Rubber composition for rubber core of automobile hose and preparation method of rubber composition
By combining modified polyketone and silica with polyamide resin, the problems of high water absorption and easy hydrolysis of polyamide materials in automotive hoses are solved, improving mechanical strength and chemical stability and extending service life.
Patent Information
- Application Number
- CN202411195022.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
Polyamide materials used in automotive hoses have the problems of high water absorption and easy hydrolysis, which leads to reduced mechanical strength and chemical stability. In addition, inorganic fillers have poor compatibility with polyamide materials and are prone to agglomeration.
Modified polyketone masterbatch and modified silica were prepared by modifying polyketone and silica, and then compounded with polyamide resin to form a rubber composition, thereby improving the hydrolysis resistance and mechanical strength of polyamide materials.
It improves the mechanical strength and chemical stability of polyamide rubber compositions, reduces water absorption, and extends service life, making it suitable for the manufacture of rubber cores for automotive hoses.
Smart Images

Figure BDA0005016121320000131 
Figure BDA0005016121320000141
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a rubber composition for a rubber core of an automobile hose and a preparation method thereof. Background Art
[0002] Automobile hoses are pipes used to connect different parts and transmit fluids in automobile systems. They are usually made of rubber or a composite material of rubber and inorganic materials. The functions of automobile hoses include: being used to transmit liquids such as fuel, coolant, brake fluid, etc. to ensure that these key liquids can flow smoothly inside the car; in the brake system and some pneumatic systems, hoses are used to transmit and control air pressure to achieve corresponding functions; through hoses such as cooling water pipes, coolant can be circulated into the engine to reduce the engine temperature and protect the engine from overheating damage.
[0003] For automotive hoses used in different scenarios, technicians in this field have different requirements for their performance. For example: the brake hose (commonly known as the brake pipe) is an important component of the automotive braking system, responsible for transmitting the hydraulic pressure required by the braking system to the brake to realize the braking function of the car. The brake hose needs to be resistant to high pressure, low temperature and wear to ensure the safety of the car; the cooling water pipe is used in the cooling system of the car engine, responsible for circulating the coolant from the water tank into the engine to reduce the engine temperature. The rubber material used to make the cooling water pipe has a smooth internal surface, which helps the coolant flow smoothly; the fuel hose is a pipe connecting the car's fuel system, used to transmit the car's fuel to the engine for combustion. The fuel hose is generally made of a rubber material with good oil resistance and has a smooth internal surface to ensure the smooth flow of fuel; the vacuum tube is a pipe connecting the car engine and various accessories, used to control the engine's air intake, emissions and other related functions. The vacuum tube is generally made of a high temperature resistant and corrosion resistant rubber material;
[0004] In summary, although technicians in this field have different requirements for automotive hoses used in different scenarios, high mechanical strength, smooth inner wall, oil resistance, water resistance and corrosion resistance are common general requirements for automotive hoses.
[0005] Polyamide material is commonly known as nylon (Nylon), and its English name is Polyamide (PA for short). It is a general term for polymers containing amide groups (-CONH-) in the repeating units of the macromolecular main chain. Long-chain nylon refers to a type of nylon in which the number of methylene groups between adjacent amide bonds in the molecular chain is greater than 10, such as PA610, PA612, PA1010, PA11, PA12, PA1212, etc. Long-chain nylon has the advantages of light weight, good flexibility, hydrolysis resistance, oil resistance, acid and alkali resistance, and corrosion resistance. After processing and modification, it can be widely used in automotive system pipelines such as fuel pipes, cooling pipes, and brake oil pipes.
[0006] However, one of the shortcomings of polyamide materials in the prior art is that polyamide materials have strong water absorption and are easily hydrolyzed. The hydrolysis of polyamide materials refers to the attack of amide bonds (-CONH-) in polyamide molecular chains by water molecules or other solvent molecules under specific conditions (such as the presence of acid, alkali or enzyme, and heating, etc.), resulting in the rupture of amide bonds, thereby initiating the degradation and decomposition process of polyamide molecular chains. Specifically, the hydrolysis process will reduce the molecular weight of polyamide and may form monomers, oligomers and other by-products. After hydrolysis, the tensile strength and elongation at break of polyamide materials will be significantly reduced, and its dimensional stability will be affected.
[0007] In the prior art, inorganic materials such as glass fiber, silica, alumina, kaolin, mica, graphite, etc. are usually added to polymer materials to reduce the water absorption rate of polyamide, prevent its hydrolysis, and further improve the mechanical strength, chemical stability and thermal stability of polyamide automotive hose materials.
