Reflective heat-insulating coating as well as preparation method and application thereof

By combining three hollow acrylic emulsions with different particle sizes and elastic acrylic emulsions, combined with a specific preparation process, the shortcomings of existing coatings in terms of reflective insulation, mechanical properties and weather resistance are solved, and efficient reflection isolation is achieved Thermal and mechanical properties are improved and suitable for building walls.

CN118931280AActive Publication Date: 2024-11-12SICHUAN UNIV +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411158199.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing reflective thermal insulation coatings have shortcomings in taking into account reflective thermal insulation performance, mechanical properties and weather resistance, and it is difficult to meet the needs of exterior wall buildings.

Method used

Three hollow acrylic emulsions with different particle size ranges are combined. The shell layer of the hollow microspheres has a specific dimensional relationship with the particle size. Combined with the elastic acrylic emulsion, a coating with good thermal insulation and light shielding is formed, and the coating is formed through specific The preparation process improves the stability of microspheres.

Benefits of technology

The coating has achieved efficient reflective thermal insulation, mechanical properties and weather resistance, and the solar light reflectance, near-infrared reflectance and hemispherical emissivity have been significantly improved, and the tensile strength and elongation of break have also been significantly improved. It is suitable for building walls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005677720000141
    Figure BDA0005005677720000141
  • Figure HDA0005005677730000011
    Figure HDA0005005677730000011
Patent Text Reader

Abstract

The invention belongs to the technical field of coatings, and particularly relates to a reflective heat-insulating coating as well as a preparation method and application thereof. The reflective heat-insulating coating comprises a hollow acrylic emulsion A, a hollow acrylic emulsion B, a hollow acrylic emulsion C and an elastic acrylic emulsion, latex particles in the hollow acrylic emulsion A, the hollow acrylic emulsion B and the hollow acrylic emulsion C are hollow microspheres; the ratio of the thickness of the shell layer of the hollow microsphere to the particle size of the hollow microsphere is (9-33): 100; the particle sizes of latex particles in the hollow acrylic emulsion A, the hollow acrylic emulsion B and the hollow acrylic emulsion C are 450 to 750 nm, 900 to 1300 nm and 1400 to 1800 nm respectively. According to the invention, three kinds of hollow acrylic acid emulsions with different particle sizes are compounded, and hollow microspheres with different sizes have a synergistic effect, so that the reflective insulation performance, the mechanical property, the stain resistance and the weather resistance of the coating can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a reflective heat-insulating coating and a preparation method and application thereof. Background Art

[0002] With the development and progress of society, energy-saving urban building materials have attracted much attention. Energy-saving buildings can significantly reduce energy consumption, alleviate energy supply pressure, reduce environmental pollution, and better meet ecological needs.

[0003] Reflective heat insulation is one of the important indicators for evaluating the performance of exterior wall architectural coatings, but the reflective heat insulation effect that existing exterior wall coatings can provide is limited. Some studies have tried to improve the reflective heat insulation performance by adding glass microspheres, but their tensile strength is poor and they are very easy to crack during long-term use, thus causing the paint film to be damaged. Some studies have tried to improve the reflective heat insulation performance by adding polyethylene hollow microspheres, but their weather resistance is poor and as exterior wall coatings, they will have problems such as yellowing and aging, and the reflective heat insulation performance needs to be further improved. In short, it is difficult for current reflective heat insulation coatings to take into account reflective heat insulation performance, mechanical properties and weather resistance.

[0004] Therefore, it is of great significance to provide a coating that has good reflective thermal insulation performance, mechanical properties and weather resistance. Summary of the invention

[0005] The present invention aims to solve one or more technical problems existing in the above-mentioned prior art, and at least provide a beneficial choice or create conditions. Specifically, the present invention provides a reflective heat-insulating coating, which has good reflective heat-insulating performance, mechanical properties and weather resistance, and can meet the requirements of exterior wall buildings for coating performance.

[0006] The inventive concept of the present invention is as follows: the coating of the present invention comprises hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C and elastic acrylic emulsion; the particle sizes of latex particles in the hollow acrylic emulsion A, hollow acrylic emulsion B and hollow acrylic emulsion C are 450-750nm, 900-1300nm and 1400-1800nm ​​respectively; the latex particles in the hollow acrylic emulsion A, hollow acrylic emulsion B and hollow acrylic emulsion C are all hollow microspheres; the hollow microspheres comprise a shell layer, and the ratio of the thickness of the shell layer to the particle size of the hollow microspheres is (9-33):100. When the polymer microspheres with hollow structures of the present invention are in liquid state, the cavity is filled with water, and after the water evaporates and dries, the cavity is filled with air. Since the refractive index of the shell polymer and the air in the hollow part is quite different, the coating can be endowed with good heat insulation and light-shielding properties, and the polymer hollow microspheres have excellent properties such as deformability and small specific gravity, so that the coating has better tensile strength and can better resist cracking of the base layer. At the same time, the present invention adopts three hollow acrylic emulsions with different particle size ranges to compound, and hollow microspheres of different sizes can play a synergistic role, and the shell layer of the hollow microspheres and the particle size of the hollow microspheres have a specific size relationship, which is conducive to improving the reflective heat insulation performance, mechanical properties, stain resistance and weather resistance of the coating.

[0007] Therefore, a first aspect of the present invention provides a reflective, heat-insulating coating.

[0008] Specifically, the reflective heat-insulating coating includes hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C, and elastic acrylic emulsion;

[0009] The particle sizes of the latex particles in the hollow acrylic emulsion A, the hollow acrylic emulsion B, and the hollow acrylic emulsion C are 450-750 nm, 900-1300 nm, and 1400-1800 nm, respectively;

[0010] The latex particles in the hollow acrylic emulsion A, the hollow acrylic emulsion B and the hollow acrylic emulsion C are all hollow microspheres; the hollow microspheres include a shell layer, and the ratio of the thickness of the shell layer to the particle size of the hollow microspheres is (9-33):100.

