Graphene additive and preparation method of high-conductivity graphene / copper composite material
By using reduced graphene oxide or phthalocyanine materials as additives in graphene/copper composites, the problems of poor dispersion of graphene in solvents and uneven coating distribution are solved, and the conductivity and binding force are significantly improved, thus achieving Highly efficient preparation of graphene/copper composites.
Patent Information
- Application Number
- CN202411135036.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing graphene/copper composite materials, the poor dispersion of graphene in solvents and uneven coating distribution leads to poor conductivity and insufficient bonding with copper substrates, which limits its inclusion in composite materials and electrochemical energy storage. Applications in devices.
Reduced graphene oxide (rGO) or phthalocyanine material (PC) is used as graphene additives, and dispersed in the mixed solvent by ultrasonic to form a uniform graphene dispersion liquid, and a uniform and stable surface of the copper matrix is formed by coating and plating. Coating to improve the bonding and conductivity of graphene and copper matrix.
It significantly improves the dispersion of graphene in solvent and the flatness of the coating, enhances the binding force between graphene and copper matrix, improves the conductivity and electrochemical properties of the composite material, and ensures the stability and efficiency of the coating. Conductivity.
Smart Images

Figure CN118931249A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of graphene metal composite materials, and in particular relates to a preparation method of a graphene additive and a high-conductivity graphene / copper composite material. Background Art
[0002] Graphene has been widely studied due to its excellent electrical and mechanical strength. Graphene / copper composites have shown wide application potential in electronic devices, heat dissipation materials and high-strength conductive materials due to their excellent electrical conductivity, thermal conductivity and mechanical strength. The existing preparation technology of graphene / copper composites mainly focuses on dispersing graphene into the copper matrix uniformly through different methods to enhance the electrical conductivity, thermal conductivity and mechanical properties of the material. Common preparation methods include mechanical mixing, powder metallurgy, electroplating and chemical vapor deposition (CVD). These methods have their own advantages and disadvantages. For example, the mechanical mixing method is simple to operate, but graphene is easy to agglomerate; the powder metallurgy method can achieve good dispersion, but the process is relatively complicated; the electroplating method is suitable for the preparation of thin film composite materials, but it is difficult to control the thickness and uniformity; the CVD method can accurately control the number and quality of graphene layers, but the equipment requirements are high and the cost is high. Although existing technologies have made certain progress in improving the performance of graphene / copper composites, in practical applications, how to further improve the dispersion uniformity of graphene in the copper matrix or on the surface, improve the interface bonding strength, and reduce production costs are still urgent issues to be solved.
[0003] Graphene is dispersed in a solvent to form a dispersion, and the preparation of graphene / copper composite materials using a surface coating method is more operable and has better economic benefits. However, since graphene is a 2D material with a large specific surface area and strong van der Waals force, its dispersibility in the solvent is poor, it is easy to agglomerate to form larger aggregates, and it is difficult to be evenly distributed on the surface of the copper substrate. This uneven distribution can cause defects on the coating surface, reduce its mechanical strength and conductivity, and limit its performance in applications such as composite materials and electrochemical energy storage devices. In addition, the graphene coating has poor wettability and bonding with the copper substrate, resulting in an unstable coating structure, making it easier to fall off and fail during application. Therefore, how to improve the dispersibility of Gr in the solvent and the bonding quality of the graphene coating with the copper substrate is of great significance.
[0004] Reduced graphene oxide (rGO) is a material obtained by chemically reducing graphene oxide (GO). The surface of rGO retains some oxygen groups (such as hydroxyl, carboxyl and epoxy groups) and other functional groups (such as amino and thiol groups). These functional groups can form stable interactions with solvent molecules, such as hydrogen bonds, van der Waals forces or π-π interactions, thereby effectively increasing the dispersion stability of Gr. In addition, the surface functional groups in rGO can reduce the aggregation of Gr through electrostatic repulsion and steric hindrance effects, further improving its dispersion performance in solvents. rGO has better wettability than Gr on copper substrates. Therefore, rGO provides an effective way to improve the dispersion of Gr. Highly dispersed rGO-modified Gr shows broad application prospects in composite materials, conductive inks, energy storage devices, electrocatalysts and other fields. The groups on rGO can also improve its wettability with the copper substrate, significantly improving the interfacial bonding ability of the graphene coating and the copper substrate.