[0008] However, the compatibility between the above-mentioned inorganic materials and polyamide materials is poor, the inorganic material particles are not easy to disperse, and are easy to agglomerate during the processing, which is a technical problem that needs to be solved by those skilled in the art. Summary of the invention
[0009] One of the problems solved by the present invention is how to provide a polyamide rubber composition for a rubber core of an automobile hose with a long service life and high mechanical strength.
[0010] In order to solve at least one of the above problems, the present invention provides a method for preparing a rubber composition for a rubber core of an automobile hose, the preparation method comprising:
[0011] S100, modifying polyketone with pentaerythritol stearate to prepare modified polyketone masterbatch;
[0012] S200, modifying silicon dioxide with organic matter to prepare modified silicon dioxide;
[0013] S300, preparing a rubber composition using raw materials including modified polyketone masterbatch, modified silica and polyamide resin.
[0014] In the above technical solution, S100 specifically includes:
[0015] S110, uniformly mixing pentaerythritol stearate and polyketone to obtain a first mixture;
[0016] S120, feeding the first mixture into a twin-screw extruder, melt-blending, extruding and granulating, and preparing a modified polyketone masterbatch.
[0017] In the above technical solution, S100 specifically includes:
[0018] S110, uniformly mixing pentaerythritol stearate and polyketone at a mass ratio of pentaerythritol stearate:polyketone=(8-10):100 to obtain a first mixture;
[0019] S120, feeding the first mixture into a twin-screw extruder, melt-blending for 0.5 h to 1 h at a temperature of 200° C. to 240° C. and a screw speed of 250 r / min to 300 r / min, extruding and granulating to obtain a modified polyketone masterbatch.
[0020] In the above technical solution, S200 specifically includes:
[0021] S210, mixing water and ethanol to prepare a hydroalcoholic solution, adding silicon tetrachloride dropwise to the hydroalcoholic solution and stirring to obtain a silica sol;
[0022] S220, immersing the silica sol in ethanol for aging, and taking it out to obtain a silica gel;
[0023] S230, dissolving p-phenylenediamine in ethanol to obtain a p-phenylenediamine solution, and adding diphenyl ether tetraacid dianhydride dropwise to the p-phenylenediamine solution with stirring to obtain a polyamide solution;
[0024] S240, sending the silica gel and the polyamide solution into a reaction kettle for heating and pressurizing treatment to obtain modified silica.
[0025] In the above technical solution, S200 specifically includes:
[0026] S210, mixing water and ethanol in a mass ratio of water: ethanol = (30-35): 100 to prepare a hydroalcoholic solution, and adding silicon tetrachloride dropwise to the hydroalcoholic solution in a mass ratio of silicon tetrachloride: ethanol = (10-20): 100 according to the amount of ethanol used, while stirring simultaneously, and after the addition is completed, adding hydrochloric acid to adjust the pH value to 3-5 and continue stirring for 3h to 4h to obtain a silica sol;
[0027] S220, immersing the silica sol in ethanol for aging for 20 to 24 hours, and taking it out to obtain a silica gel;
[0028] S230, dissolving p-phenylenediamine in ethanol at a mass ratio of p-phenylenediamine:ethanol=(6-12):100 to obtain a p-phenylenediamine solution, and adding diphenyl ether tetraacid dianhydride dropwise to the p-phenylenediamine solution at a molar ratio of p-phenylenediamine:diphenyl ether tetraacid dianhydride=(90-110):100 and stirring, and continuing to stir the reaction for 4 to 6 hours after the addition is complete to obtain a polyamide solution;
[0029] S240. The silica gel and the polyamide solution are fed into a reaction kettle at a mass ratio of silica gel: polyamide solution = (80-100): 100, and subjected to a heating and pressurizing treatment for 2 h to 3 h at a temperature of 250° C. to 260° C. and a pressure of 6.5 MPa to 7.5 MPa. After the treatment, the temperature is reduced and the pressure is released, and the solid is separated, washed with water, and dried to obtain modified silica.
[0030] In the above technical solution, S300 specifically includes:
[0031] S310, mixing the lubricant, antioxidant, plasticizer, compatibilizer, modified silica, modified polyketone masterbatch and polyamide resin uniformly to obtain a second mixture;
[0032] S320, feeding the second mixture into a twin-screw extruder, melt blending, extruding and granulating, and obtaining a rubber composition.