[0011] Preferably, the hollow microspheres include a shell layer; the ratio of the thickness of the shell layer to the particle size of the hollow microspheres is (10-30):100.

[0012] Preferably, the particle sizes of the latex particles in the hollow acrylic emulsion A, the hollow acrylic emulsion B, and the hollow acrylic emulsion C are 500-700 nm, 1000-1200 nm, and 1500-1700 nm, respectively.

[0013] Preferably, in the coating, the hollow acrylic emulsion A, the hollow acrylic emulsion B, and the hollow acrylic emulsion C are all 1.8-11 parts by weight.

[0014] Further preferably, in the coating, the hollow acrylic emulsion A, the hollow acrylic emulsion B, and the hollow acrylic emulsion C are all 2-10 parts by weight.

[0015] Preferably, the solid content of the elastic acrylic emulsion is 45-60%; further preferably, the solid content of the elastic acrylic emulsion is 48-55%.

[0016] Preferably, the particle size of the latex particles in the elastic acrylic emulsion is 90-330 nm; further preferably, the particle size of the latex particles in the elastic acrylic emulsion is 100-300 nm.

[0017] Preferably, the coating further comprises at least one of a filler, a wetting agent, a dispersant, a defoamer, a thickener, a bactericide, a preservative, a mildew preventer, a pH adjuster, an antifreeze-thaw aid, a film-forming aid, a functional aid, and water.

[0018] Preferably, the coating comprises hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C, elastic acrylic emulsion, filler, wetting agent, dispersant, defoamer, thickener, bactericide, preservative, mildewproof agent, pH adjuster, antifreeze-thaw aid, film-forming aid, functional aid, and water; and by weight, the coating comprises hollow acrylic emulsion A 1.8-11 parts, hollow acrylic emulsion B 1.8-11 parts, hollow acrylic emulsion C 1.8-11 parts, elastic acrylic emulsion 18-33 parts, filler 23-40 parts, wetting agent 0.27-0.55 parts, dispersant 0.55-1.2 parts, defoaming agent 0.55-1.1 parts, thickener 0.27-0.55 parts, bactericide 0.1-0.33 parts, preservative 0.18-0.33 parts, mildewproof agent 0.18-0.44 parts, pH adjuster 0.1-0.22 parts, antifreeze-thaw aid 0.9-2.2 parts, film-forming aid 0.45-1.1 parts, functional additive 0.9-2.2 parts, water 20-25 parts.

[0019] Further preferably, the coating comprises hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C, elastic acrylic emulsion, filler, wetting agent, dispersant, defoamer, thickener, bactericide, preservative, mildewproof agent, pH adjuster, antifreeze-thaw aid, film-forming aid, functional aid, and water; and by weight, the coating comprises 2-10 parts of hollow acrylic emulsion A, 2-10 parts of hollow acrylic emulsion B, 10 parts of hollow acrylic emulsion C, 10 parts of hollow acrylic emulsion C, 10 parts of hollow acrylic emulsion A, 10 parts of hollow acrylic emulsion B, 10 parts of hollow acrylic emulsion C, 10 parts of hollow acrylic emulsion C, 10 parts of hollow acrylic emulsion A, 10 parts of hollow acrylic emulsion B, 10 parts of hollow acrylic emulsion C, 10 parts of hollow acrylic emulsion A ... 2-10 parts, elastic acrylic emulsion 20-30 parts, filler 25-38 parts, wetting agent 0.3-0.5 parts, dispersant 0.6-1.1 parts, defoamer 0.6-1.0 parts, thickener 0.3-0.5 parts, bactericide 0.1-0.3 parts, preservative 0.2-0.3 parts, mildewproof agent 0.2-0.4 parts, pH adjuster 0.1-0.2 parts, antifreeze-thaw aid 1-2 parts, film-forming aid 0.5-1.0 parts, functional additive 1-2 parts, water 20-25 parts.

[0020] Preferably, the filler includes at least one of calcite powder, titanium dioxide and diatomaceous earth; further preferably, the filler includes calcite powder, titanium dioxide and diatomaceous earth.

[0021] Preferably, the wetting agent includes at least one of anionic wetting agents and nonionic wetting agents.

[0022] Preferably, the dispersant includes at least one of polycarboxylates, polyacrylates, and carboxylic acid copolymer salts.

[0023] Preferably, the defoaming agent includes at least one of polymer composite mineral oil, metal soap defoaming agent and silicone defoaming agent.

[0024] Preferably, the thickener comprises hydroxyethyl cellulose.

[0025] Preferably, the fungicide includes at least one of pyrimidine copper zinc thiourea and zinc oxide; further preferably, the fungicide includes pyrimidine copper zinc thiourea and zinc oxide.

[0026] Preferably, the preservative includes at least one of 5-chloro-2-methyl-4-isothiazoline-3-one and 2-methyl-4-isothiazoline-3-one; further preferably, the preservative includes 5-chloro-2-methyl-4-isothiazoline-3-one and 2-methyl-4-isothiazoline-3-one.

[0027] Preferably, the mildewcide comprises methyl 2-benzimidazolecarbamate.

[0028] Preferably, the pH adjuster comprises 2-amino-2-methyl-1-propanol.

[0029] Preferably, the antifreeze-thaw aid comprises propylene glycol.

[0030] Preferably, the film-forming aid comprises dodecyl alcohol ester.

[0031] Preferably, the functional additive comprises a nonionic polyurethane leveling modifier.

[0032] Preferably, the raw materials for preparing the hollow acrylic emulsion A, the hollow acrylic emulsion B, and the hollow acrylic emulsion C all include an emulsifier, an unsaturated acid, an olefin monomer, an initiator, a seed emulsion, and water;

[0033] The raw materials for preparing the seed emulsion include emulsifier, unsaturated acid, olefin monomer, initiator, siloxane compound with active groups and water.