[0005] Phthalocyanine (PC) molecules have a conjugated large π electron system, which enables them to interact with the π electron system of graphene, forming a compact and flat stacking structure when preparing the coating. Phthalocyanine materials contain a large number of nitrogen atoms, which can form coordination bonds with copper atoms. This coordination effect can increase the binding of copper to phthalocyanine molecules, thereby indirectly enhancing the binding between copper and graphene. Summary of the invention
[0006] In order to improve the dispersibility of graphene and the bonding quality of graphene coating and copper substrate, it is particularly important to optimize the dispersion method of graphene and select suitable additives. The purpose of the present invention is to provide a graphene additive and a method for preparing a high-conductivity graphene / copper composite material, so as to solve the problem that graphene has poor dispersibility in solvents and the graphene coating in the currently prepared graphene / copper composite material is unevenly distributed and poorly bonded to the copper substrate, resulting in poor overall conductivity of the graphene / copper composite material.
[0007] The present invention firstly proposes a graphene (Gr) additive, wherein the graphene (Gr) additive is reduced graphene oxide (rGO) or phthalocyanine material (PC), and the phthalocyanine material (PC) is a composite of aluminum phthalocyanine (AlPC) and cobalt phthalocyanine (CoPC) in a mass ratio of 1:3 to 3:1.
[0008] The present invention also provides a method for preparing a high-conductivity graphene / copper composite material. By adding the graphene (Gr) additive during the preparation process, the dispersibility of graphene in the solvent is improved, so that the graphene coating coated on the surface of the copper substrate is evenly distributed, the stability and uniformity of the graphene coating on the surface of the copper substrate are maintained, and the bonding between the graphene coating and the copper substrate is improved, thereby improving the conductivity of the graphene / copper composite material.
[0009] The high-conductivity graphene / copper composite material is specifically a Gr / rGO / Cu composite material or a Gr / PC / Cu composite material, and its preparation method specifically comprises the following steps: (1) Preparation of graphene dispersion: Graphene nanosheets and graphene additives are dispersed in a mixed solvent A consisting of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP), and dispersed uniformly by ultrasonication; (2) Preparation of film-forming agent precursor solution: a certain amount of rosin is dispersed in a mixed solvent B consisting of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP), and ultrasonically dispersed until the rosin is dissolved; (3) The graphene dispersion obtained in step (1) and the film-forming agent precursor solution obtained in step (2) are mixed and uniformly dispersed by ultrasonication to obtain a coating solution; the coating solution is coated on the surface of the copper wire through a coating machine (the coating machine of the model of Mai Ke MK-TTL2-21 can be selected), and the excess coating solution is scraped off with a diamond drawing die, followed by preliminary drying.
[0010] (4) The coated and preliminarily dried samples are dried in a forced air drying oven and a vacuum drying oven in turn, and then thermally deposited in a vacuum tube furnace to volatilize solutes and solvents such as rosin, thereby promoting the deposition of graphene on the copper surface to obtain a highly conductive graphene / copper composite material.
[0011] Preferably, the graphene additive in step (1) is reduced graphene oxide or phthalocyanine material, and the phthalocyanine material is a composite of aluminum phthalocyanine and cobalt phthalocyanine in a mass ratio of 1:3 to 3:1.
[0012] Furthermore, when reduced graphene oxide is selected as the graphene additive, the reduced graphene oxide accounts for 10-50% of the total mass of graphene and reduced graphene oxide, and the total concentration of graphene and reduced graphene oxide in the mixed solvent A is 1.5-30 mg / mL.
[0013] Furthermore, when the graphene additive is a phthalocyanine material, the concentration of graphene in the mixed solvent A is 1.5-30 mg / mL, and the concentration of the phthalocyanine material in the mixed solvent A is 1.0-10 mg / mL.
[0014] Preferably, the volume percentages of isopropanol, N-dimethylformamide, terpineol and N-methylpyrrolidone in the mixed solvent A in step (1) are 30-40%, 25-35%, 10-20% and 5-15% respectively.