[0033] In the above technical solution, S300 specifically includes:
[0034] S310, mixing the lubricant, antioxidant, plasticizer, compatibilizer, modified silica, modified polyketone masterbatch and polyamide resin uniformly according to the mass ratio of lubricant: antioxidant: plasticizer: compatibilizer: modified silica: modified polyketone masterbatch: polyamide resin = (0.5-1): (1-2): (2-4): (6-8): (10-20): (20-30): 100 to obtain a second mixture;
[0035] S320, feeding the second mixture into a twin-screw extruder, melt-blending for 1 h to 1.5 h at a temperature of 220° C. to 260° C. and a screw speed of 250 r / min to 300 r / min, extruding and granulating to obtain a rubber composition.
[0036] In the above technical scheme, the lubricant includes at least one of the following or a combination thereof: oxidized polyethylene wax, montanic acid wax, ethylene bisstearamide; and / or the antioxidant includes at least one of the following or a combination thereof: β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexamethylenediamine, tris(2,4-di-tert-butylphenyl) phosphite, dilauryl thiodipropionate; and / or the compatibilizer includes at least one of the following or a combination thereof: maleic anhydride, maleic anhydride grafted polyphenylene sulfide, ethylene-maleic anhydride copolymer.
[0037] In the above technical solution, the plasticizer includes N-butylbenzenesulfonamide and diisononyl phthalate in a mass ratio of 1:1.
[0038] The present invention also provides a rubber composition for a rubber core of an automobile hose, and the rubber composition is obtained by using the preparation method of any of the above technical solutions.
[0039] Beneficial Effects
[0040] The present invention provides a method for preparing a rubber composition for a rubber core of an automobile hose. The method firstly uses pentaerythritol stearate to modify polyketone to prepare a modified polyketone masterbatch. Then, an organic matter is used to modify silicon dioxide to prepare modified silicon dioxide. Finally, a rubber composition is prepared using raw materials including the modified polyketone masterbatch, modified silicon dioxide and polyamide resin. Polyketone is a polymer material formed by coordination polymerization of carbon monoxide, ethylene and propylene, which has excellent hydrolysis resistance, excellent wear resistance, fuel resistance, impact resistance, high bending strength and gas barrier performance. In addition, polyketone also has a high heat deformation temperature and can be used at a high temperature for a long time under high temperature environmental conditions. Therefore, the present invention uses polyketone and polyamide resin to compound and jointly prepare a rubber composition for the rubber core of an automobile hose. Polyketone can significantly improve the hydrolysis resistance of polyamide materials. Considering the presence of carbonyl carbon structure in polyketone resin, the aldol condensation reaction between molecules and within molecules during melt processing is cross-linked, resulting in a rapid increase in viscosity of polyketone resin during melt processing, easy adhesion in equipment, resulting in difficulty in equipment cleaning, and uneven discharging. The present invention uses pentaerythritol stearate to modify the polyketone used. Pentaerythritol stearate can suppress the viscosity increase caused by aldol condensation cross-linking curing in the molecular structure of polyketone, thereby making polyketone easy to process and shape. Therefore, the modified polyketone masterbatch obtained by modifying with pentaerythritol stearate can not only effectively prevent polyamide hydrolysis, but also ensure that mixing and discharging are uniform during the melt extrusion of polyamide rubber composition materials, and improve the processability of polyamide rubber composition. Silicon dioxide, as an inorganic filler, can improve the mechanical strength, chemical stability and thermal stability of polyamide rubber composition, and reduce the water absorption rate of polyamide, preventing its hydrolysis. Considering the poor compatibility between silica and polyamide materials, the inorganic material particles are not easy to disperse and are easy to agglomerate during processing, the present invention uses organic matter to modify silica to prepare modified silica with better compatibility with polyamide. In summary, the present invention uses raw materials including modified polyketone masterbatch, modified silica and polyamide resin to prepare a rubber composition with good mechanical strength, and it is not easy to hydrolyze and has a longer service life, and is particularly suitable for the manufacture of automotive hose rubber cores. DETAILED DESCRIPTION
[0041] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description of the specific embodiments of the present invention.
[0042] Unless otherwise specified, the reagents and raw materials used in the present invention can be purchased through commercial channels. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications.
