Hydrotalcite two-dimensional material-based composite nanofiller and anticorrosive paint
By introducing two-dimensional material-based hydrotalcite composite nanofillers into aqueous epoxy resins, combining the passive shielding of two-dimensional materials and the active anticorrosion ability of hydrotalcites, the problem of insufficient anticorrosion performance of traditional aqueous epoxy resins is solved, and significant Anti-corrosion effect.
Patent Information
- Application Number
- CN202410935900.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional water-based epoxy resins have problems with high porosity and insufficient corrosion resistance in terms of corrosion resistance. The introduction of nanomaterials alone cannot achieve comprehensive corrosion resistance improvement.
Using two-dimensional material-based hydrotalcite composite nanofiller, the hydrotalcite with anionic intercalation is grown in situ on the surface of the two-dimensional material, and modified by catechol compounds, combining the passive shielding effect of the two-dimensional material and the active hydrotalcite Anti-corrosion ability, forming a dual anti-corrosion protection mechanism.
It significantly improves the corrosion resistance of aqueous epoxy resin, delays the penetration of corrosive media, and interferes with the corrosion process by releasing corrosion inhibitors, provides multiple protection, and significantly improves the corrosion resistance of metals.
Smart Images

Figure CN118931229A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of anti-corrosion coatings, and in particular to a method for preparing a hydrotalcite / two-dimensional material-based composite nanofiller capable of enhancing the friction resistance of a coating and an anti-corrosion coating thereof, and belongs to the cross-cutting frontier field of polymer synthesis and anti-corrosion control. Background Art
[0002] Metal materials play an indispensable role in various fields of modern society, especially in construction, transportation and industrial production. However, the problem of metal corrosion has always been a difficult problem that plagues all walks of life. Metal corrosion not only shortens the service life of equipment and components, but also causes huge economic losses and potential safety hazards. Therefore, how to effectively prevent metal corrosion has become an important research topic.
[0003] There are many traditional anti-corrosion measures, among which spraying polymer coating on metal surface is a commonly used anti-corrosion method. Polymer coating can form a protective film on the metal surface to block the corrosive medium, thus playing an anti-corrosion role. Epoxy resin, as a kind of polymer coating, has been widely used due to its high cross-linking density, good shielding properties and strong adhesion to metal substrates. However, traditional solvent-based epoxy resin releases a large amount of volatile organic compounds (VOCs) during the spraying and curing process, posing a threat to the environment and human health.
[0004] In order to solve this problem, waterborne epoxy resin (WEP) came into being. Waterborne epoxy resin uses water as a dispersion medium, which greatly reduces the emission of VOCs. However, waterborne epoxy resin still has some shortcomings in practical applications, such as high porosity and anti-corrosion performance that needs to be improved. In order to further improve the anti-corrosion performance of waterborne epoxy resin, introducing various nanomaterials into the coating has become an effective method. However, the current public information shows that although the introduction of any one nanomaterial alone can improve a specific performance of the coating, it still cannot achieve comprehensive anti-corrosion performance. Therefore, finding a solution that can improve comprehensive performance is still the direction that industry R&D personnel have been exploring. Summary of the invention
[0005] The present invention aims to provide a two-dimensional material-based hydrotalcite composite nanofiller and an anticorrosive coating. As an inorganic compound with a layered structure, hydrotalcite exhibits excellent active anticorrosion ability. Relying on its strong anion exchange capacity, hydrotalcite can protect the metal substrate by replacing corrosive anions between layers and slowing down the cathode reaction in the corrosion reaction. Two-dimensional materials such as MXene and graphene, due to their unique layered structure and excellent shielding properties, can form a physical barrier in the coating, effectively blocking the penetration of corrosive media, thereby playing a passive anticorrosion role.
[0006] Combining the active anti-corrosion ability of hydrotalcite with the passive shielding effect of two-dimensional materials can significantly improve the overall anti-corrosion performance of water-based coatings. This composite coating can not only delay the penetration of corrosive media through physical shielding effects, but also actively interfere with the corrosion process by releasing corrosion inhibitors, thus providing dual protection. Studies have shown that this combination method has shown significant effects in improving the anti-corrosion performance of water-based epoxy resins and has broad application prospects.