[0015] Preferably, the mixed solvent B described in step (2) has the same components and ratios as the mixed solvent A described in step (1).
[0016] Preferably, the concentration of the rosin in step (2) in the mixed solvent B is 0.1-0.5 g / mL.
[0017] Preferably, in step (3), the ultrasonic power is 500-900 W, and the ultrasonic time is 1-3 h.
[0018] Preferably, in step (3), the diameter of the copper wire is 0.2-0.5 mm, the coating speed is 2-20 m / min, the aperture of the diamond drawing die is 0.21-0.53 mm, the initial drying temperature is 180-380 °C, and the drying time is 0.05-0.5 min.
[0019] Preferably, in step (4), the temperature of the blast drying oven is set to 50-80°C, and the drying time is 0.5-2 h; the temperature of the vacuum drying oven is set to 80-150°C, and the drying time is 0.5-2 h; the temperature of the vacuum tube furnace thermal deposition is set to 260-500°C, and the processing time is 0.1-1 h.
[0020] Furthermore, when the graphene additive selected in step (1) is reduced graphene oxide, a Gr / rGO / Cu composite material is finally obtained; when the graphene additive selected in step (1) is phthalocyanine material (PC), a Gr / PC / Cu composite material is finally obtained.
[0021] Compared with the prior art, the present invention has obvious advantages and beneficial effects. By means of the above technical solution, the present invention can achieve considerable technical progress and practicality, and has a wide range of utilization value, and has at least the following advantages: (1) The graphene (Gr) additive of the present invention is mainly a phthalocyanine material (PC) formed by reducing graphene oxide (rGO) or aluminum phthalocyanine (AlPC) and cobalt phthalocyanine (CoPC). The rGO group has a non-covalent interaction with the mixed solvent A, and the rGO and Gr have a π-π interaction, which can synergistically improve the dispersibility of graphene, help improve the stability and uniformity of the graphene dispersion, thereby improving the flatness of the graphene coating, increasing the contact area between the coating and the copper substrate, and thus improving the bonding between the two and the conductivity of the composite material. Phthalocyanine can use its aromatic ring to form a π-π interaction with graphene, improve the flatness and density of the graphene stack, and phthalocyanine can effectively adsorb on the copper substrate, thereby improving the bonding between the graphene coating and the copper substrate, ensuring the stability of the graphene / copper composite material structure, and PC can act as an electron transmission bridge between graphene and between graphene and the copper substrate, effectively improving the conductivity of the composite material.
[0022] (2) In the preparation process of the present invention, the high dispersibility of reduced graphene oxide (rGO) in the solvent and the strong π-π interaction with graphene (Gr) are utilized to intercalate rGO and Gr, which effectively improves the problem of Gr being easy to agglomerate in the solvent and the serious stacking warping during thermal deposition, thereby increasing the interlayer bonding force and the bonding force with the copper substrate; similarly, the strong adsorption of phthalocyanine to the copper substrate and the strong π-π interaction with Gr are utilized to increase the interlayer bonding force and the bonding force with the copper substrate, thereby improving the stability of the coating structure.
[0023] (3) The Gr / rGO / Cu or Gr / PC / Cu composites prepared by the present invention exhibit excellent electrical and electrochemical properties. The electrical conductivity of the composite material reaches 105% IACS at a length of 1 m, and the corrosion potential is E corr =-0.21 V vs. Ag / AgCl, corrosion current density is i corr = 6.31 × 10 -5 A.cm -2 .
[0024] (4) The preparation of graphene and reduced graphene oxide of the present invention can use natural graphene as raw material, which has a wide range of sources; PC is synthesized using a solid phase method, which is simple to operate and has low raw material costs. The graphene / copper composite material is prepared by a coating method, which is simple and efficient, low in cost, and can be industrialized on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the synthesis principle of the Gr / rGO / Cu-1 composite material prepared in Example 1.
[0027] Figure 2 It is a schematic diagram of coating a graphene dispersion on the surface of a copper wire, wherein: 1-copper wire, 2-graphene coating liquid container, 3-diamond wire drawing die, 4-preliminary drying equipment, 5-Gr / rGO / Cu composite material.