[0043] An embodiment of the present invention provides a method for preparing a rubber composition for a rubber core of an automobile hose, the preparation method comprising:
[0044] S100, modifying polyketone with pentaerythritol stearate to prepare modified polyketone masterbatch;
[0045] S200, modifying silicon dioxide with organic matter to prepare modified silicon dioxide;
[0046] S300, preparing a rubber composition using raw materials including modified polyketone masterbatch, modified silica and polyamide resin.
[0047] The purpose of the present invention is to provide a polyamide rubber composition that is not easily hydrolyzed. The means for achieving the above purpose of the present invention is to add polyketone with excellent hydrolysis resistance and silica as a filler that can prevent polyamide from absorbing water into the polyamide rubber composition.
[0048] Considering that polyketone has high viscosity after heating and melting, it is easy to adhere to the equipment and difficult to discharge uniformly, the present invention uses pentaerythritol stearate to modify polyketone. In order to achieve the modification of polyketone, S100 specifically includes:
[0049] S110, uniformly mixing pentaerythritol stearate and polyketone to obtain a first mixture;
[0050] S120, feeding the first mixture into a twin-screw extruder, melt-blending, extruding and granulating, and preparing a modified polyketone masterbatch.
[0051] Preferably, S100 specifically includes:
[0052] S110, uniformly mixing pentaerythritol stearate and polyketone at a mass ratio of pentaerythritol stearate:polyketone=(8-10):100 to obtain a first mixture;
[0053] S120, feeding the first mixture into a twin-screw extruder, melt-blending for 0.5 h to 1 h at a temperature of 200° C. to 240° C. and a screw speed of 250 r / min to 300 r / min, extruding and granulating to obtain a modified polyketone masterbatch.
[0054] The reason for adopting the above steps is that pentaerythritol stearate can inhibit the increase in viscosity caused by aldol condensation cross-linking and curing in the molecular structure of polyketone. Therefore, the modified polyketone masterbatch obtained by modification with pentaerythritol stearate can not only effectively prevent the hydrolysis of polyamide, but also ensure uniform mixing and discharging during the melt extrusion of the polyamide rubber composition material, thereby improving the processability of the polyamide rubber composition.
[0055] Considering the poor compatibility between silicon dioxide and polyamide materials and the difficulty in dispersing inorganic material particles, the present invention uses organic matter to modify silicon dioxide. In order to achieve the modification of silicon dioxide, S200 specifically includes:
[0056] S210, mixing water and ethanol to prepare a hydroalcoholic solution, adding silicon tetrachloride dropwise to the hydroalcoholic solution and stirring to obtain a silica sol;
[0057] S220, immersing the silica sol in ethanol for aging, and taking it out to obtain a silica gel;
[0058] S230, dissolving p-phenylenediamine in ethanol to obtain a p-phenylenediamine solution, and adding diphenyl ether tetraacid dianhydride dropwise to the p-phenylenediamine solution with stirring to obtain a polyamide solution;
[0059] S240, sending the silica gel and the polyamide solution into a reaction kettle for heating and pressurizing treatment to obtain modified silica.
[0060] Preferably, S200 specifically includes:
[0061] S210, mixing water and ethanol in a mass ratio of water: ethanol = (30-35): 100 to prepare a hydroalcoholic solution, and adding silicon tetrachloride dropwise to the hydroalcoholic solution in a mass ratio of silicon tetrachloride: ethanol = (10-20): 100 according to the amount of ethanol used, while stirring simultaneously, and after the addition is completed, adding hydrochloric acid to adjust the pH value to 3-5 and continue stirring for 3h to 4h to obtain a silica sol;
[0062] S220, immersing the silica sol in ethanol for aging for 20 to 24 hours, and taking it out to obtain a silica gel;
[0063] S230, dissolving p-phenylenediamine in ethanol at a mass ratio of p-phenylenediamine:ethanol=(6-12):100 to obtain a p-phenylenediamine solution, and adding diphenyl ether tetraacid dianhydride dropwise to the p-phenylenediamine solution at a molar ratio of p-phenylenediamine:diphenyl ether tetraacid dianhydride=(90-110):100 and stirring, and continuing to stir the reaction for 4 to 6 hours after the addition is complete to obtain a polyamide solution;
[0064] S240. The silica gel and the polyamide solution are fed into a reaction kettle at a mass ratio of silica gel: polyamide solution = (80-100): 100, and subjected to a heating and pressurizing treatment for 2 h to 3 h at a temperature of 250° C. to 260° C. and a pressure of 6.5 MPa to 7.5 MPa. After the treatment, the temperature is reduced and the pressure is released, and the solid is separated, washed with water, and dried to obtain modified silica.