[0007] To achieve the above object, the present invention provides a two-dimensional material-based hydrotalcite composite nanofiller, which is special in that it includes a single layer or less than 10 layers of a two-dimensional material matrix, and an anion-intercalated hydrotalcite is in-situ grown on the surface of the two-dimensional material to obtain a composite nanofiller, and the composite nanofiller is in-situ modified by a catechol compound. The two-dimensional material matrix preferably has less than 5 layers.
[0008] Preferably, the two-dimensional material matrix is one of MXene, graphene and its derivatives, hexagonal boron nitride, and layered zirconium phosphate as the two-dimensional material.
[0009] Furthermore, the average size of the two-dimensional material matrix is 5-30 microns.
[0010] Preferably, the two-dimensional material matrix is processed by the following process:
[0011] The two-dimensional material is dispersed in a solution containing a stripping agent, and after adjusting the pH value of the solution, ultrasonic stripping is performed; wherein the stripping agent is selected from one or more of organic strong bases, quaternary ammonium salts, and tris(hydroxymethyl)aminomethane; the solution solvent is one or more of deionized water, ethanol, tetrahydrofuran, and N,N-dimethylformamide; the solution pH value is 7.0-9.0; the ultrasonic treatment conditions include: ultrasonic frequency of 20-70kHz, and ultrasonic time of 0.5h-3h.
[0012] Preferably, the anion intercalated hydrotalcite conforms to the following general formula:
[0013] M 2+ 1-x M 3+ x (OH)2] x+ A n- x / n mH2O;
[0014] Among them, M 2+ Mg 2+ 、Co 2+ 、Ni 2+ 、Zn 2+ and Cu 2+ Divalent metal cations, M3+ For Al 3+ Cr 3+ , Fe 3+ , Ga 3+ Equivalent metal cations; A n- NO 3- , Cl - OH - 、SO4 2- PO4 3- 、C6H4(COO)2 2- Anion; x is M 3+ / M 2+ The molar ratio is generally between 0.2 and 0.4; m represents the number of crystalline water between layers in the entire hydrotalcite structure.
[0015] Preferably, the catechol compound is selected from one or more of dopamine, tannic acid, catechin, epicatechin and epicatechin.
[0016] Another object of the present invention is to provide a water-based epoxy anti-corrosion coating, which comprises: a water-based epoxy resin, a curing agent, and any of the above-mentioned two-dimensional material-based hydrotalcite composite nanofillers; in terms of mass fraction, the content of the water-based epoxy resin is 15wt% to 30wt%, the content of the curing agent is 25wt% to 35wt%, the content of deionized water is 45wt% to 55wt%, and the content of the composite nanofiller is 0.2wt% to 1.0wt%.
[0017] Preferably, the waterborne epoxy resin brand is selected from one or more of E-51, E-20, E-12 and E-06.
[0018] Preferably, the curing agent is selected from one or more of United Curing Chemicals Banco901, United Curing Chemicals Banco916, CardoliteNX-8101, Shanghai Hanzhong Chemical H208B, and Shanghai Hanzhong Chemical H202B.
[0019] Preferably, the two-dimensional material-based hydrotalcite composite nanofiller is prepared by the following method:
[0020] Step 1. Dispersing the two-dimensional material in a buffer solution containing a stripping agent, and obtaining a single-layer or few-layer two-dimensional material suspension by ultrasonic-assisted stripping, specifically comprising:
[0021] The two-dimensional material zirconium phosphate (α-ZrP) and the stripping agent tris(hydroxymethyl)aminomethane (Tris) were dispersed and dissolved in deionized water at a ratio of 1:1 by mass fraction, and the pH was adjusted to 7.0-9.0 with 1.0 mol / L dilute hydrochloric acid;
[0022] The above solution is subjected to ultrasonic assisted exfoliation, the ultrasonic frequency is 20-70kHz, and the ultrasonic time is 0.5h to 3h; the obtained exfoliated ZrP (e-ZrP) is repeatedly washed by centrifugation with deionized water until it is neutral, a small amount of the suspension is freeze-dried, the solid content is measured, and the solid content of e-ZrP in the suspension is calculated.