[0028] Figure 3 This is the XRD pattern of the Gr / rGO / Cu-1 composite material prepared in Example 1.
[0029] Figure 4 This is the XPS spectrum of the Gr / rGO / Cu-1 composite material prepared in Example 1.
[0030] Figure 5 This is a confocal three-dimensional reconstruction image of the Gr / rGO / Cu-1 composite material taken using a three-dimensional laser confocal microscope.
[0031] Figure 6 This is the SEM image of the Gr / rGO / Cu-1 composite material prepared in Example 1.
[0032] Figure 7 This is a transmission electron microscope image of the graphene dispersion of Example 1.
[0033] Figure 8 It is a conductivity test graph of copper wire, Gr / Cu-1 prepared in Control Example 1, and Gr / rGO / Cu-1 composite material prepared in Example 1.
[0034] Fig. 9 It is the TAFEL curve of copper wire, Gr / Cu-1 prepared in Control Example 1, and Gr / rGO / Cu-1 composite material prepared in Example 1 in 3.5wt% NaCl electrolyte.
[0035] Fig.10 It is the Nyquist curve of Gr / Cu-1 prepared in Control Example 1 and Gr / rGO / Cu-1 composite material prepared in Example 1 in 3.5 wt% NaCl electrolyte.
[0036] Fig.11 This is a cross-sectional SEM image of the Gr / rGO / Cu-1 composite material prepared in Example 1.
[0037] Fig.12 It is a conductivity test graph of copper wire, Gr / Cu-2 prepared in Control Example 2, and Gr / rGO / Cu-2 composite material prepared in Example 2.
[0038] Fig.13 This is the SEM image of the Gr / rGO / Cu-2 composite material prepared in Example 2.
[0039] Fig.14 It is a conductivity test graph of copper wire, Gr / Cu-3 prepared in Control Example 3, and Gr / PC / Cu composite material prepared in Example 3.
[0040] Fig.15 This is the SEM image of the Gr / PC / Cu composite material prepared in Example 3. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, reagents and materials used in the present invention are commercially available. It should be noted that, in the absence of conflict, the features in the embodiments of the present invention and the embodiments can be combined with each other. In order to enable those skilled in the art to better understand the technical scheme of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings.
[0044] The present invention provides a graphene additive and a method for preparing a high-conductivity graphene / copper composite material, so as to solve the problem that graphene has poor dispersibility in a solvent and the graphene coating in the currently prepared graphene / copper composite material is unevenly distributed and poorly combined with a copper substrate, resulting in poor overall conductivity of the graphene / copper composite material. The graphene / copper composite material is a graphene coating stacked and coated on a copper substrate. When preparing a graphene dispersion, reduced graphene oxide (rGO) or phthalocyanine material (PC) is added as a graphene additive, and rGO and Gr are intercalated with each other. This intercalation structure not only weakens the van der Waals force between graphene sheets and prevents agglomeration, but also provides steric hindrance and electrostatic stability, further promotes the uniform dispersion of graphene, improves the uniformity of the coating, makes the conductive network more continuous and complete, and the stacking between layers is more compact, improves the electron transmission efficiency, and thus significantly improves the conductivity and mechanical properties of the coating. Similarly, the introduction of the PC system, through the non-covalent interaction between PC and Gr, enables graphene to form a dense and flat stacking structure, thereby improving the interlayer bonding strength of graphene and the interface bonding between graphene and the copper substrate. This can effectively improve the transmission of electrons between copper and graphene, improve the bonding between the graphene coating and the copper substrate, ensure the stability of the coating, and make it less likely to fall off.
[0045] Example 1 In this example, a Gr / rGO / Cu composite material (denoted as Gr / rGO / Cu-1) is prepared, and the steps are as follows: (1) Preparation of graphene dispersion: 75 mg Gr and 10.7 mg rGO were dispersed in a mixed solvent A consisting of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP), and ultrasonically dispersed at a power of 800 W for 1 h. The mass of rGO accounts for 12.5% of the total mass of Gr and rGO, the volume ratio of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP) in the mixed solvent A is 6:5:3:1, and the total volume of the mixed solvent A is 5 mL; (2) Preparation of film-forming agent precursor solution: Disperse 0.3 g of rosin in 1 mL of mixed solvent B and disperse it ultrasonically at 800 W for 1 h.