[0034] Preferably, the emulsifier is selected from at least one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, fatty alcohol polyoxyethylene ether, polyoxyethylene alkyl ester, and sodium cetyl betaine.

[0035] Preferably, the unsaturated acid is selected from at least one of acrylic acid, methacrylic acid, itaconic acid and fumaric acid.

[0036] Preferably, the olefin monomer is selected from at least one of styrene, methyl methacrylate, butyl acrylate, acrylonitrile and isooctyl acrylate.

[0037] Preferably, the initiator is selected from at least one of sodium persulfate, ammonium persulfate and potassium persulfate.

[0038] Preferably, the siloxane compound with active groups is prepared by a preparation method comprising the following steps: methacryloxypropyl alkoxysilane reacts with alkyl silicate to prepare the siloxane compound with active groups.

[0039] Specifically, the siloxane compound with active groups can improve the stability of hollow microspheres during the synthesis process, solve the problem that hollow microspheres are easily broken during expansion, improve the thermal insulation performance of hollow acrylic emulsion, and thus make the coating prepared using the siloxane compound have good reflective thermal insulation effect.

[0040] The second aspect of the present invention provides a method for preparing the reflective heat-insulating coating according to the first aspect of the present invention.

[0041] Specifically, the method for preparing the reflective heat-insulating coating comprises the following steps:

[0042] The coating is prepared by mixing various raw material components.

[0043] Preferably, the method for preparing the reflective heat-insulating coating comprises the following steps:

[0044] (1) dissolving the dispersant and wetting agent in water, adding the thickener, and then adding the pH adjuster and filler, mixing to obtain a premix;

[0045] (2) Mixing the remaining components with the premix obtained in step (1) to prepare the coating.

[0046] Preferably, in step (1), after the thickener is added and mixed until the solution becomes a slurry, the pH adjuster and filler are added and mixed to obtain a premix.

[0047] Preferably, step (2) is specifically as follows: when the particle size of the premix obtained in step (1) is less than 50 μm, bactericide, preservative, mildew preventer, antifreeze-thaw aid, film-forming aid and functional aid are added and mixed, and then hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C, elastic acrylic emulsion and defoaming agent are added and mixed to obtain the reflective heat-insulating coating.

[0048] Preferably, the preparation methods of the hollow acrylic emulsion A, the hollow acrylic emulsion B, and the hollow acrylic emulsion C all include the following steps:

[0049] S1: reacting an emulsifier, an unsaturated acid, an olefin monomer, an initiator, a siloxane compound with an active group and water to obtain the seed emulsion;

[0050] S2: reacting an emulsifier, an unsaturated acid, an olefin monomer, an initiator, water and the seed emulsion obtained in step (1) to obtain the hollow acrylic emulsion A, the hollow acrylic emulsion B or the hollow acrylic emulsion C.

[0051] Preferably, step S1 specifically includes the following steps: mixing an emulsifier, an unsaturated acid, an olefin monomer and water, first adding part of the initiator to carry out reaction a, then adding the remaining initiator to carry out reaction b, and finally adding a siloxane compound with an active group to carry out reaction c to obtain the seed emulsion.

[0052] Preferably, the reaction a is carried out at 80-90°C for 10-20 min; further preferably, the reaction a is carried out at 83-85°C for 10-20 min.

[0053] Preferably, the reaction b is carried out at 80-90°C for 3-5 h; further preferably, the reaction b is carried out at 83-85°C for 3.5-4.5 h.

[0054] Preferably, the reaction c is carried out at 80-90°C for 1-3 h; further preferably, the reaction c is carried out at 83-85°C for 1.5-2.5 h.

[0055] Preferably, step S2 specifically comprises the following steps: mixing the seed emulsion and water, adding part of the initiator, slowly adding a mixture consisting of an emulsifier, an unsaturated acid, an olefin monomer, and the remaining initiator, and reacting to obtain the hollow acrylic emulsion A, the hollow acrylic emulsion B, or the hollow acrylic emulsion C.

[0056] Preferably, the reaction temperature of the reaction in step S2 is 80-93°C; further more preferably, the reaction temperature of the reaction in step S2 is 85-88°C.

[0057] Preferably, in step S2, after completion of the reaction, post-treatment is performed using tert-butyl hydroperoxide and ascorbic acid.

[0058] The third aspect of the present invention provides a use of the reflective heat-insulating coating described in the first aspect of the present invention in the field of construction.

[0059] Preferably, the construction field includes building exterior walls.

[0060] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0061] (1) The present invention uses three hollow acrylic emulsions with different particle size ranges to compound, and hollow microspheres of different sizes can play a synergistic role, and the shell layer of the hollow microspheres and the particle size of the hollow microspheres have a specific size relationship, which is beneficial to the reflective heat insulation performance, mechanical properties, stain resistance, and weather resistance of the coating. The solar reflectance of the reflective heat insulation coating of the present invention is 0.86-0.88, the near-infrared reflectance is 0.87-0.9, the hemispherical emissivity is as high as 0.91-0.93, and the temperature in the measuring room of the heat insulation performance test can even be reduced by 11.8°C. The tensile strength is 2.82-2.89MPa, and the elongation at break is 488-507%. It has great application potential in the field of building walls.

[0062] (2) The latex particles in the hollow acrylic emulsion of the present invention are polymer microspheres with a hollow structure. When in a liquid state, the cavity is filled with water, and after the water evaporates and dries, the cavity is filled with air. Since the refractive index of the shell polymer and the air in the hollow part is quite different, the coating can be endowed with good heat insulation and light-shielding properties. In addition, the polymer hollow microspheres have excellent properties such as deformability and low specific gravity, so that the coating has more excellent mechanical properties and can better resist cracking of the base layer.