[0023] Step 2. Weigh M according to a certain ratio 3+ With M 2+ The metal salt is dissolved in deionized water, and then sodium molybdate dihydrate solution is slowly added dropwise, and the pH is adjusted with sodium hydroxide solution; the mixed solution is subjected to magnetic stirring, filtering, washing and other steps to obtain anticorrosive hydrotalcite, which specifically includes:
[0024] Weigh ZnCl2 and AlCl3·6H2O in a certain molar ratio and dissolve them in deionized water, then slowly drop sodium molybdate dihydrate solution;
[0025] The pH of the mixed solution was adjusted to 8.0-10.0 with 1.0 mol / L sodium hydroxide solution;
[0026] The above solution is aged at a constant temperature for 12 to 24 hours. After the aging is completed, the mixed solution is filtered, and the filter cake is repeatedly washed with deionized water until it is neutral to obtain the anticorrosive hydrotalcite.
[0027] Step 3. In-situ growth of Zn-Al hydrotalcite on the surface of e-ZrP to obtain a composite nanofiller, specifically comprising:
[0028] A certain molar concentration of ZnCl2 and AlCl3·6H2O was dissolved in deionized water to form a salt solution, which was slowly added dropwise to the e-ZrP suspension;
[0029] The pH of the mixed solution was adjusted to 8.0-10.0 with 1.0 mol / L sodium hydroxide solution;
[0030] The solution was magnetically stirred in an oil bath for 12 to 24 hours. After the reaction was completed, it was repeatedly washed with deionized water and filtered until neutral to obtain a Zn-Al hydrotalcite / e-ZrP composite nanofiller (denoted as LZ).
[0031] Step 4. Surface modification of LZ to obtain a modified composite nanofiller specifically comprises:
[0032] Take a certain amount of Tris and dissolve it in deionized water. Use 1.0 mol / L dilute hydrochloric acid to adjust the pH of the solution to 8.0-10.0.
[0033] LZ and tannic acid were added to the above solution in sequence, and magnetic stirring was carried out at a constant speed for 12 to 24 hours in an air atmosphere at room temperature;
[0034] The product was repeatedly washed with deionized water and filtered until neutral to obtain a modified Zn-Al hydrotalcite / e-ZrP composite nanofiller (denoted as m-LZ).
[0035] Preferably, the waterborne epoxy anticorrosive coating is prepared by the following method:
[0036] Step 1. Mixing the prepared composite nanomaterial with deionized water, and ultrasonically dispersing it in an ultrasonic cell disruptor to obtain a suspension in which the composite nanomaterial is uniformly dispersed;
[0037] Step 2. adding epoxy resin to the suspension, and stirring at high speed to obtain a water-based anticorrosive coating mother solution;
[0038] Step 3. Add the curing agent into the mother liquor of the water-based anti-corrosion coating, and stir at high speed to obtain the water-based epoxy anti-corrosion coating.
[0039] The beneficial effects of the present invention are:
[0040] 1. The two-dimensional material after stripping with the aid of a stripping agent has a large diameter-to-thickness ratio. Adding it as an anti-corrosion filler to a water-based epoxy system can effectively extend the penetration path of the corrosive medium. Compared with organic strong alkaline stripping agents, the use of organic and environmentally friendly stripping agent Tris to strip α-ZrP nanosheets can not only simplify the post-processing steps of stripping, but also reduce pollution to the environment;
[0041] 2. The unique anion exchange properties of hydrotalcite enable them to replace corrosive anions between layers, slowing down the cathodic reaction in the corrosion reaction;
[0042] 3. In-situ growth of Zn-Al hydrotalcite on the surface of the two-dimensional material ZrP combines the passive shielding effect of the two-dimensional material with the active anti-corrosion ability of the hydrotalcite, achieving a dual anti-corrosion effect, thereby greatly improving the corrosion resistance of the metal. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 SEM images of LZ and m-LZ;
[0044] Figure 2 Bode spectra of the anti-corrosion performance test of the coatings of each embodiment and the comparative example (immersed in 3.5wt.% NaCl solution for 1 day and 30 days);
[0045] Figure 3 The following are scanning electron microscope photos of the metal substrate after the coatings of various embodiments and the coatings of comparative examples were immersed in a 3.5 wt. % NaCl solution for 30 days. DETAILED DESCRIPTION
[0046] The embodiments described below are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] The two-dimensional material-based hydrotalcite composite nanofiller provided by the present invention comprises a single-layer or less than 10-layer two-dimensional material matrix, and a composite nanofiller obtained by in-situ growing anion-intercalated hydrotalcite on the surface of the two-dimensional material, and the composite nanofiller is in-situ modified by a catechol compound.