[0046] The mixed solvent B has the same composition as the mixed solvent A described in step (1), and is also composed of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP), and the volume ratio of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP) is 6:5:3:1; (3) The graphene dispersion obtained in step (1) and the film-forming agent precursor solution obtained in step (2) are mixed and uniformly dispersed by ultrasonication to obtain a coating solution. The ultrasonic power is 800 W and the ultrasonic time is 2 h. The obtained coating solution is coated on the surface of a copper wire with a diameter of 0.3 mm by a coating machine (a coating machine of the model of Mai Ke MK-TTL2-21 can be selected). The coating speed is 5 m / min. The excess coating solution is scraped off by a diamond wire drawing die with an aperture of 0.32 mm, and then preliminary drying is performed. During the preliminary drying, a dryer (such as Figure 2 The temperature is set to 380 °C and the drying time is 0.2 min. (4) The graphene / copper composite sample after preliminary drying was dried in a forced air drying oven at 50 °C for 1 h, then vacuum dried in a vacuum drying oven at 120 °C for 1 h, and finally heat treated in a vacuum tube furnace at 280 °C for 30 min to obtain a graphene / copper composite material, denoted as Gr / rGO / Cu-1.
[0047] In this embodiment, a Gr / rGO / Cu-1 composite material is prepared by a coating method. The preparation method is simple. During the ultrasonic dispersion process, Gr and rGO are intercalated with each other. Figure 1 As shown, the van der Waals force of Gr in the coating solution can be weakened, the agglomeration tendency is greatly reduced, and the Gr dispersion is more uniform. After Gr and rGO are intercalated with each other, Gr and rGO are alternately stacked, which is more dense, and the interlayer bonding force between Gr and rGO is improved. The graphene sheet is spread more flat on the surface of the copper substrate, and the surface roughness of the graphene coating is significantly reduced, which largely maintains the integrity and stability of the coating structure.
[0048] Figure 2 This is a schematic diagram of coating graphene dispersion on the surface of copper wire. Nitrogen is introduced during the initial drying to prevent graphene oxidation.
[0049] Figure 3 and Figure 4 They are XRD and XPS spectra of the Gr / rGO / Cu-1 composite material prepared in this example, respectively, indicating that rGO and Gr are successfully intercalated with each other. Through calculation and comparison, it is found that the Gr interlayer spacing is expanded from 0.30 nm to 0.35 nm.
[0050] Figure 5This is a confocal three-dimensional reconstruction image of the Gr / rGO / Cu-1 composite material prepared in this example taken by a three-dimensional laser confocal microscope. Figure 6 This is the SEM image of the Gr / rGO / Cu-1 composite material prepared in this example. It can be seen that the surface of the Gr / rGO / Cu-1 composite material is smooth and the Gr warpage is low, which greatly reduces the surface roughness of the composite material.
[0051] Figure 7 This is a transmission electron microscope image of the graphene dispersion of this example. It can be seen that Gr has not agglomerated, indicating that after adding rGO, the dispersibility of Gr in the solvent is improved.
[0052] Comparative Example 1: Preparation of graphene dispersion: 85.7 mg Gr was dispersed in a mixed solvent A consisting of isopropyl alcohol (IPA), NN dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP), and ultrasonically dispersed at a power of 800 W for 1 h; the remaining steps were the same as in Example 1, and finally a Gr / Cu-1 composite material was obtained.
[0053] A 1 m long, 0.3 mm diameter pure copper wire (uncoated), Gr / Cu-1 prepared in Control Example 1, and Gr / rGO / Cu-1 composite material prepared in Example 1 were placed on a ZDCY-80 intelligent resistance tester. The two sides of the material were clamped with an instrument fixture. The conductivity test was performed at a constant length each time (the copper wire used for the three materials was the same, the test length was 1 m, and the diameter of the wire was measured at least 5 times before each test to take the average value). The results are shown in Figure 8 As shown, in Figure 8 It can be seen that the conductivity of the copper wire increases after the graphene coating. Compared with the control example 1, the conductivity of Gr / rGO / Cu-1 increases by about 5.5% IACS after adding rGO.