[0063] (3) The preparation process of the present invention is simple and convenient for large-scale production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 Schematic diagram of the device for testing the thermal insulation performance of the present invention. DETAILED DESCRIPTION

[0065] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0066] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0067] Example 1

[0068] A reflective heat-insulating coating, comprising, by weight, 4 parts of a hollow acrylic emulsion A with a latex particle size of 450 nm, 3 parts of a hollow acrylic emulsion B with a latex particle size of 900 nm, and 3 parts of a hollow acrylic emulsion C with a latex particle size of 1700 nm. 3 parts, elastic acrylic emulsion 25 parts, filler 26 parts (calcite powder 5 parts, rutile titanium dioxide 20 parts, diatomaceous earth 1 part), non-ionic alkyl polyoxyethylene ether wetting agent 0.4 parts, polyacrylate ammonium salt dispersant 0.6 parts, mineral oil defoamer 0.6 parts, thickener hydroxyethyl cellulose 0.3 parts, fungicide (a mixture of pyrimidine copper zinc and zinc oxide) 0.3 parts, preservative (a mixture of 5-chloro-2-methyl-4-isothiazoline-3-one and 2-methyl-4-isothiazoline-3-one) 0.3 parts, mildewproof agent 2-benzimidazole methyl carbamate 0.4 parts, pH adjuster 2-amino-2-methyl-1-propanol 0.1 parts, antifreeze-thaw aid propylene glycol 2 parts, film-forming aid dodecanol ester 0.5 parts, functional aid non-ionic polyurethane leveling agent 2 parts, water 25 parts;

[0069] The latex particles in hollow acrylic emulsion A, hollow acrylic emulsion B and hollow acrylic emulsion C are all hollow microspheres;

[0070] The ratio of the shell thickness to the particle size of the three hollow microspheres is 20:100.

[0071] A method for preparing a reflective heat-insulating coating comprises the following steps:

[0072] Add water, wetting agent, dispersant and 20% defoamer under stirring at 200 rpm, and stir for 3 minutes; adjust the speed to 400 rpm, add thickener, and stir for 2 minutes; adjust the speed to 1200 rpm, add filler, and stir for 15 minutes; adjust the speed to 900 rpm, add film-forming aid, antifreeze agent, bactericidal and mildew-proof preservative, and stir for 3 minutes; then add hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C, and elastic acrylic emulsion and stir for 3 minutes; add functional additives and stir for 3 minutes; add the remaining defoamer, stir evenly, and obtain a reflective heat-insulating coating.

[0073] The method for preparing a hollow acrylic emulsion having a latex particle size of 450 nm comprises the following steps:

[0074] (1) First, 100 g of ethyl silicate was added to 50 g of deionized water and stirred evenly. During the stirring process, 0.01 g of acetic acid was added, the temperature was raised to 45° C., and the stirring was continued for 5 min. Then, 10 g of γ-methacryloxypropyltriethoxysilane monomer was dropped into the water. After reacting for 30 min, the temperature was lowered, and 0.1% (w / v) of tetrahydroxypropylethylenediamine was added to the mixed solution as a stabilizer. Finally, the mixture was filtered to obtain a siloxane compound with an active group.

[0075] (2) dispersing 1 part of emulsifier sodium dodecylbenzene sulfonate (DS-4) in 16.43 parts of deionized water, slowly adding 21.36 parts of olefin monomer methyl methacrylate (MMA) and 11.5 parts of unsaturated acid methacrylic acid (MAA) into the water under stirring, dispersing at a speed of 600 rpm for 10 minutes, and preparing a pre-emulsion for dropwise reaction; mixing sodium persulfate and water evenly, and setting aside as a titration initiator;

[0076] (3) Prepare a reaction flask, add 23.66 parts of water into it, heat it to 85° C., add 20% pre-emulsion (a total of 50.29 parts of pre-emulsion), and add an aqueous solution of 0.13 parts of sodium persulfate and 0.82 parts of water, keep the temperature at 84° C. for 15 minutes, and show a blue fluorescent state; continue to dropwise add the remaining pre-emulsion and an aqueous solution of 0.07 parts of sodium persulfate and 8.22 parts of water at 84° C. at a uniform rate, and stir at a uniform rate for 4 hours until the reaction forms an emulsion; then add 6.67 parts of the siloxane compound with active groups obtained in step (1) into the reaction flask at one time, wash it with water, control the temperature to 84° C., keep the temperature for 2 hours, and finally cool it down, filter the emulsion, and obtain a seed emulsion;

[0077] (4) 14.59 parts of seed emulsion were added to 36.47 parts of water, the temperature was raised to 92°C, an aqueous solution of 0.07 parts of sodium persulfate and 0.36 parts of water was added, and an emulsion consisting of 0.51 parts of sodium dodecylbenzene sulfonate (DS-4), 21.74 parts of styrene (ST), 1.46 parts of methyl methacrylate (MMA), 0.05 parts of allyl methacrylate (AMA), 0.15 parts of methacrylic acid (MAA) and 17.51 ​​parts of water and 0. 07 parts of sodium persulfate and 3.65 parts of water aqueous solution, the dripping time is 150min, when the emulsion is dripped to 45%, 1.09 parts of ammonia water is added, react for 5min, and continue to drip; after the dripping reaction, the temperature is lowered to 82°C, and tert-butyl hydroperoxide and ascorbic acid are used for post-treatment reaction, and the temperature is kept for 20min; the material is discharged after the temperature is lowered to below 50°C to obtain a hollow acrylic emulsion with a latex particle size of 450nm and a shell thickness to hollow microsphere particle size ratio of 20:100.