[0048] The two-dimensional material matrix is one of MXene, graphene and its derivatives, hexagonal boron nitride, and layered zirconium phosphate as the two-dimensional material. The average size of the two-dimensional material matrix is 5-30 microns.
[0049] The two-dimensional material matrix is processed by the following process:
[0050] The two-dimensional material is dispersed in a solution containing a stripping agent, and after adjusting the pH value of the solution, ultrasonic stripping is performed; wherein the stripping agent is selected from one or more of organic strong bases, quaternary ammonium salts, and tris(hydroxymethyl)aminomethane; the solution solvent is one or more of deionized water, ethanol, tetrahydrofuran, and N,N-dimethylformamide; the solution pH value is 7.0-9.0; the ultrasonic treatment conditions include: ultrasonic frequency of 20-70kHz, and ultrasonic time of 0.5h-3h.
[0051] The anion intercalated hydrotalcite conforms to the following general formula:
[0052] M 2+ 1-x M 3+ x (OH)2] x+ A n- x / n mH2O;
[0053] Among them, M 2+ Mg 2+ 、Co 2+ 、Ni 2+ 、Zn 2+ and Cu 2+ Divalent metal cations, M 3+ For Al 3+ Cr 3+ , Fe 3+ , Ga 3+ Equivalent metal cations; A n- NO 3- , Cl - OH -、SO4 2- PO4 3- 、C6H4(COO)2 2- Anion; x is M 3+ / M 2+ The molar ratio is generally between 0.2 and 0.4; m represents the number of crystalline water between layers in the entire hydrotalcite structure.
[0054] The catechol compound is selected from one or more of dopamine, tannic acid, catechin and epicatechin.
[0055] The water-based epoxy anti-corrosion coating provided by the present invention comprises: a water-based epoxy resin, a curing agent, and any of the above-mentioned two-dimensional material-based hydrotalcite composite nanofillers; in terms of mass fraction, the content of the water-based epoxy resin is 15wt% to 30wt%, the content of the curing agent is 25wt% to 35wt%, the content of deionized water is 45wt% to 55wt%, and the content of the composite nanofiller is 0.2wt% to 1.0wt%.
[0056] The waterborne epoxy resin brand is selected from one or more of E-51, E-20, E-12 and E-06.
[0057] The curing agent is selected from one or more of United Curing Chemicals Banco901, United Curing Chemicals Banco916, Cardolite NX-8101, Shanghai Hanzhong Chemical H208B, and Shanghai Hanzhong Chemical H202B.
[0058] The two-dimensional material-based hydrotalcite composite nanofiller is prepared by the following method:
[0059] Step 1. Dispersing the two-dimensional material in a buffer solution containing a stripping agent, and obtaining a single-layer or few-layer two-dimensional material suspension by ultrasonic-assisted stripping, specifically comprising:
[0060] The two-dimensional material zirconium phosphate (α-ZrP) and the stripping agent tris(hydroxymethyl)aminomethane (Tris) were dispersed and dissolved in deionized water at a ratio of 1:1 by mass fraction, and the pH was adjusted to 7.0-9.0 with 1.0 mol / L dilute hydrochloric acid;
[0061] The above solution is subjected to ultrasonic assisted exfoliation, the ultrasonic frequency is 20-70kHz, and the ultrasonic time is 0.5h to 3h; the obtained exfoliated ZrP (e-ZrP) is repeatedly washed by centrifugation with deionized water until it is neutral, a small amount of the suspension is freeze-dried, the solid content is measured, and the solid content of e-ZrP in the suspension is calculated.
[0062] Step 2. Weigh M according to a certain ratio 3+ With M 2+The metal salt is dissolved in deionized water, and then sodium molybdate dihydrate solution is slowly added dropwise, and the pH is adjusted with sodium hydroxide solution; the mixed solution is subjected to magnetic stirring, filtering, washing and other steps to obtain anticorrosive hydrotalcite, which specifically includes:
[0063] Weigh ZnCl2 and AlCl3·6H2O in a certain molar ratio and dissolve them in deionized water, then slowly drop sodium molybdate dihydrate solution;
[0064] The pH of the mixed solution was adjusted to 8.0-10.0 with 1.0 mol / L sodium hydroxide solution;
[0065] The above solution is aged at a constant temperature for 12 to 24 hours. After the aging is completed, the mixed solution is filtered, and the filter cake is repeatedly washed with deionized water until it is neutral to obtain the anticorrosive hydrotalcite.