[0054] Pure copper wire, Gr / Cu-1, and Gr / rGO / Cu-1 composite materials were used as anodes, carbon rods as cathodes, and silver / silver chloride electrodes (Ag / AgCl) as reference electrodes. A 3.5 wt% NaCl solution was used as the electrolyte to assemble a three-electrode system. The electrochemical properties of pure copper wire, Gr / Cu-1, and Gr / rGO / Cu-1 were tested, and the frequency range of the impedance spectrum was extended from 0.01 Hz to 10 5 Hz, voltage amplitude is 5 mV. The test results are as follows Fig. 9 As shown in Figure 1, compared with the control example 1, the corrosion potential of the material positively shifted from -0.26 V (Gr / Cu-1) to -0.21 V (Gr / rGO / Cu-1), and the corrosion current density increased from 4.6×10 -4 A.cm -2(Gr / Cu-1) is reduced to 6.31×10 -5 A.cm -2 (Gr / rGO / Cu-1), indicating that the coating density and anti-permeability of the Gr / rGO / Cu-1 composite material obtained after adding rGO are significantly enhanced, so Gr / rGO / Cu-1 has better stability.
[0055] Fig.10 The Nyquist curves of Gr / Cu-1 and Gr / rGO / Cu-1 in 3.5 wt% NaCl electrolyte show that Gr / rGO / Cu-1 exhibits higher impedance than Gr / Cu-1. 4 ~10 5 At the frequency, the phase angle sweeps over a larger area, and the initial phase angle reaches 73°.
[0056] Fig.11 This is a cross-sectional SEM image of the Gr / rGO / Cu-1 composite material prepared in Example 1. It can be seen that the graphene coating is tightly stacked with a thickness of about 2 μm, and the graphene coating is tightly bonded to the interface of the copper substrate.
[0057] The above shows that after adding rGO, rGO and Gr are successfully intercalated with each other, the dispersibility of the graphene dispersion is improved, and after coating on the copper substrate, the graphene coating has a better interface bonding with the copper substrate and the coating has better density, which makes the graphene / copper composite material (Gr / rGO / Cu) have higher conductivity.
[0058] Example 2 In this example, a Gr / rGO / Cu composite material (Gr / rGO / Cu-2) is prepared, and the steps are as follows: (1) Preparation of graphene dispersion: 64 mg Gr and 21.7 mg rGO were dispersed in a mixed solvent A consisting of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP), and ultrasonically dispersed at a power of 800 W for 1 h. The mass of rGO accounts for 25% of the total mass of Gr and rGO, the volume ratio of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP) in the mixed solvent A is 6:5:3:1, and the total volume of the mixed solvent A is 5 mL; (2) Preparation of film-forming agent precursor solution: 0.3 g of rosin was dispersed in 1 mL of mixed solvent B, the composition of which was the same as that of the mixed solvent A described in step (1), and ultrasonically dispersed at a power of 800 W for 1 h. (3) The graphene dispersion obtained in step (1) and the film-forming agent precursor solution obtained in step (2) are mixed and uniformly dispersed by ultrasonication to obtain a coating solution. The ultrasonic power is 800 W and the ultrasonic time is 2 h. The obtained coating solution is coated on the surface of a 0.3 mm diameter copper wire through a coating machine (a coating machine of the model of Mai Ke MK-TTL2-21 can be selected). The coating speed is 5 m / min. The excess coating solution is scraped off with a diamond wire drawing die with an aperture of 0.32 mm, and then preliminary drying is performed. During the preliminary drying, the temperature of the upper drying machine is set to 380 °C and the drying time is 0.2 min. (4) The graphene / copper composite sample after preliminary drying was dried in a forced air drying oven at 50 °C for 1 h, then vacuum dried in a vacuum drying oven at 120 °C for 1 h, and finally heat treated in a vacuum tube furnace at 280 °C for 30 min to obtain a graphene / copper composite material, denoted as Gr / rGO / Cu-2, with a diameter of about 0.3 mm.
[0059] Comparative Example 2 Preparation of graphene dispersion: 85.7 mg Gr was dispersed in a mixed solvent A consisting of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP), and ultrasonically dispersed at a power of 800 W for 1 h; the rest was the same as in Example 2, and finally a Gr / Cu-2 composite material was obtained.