[0065] In the above process, by dropping silicon tetrachloride into the water-alcohol solution and stirring simultaneously, a silica sol can be obtained, and the silica sol is immersed in ethanol, so that the sol can be aged into a gel. After obtaining the gel, the gel is treated with a polyamide solution obtained by reacting p-phenylenediamine and diphenyl ether tetraacid dianhydride. The specific treatment method is to mix the silica gel and the polyamide solution, and then heat and pressurize. Among them, the temperature condition of 250°C to 260°C can make the polyamide imidized to form nano-silica loaded with polyimide. In addition, the present invention uses ethanol as a solvent for p-phenylenediamine when preparing the polyamide solution, and ethanol can reach a supercritical state under a temperature condition of 250°C to 260°C and a pressure condition of 6.5MPa to 7.5MPa. The ethanol in the supercritical state can extract the ethanol in the silica gel, so that pores are formed on the surface of the silica particles, and the porous silica can load more polyimide, thereby reducing the surface energy of the silica and improving its compatibility with the polyamide resin. It is understood that after the raw materials are fed into the reactor, it is necessary to evacuate the reactor first. Subsequently, the pressure in the reactor is maintained by ethanol vapor. In order to maintain a reasonable pressure range, the reactor of the present invention is provided with a pressure relief valve, which can release pressure when the pressure is too high. When the pressure is too low, ethanol vapor can be introduced to maintain the pressure.
[0066] In order to prepare the rubber composition of polyimide, S300 specifically includes:
[0067] S310, mixing the lubricant, antioxidant, plasticizer, compatibilizer, modified silica, modified polyketone masterbatch and polyamide resin uniformly to obtain a second mixture;
[0068] S320, feeding the second mixture into a twin-screw extruder, melt blending, extruding and granulating, and obtaining a rubber composition.
[0069] Preferably, S300 specifically includes:
[0070] S310, mixing the lubricant, antioxidant, plasticizer, compatibilizer, modified silica, modified polyketone masterbatch and polyamide resin uniformly according to the mass ratio of lubricant: antioxidant: plasticizer: compatibilizer: modified silica: modified polyketone masterbatch: polyamide resin = (0.5-1): (1-2): (2-4): (6-8): (10-20): (20-30): 100 to obtain a second mixture;
[0071] S320, feeding the second mixture into a twin-screw extruder, melt-blending for 1 h to 1.5 h at a temperature of 220° C. to 260° C. and a screw speed of 250 r / min to 300 r / min, extruding and granulating to obtain a rubber composition.
[0072] In some embodiments of the present invention, the lubricant includes at least one of the following or a combination thereof: oxidized polyethylene wax, montanic acid wax, and ethylene bisstearamide.
[0073] In some embodiments of the present invention, the antioxidant includes at least one of the following or a combination thereof: β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine, tris(2,4-di-tert-butylphenyl) phosphite, and dilauryl thiodipropionate.
[0074] In some embodiments of the present invention, the compatibilizer includes at least one of the following or a combination thereof: maleic anhydride, maleic anhydride grafted polyphenylene sulfide, and ethylene-maleic anhydride copolymer.
[0075] In some embodiments of the present invention, the plasticizer includes N-butylbenzenesulfonamide and diisononyl phthalate in a mass ratio of 1:1.
[0076] In some embodiments of the present invention, the polyamide resin includes at least one of the following or a combination thereof: PA6, PA610, PA612, PA1012, and PA12.
