 1, characterized in that: The usage ratio of the carbon fiber and anhydrous acetone in step 4 is 5g:50-60mL.

6. The preparation process of a high-toughness wear-resistant TPU composite material according to claim 1, characterized in that: The model of the carbon fiber in step 4 is T700SC-12000-50C.

7. The process for preparing a high-toughness wear-resistant TPU composite material according to claim 1, characterized in that: The usage ratio of the pretreated carbon fiber, anhydrous toluene, 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate in step 5 is 5g: 60-65mL: 2.5-5.5g: 0.2-0.3g.

8. The process for preparing a high-toughness wear-resistant TPU composite material according to claim 1, characterized in that: The volume fraction of the ethanol solution in step five is 50-60%.

9. The process for preparing a high-toughness wear-resistant TPU composite material according to claim 1, characterized in that: The usage ratio of the 4,4'-diphenylmethane diisocyanate, fluorinated diol, dibutyltin dilaurate, N-methylpyrrolidone, 1,4-butanediol and modified carbon fiber in step six is ​​20-25g: 60-80g: 0.4-0.8g: 100-120g: 4-8g: 5-11g.