[0060] A 1 m long pure copper wire (uncoated), Gr / Cu-2 prepared in Control Example 2, and Gr / rGO / Cu-2 composite material prepared in Example 2 were placed on a ZDCY-80 intelligent resistance tester. The two sides of the material were clamped with an instrument fixture. The conductivity test was performed at a constant length each time (the copper wire used for the three materials was the same, the test length was 1 m, and the diameter of the wire was measured at least 5 times before each test to take the average value). The results are shown in Fig.12 As shown, in Fig.12 It can be seen that the conductivity of copper wire increases after being coated with graphene. Compared with Gr / Cu-2, the conductivity of Gr / rGO / Cu-2 increases by about 5.3% IACS after adding rGO.
[0061] The Gr / rGO / Cu-2 composite material was observed by scanning electron microscopy. Fig.13 As shown, it can be seen that the surface of the Gr / rGO / Cu-2 composite material obtained by adding rGO is relatively smooth and its structure is more stable.
[0062] Example 3 In this embodiment, the Gr / PC / Cu composite material is prepared, and the method steps are as follows: (1) Preparation of graphene dispersion: 85.7 mg Gr and 7 mg phthalocyanine (PC) were dispersed in a mixed solvent A consisting of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP), and ultrasonically dispersed at a power of 800 W for 1 h.
[0063] Among them, 7 mg phthalocyanine material (PC) is composed of 3.5 mg aluminum phthalocyanine (AlPC) and 3.5 mg cobalt phthalocyanine (CoPC), the volume ratio of isopropyl alcohol (IPA), NN dimethylformamide (DMF), pinene alcohol, and N-methylpyrrolidone (NMP) in the mixed solvent A is 6:5:3:1, the total volume of the mixed solvent A is 5 mL, and the concentration of PC in the mixed solvent A is 1.4 mg / mL.
[0064] (2) Preparation of film-forming agent precursor solution: 0.3 g of rosin was dispersed in 1 mL of mixed solvent B, where the composition of mixed solvent B was the same as that of mixed solvent A described in step (1), and ultrasonically dispersed at a power of 800 W for 1 h.
[0065] (3) The graphene dispersion obtained in step (1) and the film-forming agent precursor solution obtained in step (2) are mixed and uniformly dispersed by ultrasonication to obtain a coating solution. The ultrasonic power is 800 W and the ultrasonic time is 2 h. The obtained coating solution is coated on the surface of a 0.3 mm diameter copper wire through a coating machine (the coating machine of the model of Mai Ke MK-TTL2-21 can be selected). The coating speed is 5 m / min. The excess coating solution is scraped off with a diamond wire drawing die with an aperture of 0.32 mm, and then preliminary drying is performed. During the preliminary drying, the temperature of the upper dryer is set to 380 °C and the drying time is 0.2 min.
[0066] (4) The graphene / copper composite sample after preliminary drying was dried in a forced air drying oven at 50 °C for 1 h, then vacuum dried in a vacuum drying oven at 120 °C for 1 h, and finally heat treated in a vacuum tube furnace at 280 °C for 30 min to obtain a graphene / copper composite material, denoted as Gr / PC / Cu, with a diameter of about 0.3 mm.
[0067] Comparative Example 3 Preparation of graphene dispersion: 85.7 mg Gr was dispersed in a mixed solvent A consisting of isopropyl alcohol (IPA), N-dimethylformamide (DMF), terpineol, and N-methylpyrrolidone (NMP), and ultrasonically dispersed at a power of 800 W for 1 h; the rest was the same as in Example 3, and finally a Gr / Cu-3 composite material was obtained.
[0068] A 1 m long pure copper wire (uncoated), Gr / Cu-3 prepared in Control Example 3, and Gr / PC / Cu composite material prepared in Example 3 were placed on a ZDCY-80 intelligent resistance tester. The two sides of the material were clamped with an instrument fixture. The conductivity test was performed at a constant length each time (the copper wire used for the three materials was the same, the test length was 1 m, and the diameter of the wire was measured at least 5 times before each test to take the average value). The results are as follows: Fig.14 As shown, in Fig.14 It can be seen that the conductivity of the copper wire increases after the graphene coating is applied. Compared with the control example 3, the conductivity of Gr / PC / Cu increases by about 6.5% IACS after adding PC.