[0077] Example 1
[0078] This embodiment provides a rubber composition for a rubber core of an automobile hose, which is prepared by the following steps:
[0079] S1, mixing pentaerythritol stearate and K950 polyketone in a mass ratio of pentaerythritol stearate: K950 polyketone = 8:100 to obtain a first mixture;
[0080] S2. Feed the first mixture into a twin-screw extruder, melt blend for 1 hour, and extrude and granulate to obtain a modified polyketone masterbatch; the twin-screw extruder has multiple heating zones from 1# to 10#, and the temperatures of the multiple heating zones and the die are set to 210°C, 210°C, 220°C, 220°C, 220°C, 235°C, 235°C, 230°C, 230°C, 240°C, and 240°C in sequence; the screw speed of the main machine is 250r / min;
[0081] S3, mixing water and ethanol at a mass ratio of water: ethanol = 32:100 to prepare a hydroalcoholic solution, and adding silicon tetrachloride to the hydroalcoholic solution at a mass ratio of silicon tetrachloride: ethanol = 16:100 according to the amount of ethanol used, and stirring simultaneously, after the addition is completed, adding hydrochloric acid to adjust the pH value to 4 and continue stirring for 4 hours to obtain a silica sol;
[0082] S4, immersing the silica sol in ethanol for aging for 24 hours, and taking it out to obtain silica gel;
[0083] S5, dissolving p-phenylenediamine in ethanol at a mass ratio of p-phenylenediamine:ethanol=10:100 to obtain a p-phenylenediamine solution, and adding diphenyl ether tetraacid dianhydride dropwise to the p-phenylenediamine solution at a molar ratio of p-phenylenediamine:diphenyl ether tetraacid dianhydride=100:100 and stirring, and continuing to stir and react for 4 hours after the addition is complete to obtain a polyamide solution;
[0084] S6. According to the mass ratio of silica gel: polyamide solution = 80:100, the silica gel and the polyamide solution are fed into a reaction kettle, and a heating and pressurizing treatment is carried out for 3 hours at a temperature of 250±2° C. and a pressure of 6.7±0.2 MPa. After the treatment, the temperature is lowered and the pressure is released, and the solid is separated, washed with water twice, and infrared dried to obtain modified silica;
[0085] S7. Mix oxidized polyethylene wax, dilauryl thiodipropionate, N-butylbenzenesulfonamide, diisononyl phthalate, maleic anhydride, modified silica, modified polyketone masterbatch and PA6 polyamide resin in a mass ratio of oxidized polyethylene wax: dilauryl thiodipropionate: N-butylbenzenesulfonamide: diisononyl phthalate: maleic anhydride: modified silica: modified polyketone masterbatch: PA6 polyamide resin = 0.5:1:1:1:6:15:25:100 to obtain a second mixture;
[0086] S8. Feed the second mixture into a twin-screw extruder, melt blend for 1.5 hours, and extrude and granulate to obtain a rubber composition; the twin-screw extruder has multiple heating zones from 1# to 10#, and the temperatures of the multiple heating zones and the die are set to 220°C, 220°C, 230°C, 230°C, 240°C, 240°C, 245°C, 250°C, 250°C, 260°C, and 260°C in sequence; the screw speed of the main engine is 250r / min.
[0087] Example 2
[0088] This embodiment provides a rubber composition for a rubber core of an automobile hose, which is prepared by the following steps:
[0089] S1, mixing pentaerythritol stearate and K950 polyketone in a mass ratio of pentaerythritol stearate: K950 polyketone = 8:100 to obtain a first mixture;
[0090] S2. Feed the first mixture into a twin-screw extruder, melt blend for 1 hour, and extrude and granulate to obtain a modified polyketone masterbatch; the twin-screw extruder has multiple heating zones from 1# to 10#, and the temperatures of the multiple heating zones and the die are set to 210°C, 210°C, 220°C, 220°C, 220°C, 235°C, 235°C, 230°C, 230°C, 240°C, and 240°C in sequence; the screw speed of the main machine is 250r / min;
[0091] S3, mixing water and ethanol at a mass ratio of water: ethanol = 32:100 to prepare a hydroalcoholic solution, and adding silicon tetrachloride to the hydroalcoholic solution at a mass ratio of silicon tetrachloride: ethanol = 16:100 according to the amount of ethanol used, and stirring simultaneously, after the addition is completed, adding hydrochloric acid to adjust the pH value to 4 and continue stirring for 4 hours to obtain a silica sol;
[0092] S4, immersing the silica sol in ethanol for aging for 24 hours, and taking it out to obtain silica gel;
[0093] S5, sending the silica gel into a reactor, introducing ethanol vapor, and performing a heating and pressurizing treatment for 3 hours at a temperature of 250±2° C. and a pressure of 6.7±0.2 MPa. After the treatment, cooling and releasing the pressure, separating the solid, washing with water twice, and infrared drying to obtain silica;
[0094] S6, mixing KH550 silane and silicon dioxide at a mass ratio of KH550 silane:silicon dioxide = 4:100, and grinding and mixing with a planetary ball mill for 1 hour to obtain modified silicon dioxide;
[0095] S7. Mix oxidized polyethylene wax, dilauryl thiodipropionate, N-butylbenzenesulfonamide, diisononyl phthalate, maleic anhydride, modified silica, modified polyketone masterbatch and PA6 polyamide resin in a mass ratio of oxidized polyethylene wax: dilauryl thiodipropionate: N-butylbenzenesulfonamide: diisononyl phthalate: maleic anhydride: modified silica: modified polyketone masterbatch: PA6 polyamide resin = 0.5:1:1:1:6:15:25:100 to obtain a second mixture;
[0096] S8. Feed the second mixture into a twin-screw extruder, melt blend for 1.5 hours, and extrude and granulate to obtain a rubber composition; the twin-screw extruder has multiple heating zones from 1# to 10#, and the temperatures of the multiple heating zones and the die are set to 220°C, 220°C, 230°C, 230°C, 240°C, 240°C, 245°C, 250°C, 250°C, 260°C, and 260°C in sequence; the screw speed of the main engine is 250r / min.