[0066] Step 3. In situ growth of Zn-Al hydrotalcite on the surface of e-ZrP to obtain a composite nanofiller, specifically comprising:
[0067] A certain molar concentration of ZnCl2 and AlCl3·6H2O was dissolved in deionized water to form a salt solution, which was slowly added dropwise to the e-ZrP suspension;
[0068] The pH of the mixed solution was adjusted to 8.0-10.0 with 1.0 mol / L sodium hydroxide solution;
[0069] The above solution was magnetically stirred in an oil bath for 12 to 24 hours. After the reaction was completed, it was repeatedly washed with deionized water and filtered until neutral to obtain a Zn-Al hydrotalcite / e-ZrP composite nanofiller (denoted as LZ).
[0070] Step 4. Surface modification of LZ to obtain a modified composite nanofiller specifically comprises:
[0071] Take a certain amount of Tris and dissolve it in deionized water. Use 1.0 mol / L dilute hydrochloric acid to adjust the pH of the solution to 8.0-10.0.
[0072] LZ and tannic acid were added to the above solution in sequence, and magnetic stirring was carried out at a constant speed for 12 to 24 hours in an air atmosphere at room temperature;
[0073] The product was repeatedly washed with deionized water and filtered until neutral to obtain a modified Zn-Al hydrotalcite / e-ZrP composite nanofiller (denoted as m-LZ).
[0074] The waterborne epoxy anticorrosive coating is prepared by the following method:
[0075] Step 1. Mixing the prepared composite nanomaterial with deionized water, and ultrasonically dispersing it in an ultrasonic cell disruptor to obtain a suspension in which the composite nanomaterial is uniformly dispersed;
[0076] Step 2. adding epoxy resin to the suspension, and stirring at high speed to obtain a water-based anticorrosive coating mother solution;
[0077] Step 3. Add the curing agent into the mother liquor of the water-based anti-corrosion coating, and stir at high speed to obtain the water-based epoxy anti-corrosion coating.
[0078] The anti-corrosion coating of the waterborne epoxy anti-corrosion coating is formed by the following method:
[0079] The waterborne epoxy anti-corrosion coating is applied on a low-carbon steel substrate with an applicator, and the surface is dried at room temperature for 4 to 7 days, and then transferred to a 120° C. oven for curing for 2 to 4 hours to obtain an anti-corrosion coating having the waterborne epoxy anti-corrosion coating.
[0080] The preparation method of the waterborne epoxy anticorrosive coating of the present invention is described in detail below.
[0081] Example 1: A method for preparing a Zn-Al hydrotalcite anti-corrosion nanomaterial and a composite anti-corrosion coating thereof.
[0082] The present embodiment provides a method for preparing a Zn-Al hydrotalcite anticorrosive nanomaterial and a composite anticorrosive coating thereof, which specifically comprises the following steps:
[0083] Step 1: Dissolve 0.5g of sodium molybdate dihydrate and 0.35g of sodium hydroxide in 60mL of deionized water to obtain solution A; dissolve 1g of zinc nitrate hexahydrate and 0.4g of aluminum nitrate nonahydrate in deionized water to obtain solution B; mix solution A and solution B, and adjust the pH to 9.5. Aging the above solution at 140°C for 14h. Finally, the aged mixed solution is filtered and washed several times, and dried in a vacuum drying oven for use.
[0084] Step 2: Take 5.8g of curing agent 901 (solid content 60wt.%), 6.2g of deionized water, 40mg of Zn-Al hydrotalcite, stir at high speed for 10min, then add 4.6g of epoxy resin E51, stir at high speed for 5min. Finally, a composite anticorrosive coating containing 0.5wt.% anticorrosive filler is prepared.
[0085] Step 3: Use a four-sided coater to apply the coating on the polished Q215 iron sheet. After cross-linking and curing, a pure water-based epoxy resin coating can be obtained. The coating is dried at room temperature for 7 days and then dried at 120°C for 2 hours. The wet thickness of the coating is 100 μm and the dry thickness is about 38-42 μm.
[0086] Example 2: A method for preparing a two-dimensional ZrP anti-corrosion nanomaterial and its composite anti-corrosion coating.