[0078] The difference between the preparation method of the hollow acrylic emulsion with a latex particle diameter of 900nm and the preparation method of the hollow acrylic emulsion with a latex particle diameter of 450nm is that: in step (2), 1 part of emulsifier sodium dodecylbenzene sulfonate (DS-4) is dispersed in 16.44 parts of deionized water, and 21.38 parts of olefin monomer methyl methacrylate (MMA) and 11.51 parts of unsaturated acid methacrylic acid (MAA) are slowly added to the above water under stirring; in step (3), a reaction flask is prepared, 23.68 parts of water are added thereto, and 20% of pre-emulsion liquid (a total of 50.33 parts of pre-emulsion liquid) is added; the other steps are the same as the preparation method of the hollow acrylic emulsion with a latex particle diameter of 450nm, and the hollow acrylic emulsion with a latex particle diameter of 900nm and a ratio of the thickness of the shell layer to the particle diameter of the hollow microsphere of 20:100 is obtained.

[0079] The difference between the preparation method of the hollow acrylic emulsion with a latex particle diameter of 1700nm and the preparation method of the hollow acrylic emulsion with a latex particle diameter of 450nm is that: in step (2), 1 part of emulsifier sodium dodecylbenzene sulfonate (DS-4) is dispersed in 16.45 parts of deionized water, and 21.39 parts of olefin monomer methyl methacrylate (MMA) and 11.52 parts of unsaturated acid methacrylic acid (MAA) are slowly added to the above water under stirring; in step (3), a reaction flask is prepared, 23.7 parts of water are added thereto, and 20% of pre-emulsion liquid (a total of 50.36 parts of pre-emulsion liquid) is added; 6.68 parts of siloxane compound with active groups are added to the reaction kettle at one time; the other steps are the same as the preparation method of the hollow acrylic emulsion with a latex particle diameter of 450nm, and the hollow acrylic emulsion with a latex particle diameter of 1700nm and a ratio of the thickness of the shell layer to the particle diameter of the hollow microsphere of 20:100 is obtained.

[0080] Example 2

[0081] A reflective heat-insulating coating, comprising, by weight, 2 parts of a hollow acrylic emulsion A with a latex particle size of 600 nm, 3 parts of a hollow acrylic emulsion B with a latex particle size of 1000 nm, and 1600 nm of a hollow acrylic emulsion C. 5 parts, elastic acrylic emulsion 25 parts, filler 26 parts (calcite powder 5 parts, rutile titanium dioxide 20 parts, diatomaceous earth 1 part), nonionic alkyl polyoxyethylene ether wetting agent 0.4 parts, polyacrylate ammonium salt dispersant 0.6 parts, mineral oil defoamer 0.6 parts, thickener hydroxyethyl cellulose 0.3 parts, fungicide (a mixture of pyrimidine copper zinc and zinc oxide) 0.3 parts, preservative (a mixture of 5-chloro-2-methyl-4-isothiazoline-3-one and 2-methyl-4-isothiazoline-3-one) 0.3 parts, mildewproof agent 2-benzimidazole methyl carbamate 0.4 parts, pH adjuster 2-amino-2-methyl-1-propanol 0.1 parts, antifreeze-thaw aid propylene glycol 2 parts, film-forming aid dodecanol ester 0.5 parts, functional aid nonionic polyurethane leveling agent 2 parts, water 25 parts;

[0082] The latex particles in hollow acrylic emulsion A, hollow acrylic emulsion B and hollow acrylic emulsion C are all hollow microspheres;

[0083] The ratio of the shell thickness to the particle size of the hollow microspheres of the three particle sizes is 20:100.

[0084] A method for preparing a reflective heat-insulating coating comprises the following steps:

[0085] Add water, wetting agent, dispersant and 20% defoamer under stirring at 200 rpm, and stir for 3 minutes; adjust the speed to 400 rpm, add thickener, and stir for 2 minutes; adjust the speed to 1200 rpm, add filler, and stir for 15 minutes; adjust the speed to 900 rpm, add film-forming aid, antifreeze agent, bactericidal and mildew-proof preservative, and stir for 3 minutes; then add hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C, and elastic acrylic emulsion and stir for 3 minutes; add functional additives and stir for 3 minutes; add the remaining defoamer, stir evenly, and obtain a reflective heat-insulating coating.

[0086] The difference between the preparation method of the hollow acrylic emulsion with a latex particle size of 600 nm and the preparation method of the hollow acrylic emulsion with a latex particle size of 450 nm is that: in step (2), 1 part of emulsifier sodium dodecylbenzene sulfonate (DS-4) is dispersed in 17.55 parts of deionized water, and 22.82 parts of olefin monomer methyl methacrylate (MMA) and 12.29 parts of unsaturated acid methacrylic acid (MAA) are slowly added to the above water under stirring; in step (3), a reaction flask is prepared, 25.25 parts of water are added thereto, and 20% of pre-emulsion (a total of 53.66 parts of pre-emulsion) is added; 4.45 parts of siloxane compound with active groups are added to the reactor at one time; the other steps are the same as the preparation method of the hollow acrylic emulsion with a latex particle size of 450 nm, and a hollow acrylic emulsion with a latex particle size of 600 nm and a ratio of the thickness of the shell layer to the particle size of the hollow microsphere of 20:100 is obtained.

[0087] The difference between the preparation method of the hollow acrylic emulsion with a latex particle diameter of 1000nm and the preparation method of the hollow acrylic emulsion with a latex particle diameter of 450nm is that: in step (2), 1 part of emulsifier sodium dodecylbenzene sulfonate (DS-4) is dispersed in 16.45 parts of deionized water, and 21.39 parts of olefin monomer methyl methacrylate (MMA) and 11.52 parts of unsaturated acid methacrylic acid (MAA) are slowly added to the above water under stirring; in step (3), a reaction flask is prepared, 23.69 parts of water are added thereto, and 20% of pre-emulsion liquid (a total of 50.36 parts of pre-emulsion liquid) is added; 6.67 parts of siloxane compound with active groups are added to the reaction kettle at one time; the other steps are the same as the preparation method of the hollow acrylic emulsion with a latex particle diameter of 450nm, and the hollow acrylic emulsion with a latex particle diameter of 1000nm and a ratio of the thickness of the shell layer to the particle diameter of the hollow microsphere of 20:100 is obtained.