[0097] Comparative Example 1
[0098] This embodiment provides a rubber composition for a rubber core of an automobile hose, which is prepared by the following steps:
[0099] S1. According to the mass ratio of oxidized polyethylene wax: dilauryl thiodipropionate: N-butylbenzenesulfonamide: diisononyl phthalate: maleic anhydride: TS720 silica: POK630A polyketone: PA6 polyamide resin = 0.5:1:1:1:6:15:25:100, oxidized polyethylene wax, dilauryl thiodipropionate, N-butylbenzenesulfonamide, diisononyl phthalate, maleic anhydride, TS720 silica, POK630A polyketone and PA6 polyamide resin are uniformly mixed to obtain a second mixture;
[0100] S2. Feed the second mixture into a twin-screw extruder, melt blend for 1.5 hours, and extrude and granulate to obtain a rubber composition; the twin-screw extruder has multiple heating zones from 1# to 10#, and the temperatures of the multiple heating zones and the die are set to 220°C, 220°C, 230°C, 230°C, 240°C, 240°C, 245°C, 250°C, 250°C, 260°C, and 260°C in sequence; the screw speed of the main engine is 250r / min.
[0101] Comparative Example 2
[0102] This embodiment provides a rubber composition for a rubber core of an automobile hose, which is prepared by the following steps:
[0103] S1. Evenly mix oxidized polyethylene wax, dilauryl thiodipropionate, N-butylbenzenesulfonamide, diisononyl phthalate, maleic anhydride and PA6 polyamide resin in a mass ratio of oxidized polyethylene wax: dilauryl thiodipropionate: N-butylbenzenesulfonamide: diisononyl phthalate: maleic anhydride: PA6 polyamide resin = 0.5:1:1:1:6:100 to obtain a second mixture;
[0104] S2. Feed the second mixture into a twin-screw extruder, melt blend for 1.5 hours, and extrude and granulate to obtain a rubber composition; the twin-screw extruder has multiple heating zones from 1# to 10#, and the temperatures of the multiple heating zones and the die are set to 220°C, 220°C, 230°C, 230°C, 240°C, 240°C, 245°C, 250°C, 250°C, 260°C, and 260°C in sequence; the screw speed of the main engine is 250r / min.
[0105] Performance Testing
[0106] The performance test results of the samples obtained in Examples 1 to 2 and Comparative Examples 1 to 2 are listed in Table 1. The accelerated aging test conditions for the above samples are ethanol hydrolysis aging at a temperature of 160° C. for 1000 h.
[0107] Table 1
[0108]
[0109]
[0110] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for preparing a rubber composition for an automobile hose rubber core, characterized in that: The preparation method comprises: S100, modifying polyketone with pentaerythritol stearate to prepare modified polyketone masterbatch; S200, modifying silicon dioxide with organic matter to prepare modified silicon dioxide; S300, preparing the rubber composition by using raw materials including the modified polyketone masterbatch, the modified silica and a polyamide resin.
2. The preparation method according to claim 1, characterized in that: S100 specifically includes: S110, uniformly mixing the pentaerythritol stearate and the polyketone to obtain a first mixture; S120, feeding the first mixture into a twin-screw extruder, melt blending, extruding and granulating, to prepare the modified polyketone masterbatch.
3. The preparation method according to claim 1, characterized in that: S100 specifically includes: S110, mixing the pentaerythritol stearate and the polyketone uniformly at a mass ratio of pentaerythritol stearate:polyketone=(8-10):100 to obtain a first mixture; S120, feeding the first mixture into a twin-screw extruder, melt-blending for 0.5 h to 1 h at a temperature of 200° C. to 240° C. and a screw speed of 250 r / min to 300 r / min, and extruding and granulating to obtain the modified polyketone masterbatch.