[0087] The present embodiment provides a method for preparing a two-dimensional ZrP anticorrosive nanomaterial and a composite anticorrosive coating thereof, which specifically comprises the following steps:
[0088] Step 1: Dissolve 0.1212 g of Tris in deionized water to prepare a Tris buffer solution, then add 1 g of α-ZrP to the Tris buffer solution, and adjust the pH of the suspension to 8.5 with 1.0 mol / L dilute hydrochloric acid; ultrasonically treat the α-ZrP suspension for 30 minutes; wash the resulting product with deionized water and then dry it to obtain the exfoliated e-ZrP.
[0089] Step 2: Take 5.8g of curing agent 901 (solid content 60wt.%), 6.2g of deionized water, 40mg of e-ZrP, stir at high speed for 10min, then add 4.6g of epoxy resin E51, stir at high speed for 5min. Finally, a composite anticorrosive coating containing 0.5wt.% anticorrosive filler is prepared.
[0090] Step 3: Use a four-sided coater to apply the coating on the polished Q215 iron sheet. After cross-linking and curing, a pure water-based epoxy resin coating can be obtained. The coating is dried at room temperature for 7 days and then dried at 120°C for 2 hours. The wet thickness of the coating is 100 μm and the dry thickness is about 38-42 μm.
[0091] Example 3: A method for preparing a hydrotalcite / two-dimensional material-based composite nanofiller and a composite anti-corrosion coating thereof.
[0092] The present embodiment provides a method for preparing a hydrotalcite / two-dimensional material-based composite nanofiller and a composite anti-corrosion coating thereof, which specifically comprises the following steps:
[0093] Step 1: Dissolve 0.1212 g of Tris in deionized water to prepare a Tris buffer solution, then add 1 g of α-ZrP to the Tris buffer solution, and adjust the pH of the suspension to 8.5 with 1.0 mol / L dilute hydrochloric acid; ultrasonically treat the α-ZrP suspension for 30 minutes; wash the resulting product with deionized water and then dry it to obtain the exfoliated e-ZrP.
[0094] Step 2: Dissolve 0.5g of sodium molybdate dihydrate and 0.35g of sodium hydroxide in 60mL of deionized water to obtain solution A; take 0.7g of the e-ZrP prepared in step 2, dissolve and disperse it with 1g of ZnCl2 and 0.4g of AlCl3·6H2O in deionized water to obtain solution B; mix solution A with solution B, adjust the pH to 10 with 1.0mol / L sodium hydroxide solution, and age the mixed solution at 140°C for 8 hours. After the reactant is cooled to room temperature, wash it with deionized water, and then freeze-dry it to remove moisture. The obtained solid is a hydrotalcite / two-dimensional material-based composite nanofiller (LZ);
[0095] Step 3: Take 5.8g of curing agent 901 (solid content 60wt.%), 6.2g of deionized water, 40mg of LZ, stir at high speed for 10min, then add 4.6g of epoxy resin E51, stir at high speed for 5min. Finally, a composite anticorrosive coating containing 0.5wt.% anticorrosive filler is prepared.
[0096] Step 4: Use a four-sided coater to apply the coating on the polished Q215 iron sheet, and after cross-linking and curing, a pure water-based epoxy resin coating can be obtained. The coating is dried at room temperature for 7 days and then dried at 120°C for 2 hours. The wet thickness of the coating is 100μm and the dry thickness is about 38-42μm.
[0097] Example 4: A method for preparing a modified hydrotalcite / two-dimensional material-based composite nanofiller and a composite anti-corrosion coating thereof.
[0098] The present embodiment provides a method for preparing a modified hydrotalcite / two-dimensional material-based composite nanofiller and a composite anti-corrosion coating thereof, which specifically comprises the following steps:
[0099] Step 1: Dissolve 0.1212 g of Tris in deionized water to prepare a Tris buffer solution, then add 1 g of α-ZrP to the Tris buffer solution, and adjust the pH of the suspension to 8.5 with 1.0 mol / L dilute hydrochloric acid; ultrasonically treat the α-ZrP suspension for 30 minutes; wash the resulting product with deionized water and then dry it to obtain the exfoliated e-ZrP.