[0088] The difference between the preparation method of the hollow acrylic emulsion with a latex particle size of 1600nm and the preparation method of the hollow acrylic emulsion with a latex particle size of 450nm is that: in step (2), 1 part of an emulsifier sodium dodecylbenzene sulfonate (DS-4) is dispersed in 15.8 parts of deionized water, and 20.53 parts of an olefin monomer methyl methacrylate (MMA) and 11.06 parts of an unsaturated acid methacrylic acid (MAA) are slowly added to the above water under stirring; in step (3), a reaction flask is prepared, 22.75 parts of water are added thereto, and 20% of a pre-emulsion (a total of 48.39 parts of the pre-emulsion) is added; 8.01 parts of a siloxane compound with an active group are added to a reactor at one time; in step (4), 22.61 parts of seed emulsion are added to 33.05 parts of water; an emulsion consisting of 0.46 parts of sodium dodecylbenzene sulfonate (DS-4), 19.7 parts of styrene (ST), 1.32 parts of methyl methacrylate (MMA), 0.04 parts of allyl methacrylate (AMA), 0.13 parts of methacrylic acid (MAA) and 15.68 parts of water and an aqueous solution of 0.07 parts of sodium persulfate and 0.36 parts of water are added dropwise; 0.66 parts of ammonia water are added when the emulsion is added dropwise to 45%, and the rest is the same as the preparation method of the hollow acrylic emulsion with a latex particle diameter of 450 nm, to obtain a hollow acrylic emulsion with a latex particle diameter of 1600 nm and a shell thickness to hollow microsphere particle diameter ratio of 20:100.

[0089] Example 3

[0090] A reflective heat-insulating coating, comprising, by weight, 5 parts of a hollow acrylic emulsion A with a latex particle size of 700 nm, 3 parts of a hollow acrylic emulsion B with a latex particle size of 1100 nm, and 10 parts of a hollow acrylic emulsion C with a latex particle size of 1800 nm. 2 parts, elastic acrylic emulsion 25 parts, filler 26 parts (calcite powder 5 parts, rutile titanium dioxide 20 parts, diatomaceous earth 1 part), non-ionic alkyl polyoxyethylene ether wetting agent 0.4 parts, polyacrylate ammonium salt dispersant 0.6 parts, mineral oil defoamer 0.6 parts, thickener hydroxyethyl cellulose 0.3 parts, fungicide (a mixture of pyrimidine copper zinc and zinc oxide) 0.3 parts, preservative (a mixture of 5-chloro-2-methyl-4-isothiazoline-3-one and 2-methyl-4-isothiazoline-3-one) 0.3 parts, mildewproof agent 2-benzimidazole carbamate methyl ester 0.4 parts, pH adjuster 2-amino-2-methyl-1-propanol 0.1 parts, antifreeze-thaw aid propylene glycol 2 parts, film-forming aid dodecanol ester 0.5 parts, functional aid non-ionic polyurethane leveling agent 2 parts, water 25 parts;

[0091] The latex particles in hollow acrylic emulsion A, hollow acrylic emulsion B and hollow acrylic emulsion C are all hollow microspheres;

[0092] The ratio of the shell thickness to the particle size of the hollow microspheres of the three particle sizes is 20:100.

[0093] A method for preparing a reflective heat-insulating coating comprises the following steps:

[0094] Add water, wetting agent, dispersant and 20% defoamer under stirring at 200 rpm, and stir for 3 minutes; adjust the speed to 400 rpm, add thickener, and stir for 2 minutes; adjust the speed to 1200 rpm, add titanium dioxide and filler, and stir for 15 minutes; adjust the speed to 900 rpm, add film-forming aid, antifreeze agent, bactericidal and mildew-proof preservative, and stir for 3 minutes; then add hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C, and elastic acrylic emulsion and stir for 3 minutes; add functional additives and stir for 3 minutes; add the remaining defoamer, stir evenly, and obtain a reflective heat-insulating coating.

[0095] The difference between the preparation method of the hollow acrylic emulsion with a latex particle size of 700 nm and the preparation method of the hollow acrylic emulsion with a latex particle size of 450 nm is that: in step (2), 1 part of emulsifier sodium dodecylbenzene sulfonate (DS-4) is dispersed in 18.46 parts of deionized water, and 24 parts of olefin monomer methyl methacrylate (MMA) and 12.92 parts of unsaturated acid methacrylic acid (MAA) are slowly added to the above water under stirring; in step (3), a reaction flask is prepared, 26.58 parts of water are added thereto, and 20% of pre-emulsion liquid (a total of 56.38 parts of pre-emulsion liquid) is added; 2.81 parts of siloxane compound with active groups are added to the reactor at one time; the other steps are the same as the preparation method of the hollow acrylic emulsion with a latex particle size of 450 nm, and a hollow acrylic emulsion with a latex particle size of 700 nm and a ratio of the thickness of the shell layer to the particle size of the hollow microsphere of 20:100 is obtained.