[0069] The Gr / PC / Cu composite material was observed by scanning electron microscopy. Fig.15 As shown, it can be seen that the surface of the Gr / PC / Cu composite material obtained by adding PC is smoother and its structure is more stable.
[0070] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A graphene additive, characterized in that: The graphene additive is reduced graphene oxide or phthalocyanine material, and the phthalocyanine material is a composite of aluminum phthalocyanine and cobalt phthalocyanine in a mass ratio of 1:3 to 3:
1.
2. A method for preparing a high-conductivity graphene / copper composite material, characterized in that: The following steps are involved: (1) Preparation of graphene dispersion: dispersing graphene nanosheets and graphene additives in a mixed solvent A consisting of isopropanol, N-dimethylformamide, terpineol, and N-methylpyrrolidone, and uniformly dispersing by ultrasonication; (2) Preparation of film-forming agent precursor solution: a certain amount of rosin is dispersed in a mixed solvent B consisting of isopropyl alcohol, N-dimethylformamide, terpineol, and N-methylpyrrolidone, and ultrasonically dispersed until the rosin is dissolved; (3) mixing the graphene dispersion obtained in step (1) and the film-forming agent precursor solution obtained in step (2), and uniformly dispersing them by ultrasonication to obtain a coating solution; coating the coating solution on the surface of the copper wire, and then preliminarily drying it; (4) The dried sample is dried in a forced air drying oven and a vacuum drying oven in turn, and then thermally deposited in a vacuum tube furnace to obtain a high-conductivity graphene / copper composite material.
3. The method for preparing the high-conductivity graphene / copper composite material according to claim 2, characterized in that: The graphene additive in step (1) is reduced graphene oxide or phthalocyanine material, and the phthalocyanine material is a composite of aluminum phthalocyanine and cobalt phthalocyanine in a mass ratio of 1:3 to 3:
1.
4. The method for preparing the high-conductivity graphene / copper composite material according to claim 3, characterized in that: When reduced graphene oxide is selected as the graphene additive, the reduced graphene oxide accounts for 10-50% of the total mass of graphene and reduced graphene oxide, and the total concentration of graphene and reduced graphene oxide in the mixed solvent A is 1.5-30 mg / mL.
5. The method for preparing the high-conductivity graphene / copper composite material according to claim 3, characterized in that: When phthalocyanine material is selected as the graphene additive, the concentration of graphene in the mixed solvent A is 1.5-30 mg / mL, and the concentration of phthalocyanine material in the mixed solvent A is 1-10 mg / mL.
6. The method for preparing the high-conductivity graphene / copper composite material according to claim 2, characterized in that: The volume percentages of isopropanol, N-dimethylformamide, terpineol and N-methylpyrrolidone in the mixed solvent A in step (1) are 30-40%, 25-35%, 10-20% and 5-15% respectively. The mixed solvent B in step (2) has the same components and proportions as the mixed solvent A in step (1).
7. The method for preparing the high-conductivity graphene / copper composite material according to claim 2 or 6, characterized in that: The concentration of rosin in the mixed solvent B is 0.1~0.5 g / mL.
8. The method for preparing the high-conductivity graphene / copper composite material according to claim 2, characterized in that: In step (3), the ultrasonic power is 500-900 W, and the ultrasonic time is 1-3 h.
9. The method for preparing the high-conductivity graphene / copper composite material according to claim 2, characterized in that: In step (3), the diameter of the copper wire is 0.2-0.5 mm, the coating speed is 2-20 m / min, the initial drying temperature is 180-380 °C, and the drying time is 0.05-0.5 min.
10. The method for preparing the high-conductivity graphene / copper composite material according to claim 2, characterized in that: In step (4), the temperature of the blast drying oven is set to 50~80°C, and the drying time is 0.5~2 h; the temperature of the vacuum drying oven is set to 80~150°C, and the drying time is 0.5~2 h; the temperature of the vacuum tube furnace thermal deposition is 260~500°C, and the processing time is 0.1~1 h.