[0100] Step 2: Dissolve 0.5g of sodium molybdate dihydrate and 0.35g of sodium hydroxide in 60mL of deionized water to obtain solution A; take 0.7g of the e-ZrP prepared in step 2, dissolve and disperse it with 1g of ZnCl2 and 0.4g of AlCl3·6H2O in deionized water to obtain solution B; mix solution A with solution B, adjust the pH to 10 with 1.0mol / L sodium hydroxide solution, and age the mixed solution at 140°C for 8 hours. After the reactant is cooled to room temperature, wash it with deionized water, and then freeze-dry it to remove moisture. The obtained solid is a hydrotalcite / two-dimensional material-based composite nanofiller (LZ);
[0101] Step 3: Dissolve 0.1212g Tris in deionized water to prepare a buffer solution, adjust the solution pH to 8.5 with 1.0mol / L dilute hydrochloric acid; then add 1g LZ and an equal amount of tannic acid, and stir magnetically at room temperature for 24h. Wash the obtained reactants by centrifugation with deionized water, and freeze-dry to obtain a polytannic acid-modified hydrotalcite / two-dimensional material-based composite nanofiller (m-LZ).
[0102] Step 4: Take 5.8g of curing agent 901 (solid content 60wt.%), 6.2g of deionized water, 40mg of m-LZ, stir at high speed for 10min, then add 4.6g of epoxy resin E51, stir at high speed for 5min. Finally, a composite anticorrosive coating containing 0.5wt.% anticorrosive filler is prepared.
[0103] Step 5: Use a four-sided coater to apply the coating on the polished Q215 iron sheet. After cross-linking and curing, a pure water-based epoxy resin coating can be obtained. The coating is dried at room temperature for 7 days and then dried at 120°C for 2 hours. The wet thickness of the coating is 100 μm and the dry thickness is about 38-42 μm.
[0104] Comparative Example 1: A method for preparing a water-based epoxy resin coating.
[0105] The present embodiment provides a method for preparing a water-based epoxy resin coating without anti-corrosion fillers, which specifically comprises the following steps:
[0106] Step 1: Take 5.8g of curing agent 901 (solid content 60wt.%) and 6.2g of deionized water, stir at high speed for 10min, then add 4.6g of epoxy resin E51, stir at high speed for 5min. Finally, a water-based epoxy resin coating without anticorrosive filler is prepared.
[0107] Step 2: Use a four-sided coater to apply the coating on a polished Q215 iron sheet, and after cross-linking and curing, a pure water-based epoxy resin coating can be obtained. The coating is dried at room temperature for 7 days and then dried at 120°C for 2 hours. The wet thickness of the coating is 100 μm and the dry thickness is about 38-42 μm.
[0108] The present invention uses a scanning electron microscope (SEM, SU-8200, Japan) to characterize the Zn-Al hydrotalcite / ZrP composite nanofiller (LZ) and the modified Zn-Al hydrotalcite / ZrP composite nanofiller (m-LZ).
[0109] The present invention uses an electrochemical workstation (Chenhua, 660e, China) to characterize the anti-corrosion performance of the coating. The EIS test was performed at a stable open circuit potential (OCP) with an amplitude of 10 mV and a frequency range of 10 5 -10 -2 Potentiodynamic polarization (PD) tests were performed after the coatings were immersed in 3.5 wt. % NaCl solution for 30 days, with a range of OCP ± 300 mV and a scan rate of 10 mV / s.
[0110] Table 1: Potentiokinetic polarization test data
[0111]
[0112] Microscopic morphology observation: The microscopic morphology of LZ and m-LZ was observed using a scanning electron microscope. Figure 1 shown.
[0113] Electrochemical test: From the electrochemical impedance spectroscopy test, it can be seen that ( Figure 2 ), during the entire immersion period, the low-frequency impedance modulus of Example 4 is much higher than that of the water-based epoxy resin coating and other examples, indicating that the combination of hydrotalcite and two-dimensional materials can greatly improve the corrosion resistance of the coating. After immersion for 30 days, the epoxy resin film was removed and the corrosion on the surface of the metal substrate was observed by scanning electron microscopy. It can be seen that the metal substrate coated with the coating of Comparative Example 1 has a large amount of corrosion products on the substrate surface due to the limited corrosion resistance of pure epoxy resin. However, the metal substrate coated with the coating of Example 4 still has the traces of grinding in the early stage of the coating, and basically no traces of corrosion products can be observed. This shows that the metal substrate is effectively protected, because the active corrosion protection of hydrotalcite is combined with the passive shielding of the two-dimensional material to provide multiple anti-corrosion protection effects for the metal substrate.