[0096] The difference between the preparation method of the hollow acrylic emulsion with a latex particle size of 1100 nm and the preparation method of the hollow acrylic emulsion with a latex particle size of 450 nm is that: in step (2), 1 part of an emulsifier sodium dodecylbenzene sulfonate (DS-4) is dispersed in 16.8 parts of deionized water, 20.58 parts of an olefin monomer methyl methacrylate (MMA) and 9.97 parts of an unsaturated acid methacrylic acid (MAA) are slowly added to the above water under stirring. In step (3), a reaction flask is prepared, 22.75 parts of water are added thereto, and 20% of the pre-emulsion (a total of 48.35 parts of the pre-emulsion) is added; in step (4), when the emulsion is added to 45%, 0.86 parts of ammonia water are added, and the rest is the same as the preparation method of the hollow acrylic emulsion with a latex particle size of 450nm, to obtain a hollow acrylic emulsion with a latex particle size of 1100nm and a shell thickness to hollow microsphere particle size ratio of 20:100.

[0097] The difference between the preparation method of the hollow acrylic emulsion with a latex particle size of 1800 nm and the preparation method of the hollow acrylic emulsion with a latex particle size of 450 nm is that in step (2), 1.07 parts of an emulsifier sodium dodecylbenzene sulfonate (DS-4) are dispersed in 17.55 parts of deionized water, 22.82 parts of an olefin monomer methyl methacrylate (MMA) and 12.29 parts of an unsaturated acid methacrylic acid (MAA) are slowly added under stirring. In the above water; in step (3), a reaction flask is prepared, 25.28 parts of water are added thereto, and 20% of the pre-emulsion (a total of 53.73 parts of the pre-emulsion) is added; 4.45 parts of the siloxane compound with an active group are added to the reactor at one time, and the rest is the same as the preparation method of the hollow acrylic emulsion with a latex particle size of 450nm, to obtain a hollow acrylic emulsion with a latex particle size of 1800nm ​​and a shell thickness to hollow microsphere particle size ratio of 20:100.

[0098] Comparative Example 1

[0099] The only difference between Comparative Example 1 and Example 1 is that Comparative Example 1 uses an equal amount of water to replace hollow acrylic emulsion A, hollow acrylic emulsion B, and hollow acrylic emulsion C, that is, it does not contain hollow acrylic emulsion, and the rest is the same as Example 1.

[0100] Comparative Example 2

[0101] The only difference between Comparative Example 2 and Example 1 is that Comparative Example 2 uses hollow polystyrene microspheres (ZPH-104 of Shanghai Zhenzhun Biotechnology Co., Ltd.) used in the prior art with publication number CN106867348A to replace the hollow acrylic emulsion A, hollow acrylic emulsion B, and hollow acrylic emulsion C in Example 1 in equal amounts, and the rest is the same as Example 1.

[0102] Comparative Example 3

[0103] The only difference between Comparative Example 3 and Example 1 is that the ratio of the shell thickness of the hollow microspheres in Comparative Example 3 to the particle size of the hollow microspheres is 5:100, that is, the shell thickness of the hollow microspheres is reduced, and the rest is the same as Example 1.

[0104] Comparative Example 4

[0105] The only difference between Comparative Example 4 and Example 1 is that the ratio of the shell thickness of the hollow microspheres in Comparative Example 4 to the particle size of the hollow microspheres is 50:100, that is, the shell thickness of the hollow microspheres is increased, and the rest is the same as Example 1.

[0106] Comparative Example 5

[0107] The only difference between Comparative Example 5 and Example 1 is that Comparative Example 5 uses an equal amount of hollow acrylic emulsion B with a latex particle size of 900 nm to replace the hollow acrylic emulsion A with a particle size of 450 nm, that is, it does not contain hollow acrylic emulsion A, and the rest is the same as Example 1.

[0108] Comparative Example 6

[0109] The only difference between Comparative Example 6 and Example 1 is that Comparative Example 6 uses an equal amount of hollow acrylic emulsion A with a latex particle size of 450nm to replace an equal amount of hollow acrylic emulsion B with a latex particle size of 900nm, that is, it does not contain hollow acrylic emulsion B, and the rest is the same as Example 1.

[0110] Comparative Example 7

[0111] The only difference between Comparative Example 7 and Example 1 is that Comparative Example 7 uses an equal amount of hollow acrylic emulsion B with a latex particle size of 900 nm to replace the hollow acrylic emulsion C with a latex particle size of 1700 nm, that is, it does not contain hollow acrylic emulsion C, and the rest is the same as Example 1.

[0112] Performance Testing

[0113] The coatings prepared in Examples 1-3 and Comparative Examples 1-7 were coated on aluminum plates and then cured for 168 hours under standard conditions to obtain a coating with a thickness of 0.3 mm. The performance test was then performed. The specific test items and test methods are as follows:

[0114] Test of thermal insulation performance of coating film: Prepare a simple device for measuring thermal insulation performance of coating film: The heating light source is a 275W heating lamp, which is 25cm away from the coating film. Except for the position where the test sample is placed at the top of the test chamber, the rest of the test chamber can be regarded as insulated. The thermometer shows the temperature in the test chamber (polystyrene foam box). The schematic diagram of the thermal insulation performance test device is as follows: Figure 1 , simulate the indoor temperature conditions corresponding to different exterior wall coatings under sunlight. During the experiment, the room temperature was controlled at 25°C, which is equivalent to the constant ambient temperature around the building. The sample plate to be tested is equivalent to the exterior wall coated with thermal insulation paint. The temperature test of the test chamber simulating the indoor temperature change was carried out. During the experiment, the test chamber was sealed with the sample plate to be tested, and the heating lamp was turned on until the temperature stabilized and unchanged. The final temperature in the test chamber was recorded for comparison of thermal insulation performance.

[0115] Solar reflectance: Tested in accordance with GB / T 25261-2018;

[0116] Near infrared reflectance: tested in accordance with GB / T 25261-2018;

[0117] Hemispherical emissivity: tested in accordance with GB / T 25261-2018;

[0118] Stain resistance: Tested in accordance with GB / T 9755-2014;

[0119] Tensile strength: Tested in accordance with JG / T172-2014;

[0120] Elongation at break (under standard conditions): Tested in accordance with JG / T172-2014;

[0121] Artificial aging resistance: Tested in accordance with JG / T172-2014.