4. The preparation method according to claim 1, characterized in that: S200 specifically includes: S210, mixing water and ethanol to prepare a hydroalcoholic solution, adding silicon tetrachloride dropwise to the hydroalcoholic solution and stirring to obtain a silica sol; S220, immersing the silica sol in ethanol for aging, and taking it out to obtain silica gel; S230, dissolving p-phenylenediamine in ethanol to obtain a p-phenylenediamine solution, and adding diphenyl ether tetraacid dianhydride dropwise to the p-phenylenediamine solution with stirring to obtain a polyamide solution; S240, sending the silica gel and the polyamide solution into a reaction kettle for heating and pressurizing treatment to obtain the modified silica.
5. The preparation method according to claim 1, characterized in that: S200 specifically includes: S210, mixing the water and the ethanol in a mass ratio of water: ethanol = (30-35): 100 to prepare a hydroalcoholic solution, and adding silicon tetrachloride dropwise to the hydroalcoholic solution in a mass ratio of silicon tetrachloride: ethanol = (10-20): 100 according to the amount of the ethanol used, while stirring simultaneously, and after the addition is completed, adding hydrochloric acid to adjust the pH value to 3-5 and continue stirring for 3h to 4h to obtain a silica sol; S220, immersing the silica sol in ethanol and aging it for 20 to 24 hours, and then taking it out to obtain a silica gel; S230, dissolving the p-phenylenediamine in the ethanol at a mass ratio of p-phenylenediamine:ethanol=(6-12):100 to obtain a p-phenylenediamine solution, and dropping the diphenyl ether tetraacid dianhydride into the p-phenylenediamine solution at a molar ratio of p-phenylenediamine:diphenyl ether tetraacid dianhydride=(90-110):100 and stirring, and continuing to stir the reaction for 4 to 6 hours after the dropwise addition is completed to obtain a polyamide solution; S240, feeding the silica gel and the polyamide solution into a reaction kettle at a mass ratio of silica gel: polyamide solution = (80-100): 100, and subjecting them to a heating and pressurizing treatment for 2 h to 3 h at a temperature of 250° C. to 260° C. and a pressure of 6.5 MPa to 7.5 MPa. After the treatment, cooling and releasing the pressure, separating the solids, washing with water, and drying to obtain the modified silica.
6. The preparation method according to any one of claims 1 to 5, characterized in that S300 specifically includes: S310, uniformly mixing the lubricant, the antioxidant, the plasticizer, the compatibilizer, the modified silica, the modified polyketone masterbatch and the polyamide resin to obtain a second mixture; S320, feeding the second mixture into a twin-screw extruder, melt blending, extruding and granulating, to obtain the rubber composition.
7. The preparation method according to any one of claims 1 to 5, characterized in that S300 specifically includes: S310, mixing the lubricant, the antioxidant, the plasticizer, the compatibilizer, the modified silica, the modified polyketone masterbatch and the polyamide resin uniformly according to the mass ratio of lubricant: antioxidant: plasticizer: compatibilizer: modified silica: modified polyketone masterbatch: polyamide resin = (0.5-1): (1-2): (2-4): (6-8): (10-20): (20-30): 100 to obtain a second mixture; S320, feeding the second mixture into a twin-screw extruder, melt-blending for 1 h to 1.5 h at a temperature of 220° C. to 260° C. and a screw speed of 250 r / min to 300 r / min, extruding and granulating to obtain the rubber composition.
8. The preparation method according to claim 7, characterized in that: The lubricant comprises at least one of the following or a combination thereof: oxidized polyethylene wax, montan acid wax, ethylene bis stearamide; and / or The antioxidant comprises at least one of the following or a combination thereof: β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine, tris(2,4-di-tert-butylphenyl) phosphite, dilauryl thiodipropionate; and / or The compatibilizer includes at least one of the following or a combination thereof: maleic anhydride, maleic anhydride grafted polyphenylene sulfide, and ethylene-maleic anhydride copolymer.
9. The preparation method according to claim 7, characterized in that: The plasticizer comprises N-butylbenzenesulfonamide and diisononyl phthalate in a mass ratio of 1:
1.
10. A rubber composition for a rubber core of an automobile hose, characterized in that: The rubber composition is obtained by the preparation method according to any one of claims 1 to 9.