[0114] Referring to the test data of potential dynamic polarization described in Table 1, it can be seen that the corrosion current and corrosion rate of Example 4 are the lowest. Therefore, we can draw the following conclusions: adding an appropriate amount of Zn-Al hydrotalcite / ZrP composite nanofiller into the waterborne epoxy coating can significantly improve the anti-corrosion performance of the epoxy coating, and endow the coating with excellent active and passive anti-corrosion capabilities, which brings substantial improvement to the anti-corrosion performance of the hydrotalcite / two-dimensional material with the base material being the waterborne epoxy resin, and has achieved a significant anti-corrosion effect.
[0115] The present invention is described in detail above in conjunction with the embodiments. It should be noted that the various specific technical features described in the above specific embodiments can be combined and changed in any suitable manner without contradiction, and the present invention will not further describe various possible combinations. In addition, other variations and combinations of the various technical features of the present invention should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A two-dimensional material-based hydrotalcite composite nanofiller, characterized in that: The invention comprises a two-dimensional material matrix with a single layer or less than 10 layers, and a composite nano-filler obtained by in-situ growing anion intercalated hydrotalcite on the surface of the two-dimensional material, and in-situ modification of the composite nano-filler by a catechol compound.
2. The two-dimensional material-based hydrotalcite composite nanofiller according to claim 1, characterized in that: The two-dimensional material matrix is one of MXene, graphene and its derivatives, hexagonal boron nitride, and layered zirconium phosphate as the two-dimensional material; the average size of the two-dimensional material matrix is 5-30 microns.
3. The two-dimensional material-based hydrotalcite composite nanofiller according to claim 2, characterized in that: The two-dimensional material matrix is processed by the following process: The two-dimensional material is dispersed in a solution containing a stripping agent, and after adjusting the pH value of the solution, ultrasonic stripping is performed; wherein the stripping agent is selected from one or more of organic strong bases, quaternary ammonium salts, and tris(hydroxymethyl)aminomethane; the solution solvent is one or more of deionized water, ethanol, tetrahydrofuran, and N,N-dimethylformamide; the solution pH value is 7.0-9.0; the ultrasonic treatment conditions include: ultrasonic frequency of 20-70kHz, and ultrasonic time of 0.5h-3h.
4. The two-dimensional material-based hydrotalcite composite nanofiller according to claim 1, characterized in that: The anion intercalated hydrotalcite conforms to the following general formula: M 2+ 1-x M 3+ x (OH)2] x+ A n- x / n ·mH2O; Among them, M 2+ Mg 2+ 、Co 2+ 、Ni 2+ 、Zn 2+ and Cu 2+ Divalent metal cations, M 3+ For Al 3+ Cr 3+ , Fe 3+ , Ga 3+ Equivalent metal cations; A n- NO 3- , Cl - OH - 、SO4 2- PO4 3- 、C6H4(COO)2 2- Anion; x is M 3+ / M 2+ The molar ratio is generally between 0.2 and 0.4; m represents the number of crystalline water between layers in the entire hydrotalcite structure.
5. The two-dimensional material-based hydrotalcite composite nanofiller according to claim 1, characterized in that: The catechol compound is selected from one or more of dopamine, tannic acid, catechin and epicatechin.
6. A water-based epoxy anticorrosive coating, comprising: A water-based epoxy resin, a curing agent, and a two-dimensional material-based hydrotalcite composite nanofiller according to any one of claims 1 to 6; in terms of mass fraction, the content of the water-based epoxy resin is 15wt% to 30wt%, the content of the curing agent is 25wt% to 35wt%, the content of deionized water is 45wt% to 55wt%, and the content of the composite nanofiller is 0.2wt% to 1.0wt%.
7. The waterborne epoxy anticorrosive coating according to claim 6, characterized in that: The waterborne epoxy resin brand is selected from one or more of E-51, E-20, E-12 and E-06.
8. The waterborne epoxy anticorrosive coating according to claim 6, characterized in that: The curing agent is selected from one or more of United Curing Chemicals Banco901, United Curing Chemicals Banco916, Cardolite NX-8101, Shanghai Hanzhong Chemical H208B, and Shanghai Hanzhong Chemical H202B.
Citation Information
Cited By
Water-based anticorrosive wear-resistant paint and preparation method thereof
CN119432232A