[0122] The performance test results of the coatings prepared in Examples 1-3 and Comparative Examples 1-7 are shown in Table 1.

[0123] Table 1: Performance test results of coatings prepared in Examples 1-3 and Comparative Examples 1-7

[0124]

[0125] It can be seen from Table 1 that the reflective heat-insulating coating prepared by the present invention has good reflective heat-insulating effect, the lowest temperature in the test room is 30.2° C., and it has good mechanical properties, stain resistance, and artificial aging resistance.

[0126] Comparative Example 1 does not contain hollow acrylic emulsion, so the reflective heat insulation effect, mechanical properties, stain resistance, and artificial aging resistance of the coating prepared in Comparative Example 1 are significantly worse than those in Example 1, and the final temperature in the test room is 11.8°C higher than that in Example 1.

[0127] Comparative Example 2 uses hollow polystyrene microspheres, so that the reflective heat insulation effect, mechanical properties, stain resistance, and artificial aging resistance of the coating prepared in Comparative Example 2 are significantly worse than those in Example 1, and the final temperature in the test room is 7.7°C higher than that in Example 1.

[0128] The shell thickness in Comparative Example 3 is relatively thin, while the shell thickness in Comparative Example 4 is relatively thick, so that the reflective heat insulation effect, mechanical properties, and stain resistance of the coatings prepared in Comparative Examples 3 and 4 are all inferior to those in Example 1, and the artificial aging resistance of Comparative Example 3 is also poor. The final temperatures in the test chambers of Comparative Examples 3-4 are 9.9°C and 7.2°C higher than those in Example 1, respectively.

[0129] Comparative Example 5 does not contain hollow acrylic emulsion A, Comparative Example 6 does not contain hollow acrylic emulsion B, and Comparative Example 7 does not contain hollow acrylic emulsion C, so that Comparative Examples 5-7 cannot achieve the compounding of hollow microspheres of three particle sizes, and thus their reflective heat insulation effects, mechanical properties, and stain resistance are all worse than those of Example 1. The final temperatures in the test rooms of Comparative Examples 5-7 are 6.7°C, 6.1°C, and 7.3°C higher than those of Example 1, respectively.

[0130] In summary, the present invention uses three hollow acrylic emulsions with different particle size ranges to compound, and hollow microspheres of different sizes can play a synergistic role, and the shell layer of the hollow microsphere and the particle size of the hollow microsphere have a specific size relationship, which is beneficial to the reflective heat insulation performance, mechanical properties, stain resistance, and weather resistance of the coating. The solar reflectance of the reflective heat insulation coating of the present invention is as high as 0.88, the near-infrared reflectance is as high as 0.9, and the hemispherical emissivity is as high as 0.93. Compared with Comparative Example 1, the final temperature in the measuring room can be reduced by 11.8°C, the tensile strength is as high as 2.89MPa, and the elongation at break is as high as 507%, which has great application potential in the field of building walls.

[0131] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A coating, characterized in that: Including hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C, elastic acrylic emulsion; The particle sizes of the latex particles in the hollow acrylic emulsion A, the hollow acrylic emulsion B, and the hollow acrylic emulsion C are 450-750 nm, 900-1300 nm, and 1400-1800 nm, respectively; The latex particles in the hollow acrylic emulsion A, the hollow acrylic emulsion B and the hollow acrylic emulsion C are all hollow microspheres; the hollow microspheres include a shell layer; the ratio of the thickness of the shell layer to the particle size of the hollow microspheres is (9-33):

100.

2. The coating according to claim 1, characterized in that In the coating, the hollow acrylic emulsion A, the hollow acrylic emulsion B and the hollow acrylic emulsion C are all 1.8-11 parts by weight.

3. The coating according to claim 1, characterized in that The solid content of the elastic acrylic emulsion is 45-60%.

4. The coating according to claim 1, characterized in that The particle size of the latex particles in the elastic acrylic emulsion is 90-330 nm.

5. The coating according to any one of claims 1 to 4, characterized in that The coating also includes at least one of fillers, wetting agents, dispersants, defoamers, thickeners, bactericides, preservatives, mildew inhibitors, pH regulators, antifreeze-thaw aids, film-forming aids, functional aids, and water.

6. The coating according to claim 5, characterized in that The coating comprises hollow acrylic emulsion A, hollow acrylic emulsion B, hollow acrylic emulsion C, elastic acrylic emulsion, filler, wetting agent, dispersant, defoamer, thickener, bactericide, preservative, mildewproof agent, pH adjuster, antifreeze-thaw aid, film-forming aid, functional aid, and water; and by weight, the coating comprises hollow acrylic emulsion A 1.8-11 parts, hollow acrylic emulsion B 1.8-11 parts, hollow acrylic emulsion C 1.8-11 parts, elastic acrylic emulsion 18-33 parts, filler 23-40 parts, wetting agent 0.27-0.55 parts, dispersant 0.55-1.2 parts, defoaming agent 0.55-1.1 parts, thickener 0.27-0.55 parts, bactericide 0.1-0.33 parts, preservative 0.18-0.33 parts, mildewproof agent 0.18-0.44 parts, pH adjuster 0.1-0.22 parts, antifreeze-thaw aid 0.9-2.2 parts, film-forming aid 0.45-1.1 parts, functional additive 0.9-2.2 parts, water 20-25 parts.

7. The coating according to claim 5, characterized in that The filler includes at least one of calcite powder, diatomaceous earth and titanium dioxide; And / or, the wetting agent includes at least one of anionic wetting agents and nonionic wetting agents; and / or, the dispersant comprises at least one of polycarboxylates, polyacrylates, and carboxylic acid copolymer salts; And / or, the defoamer includes at least one of polymer composite mineral oil, metal soap defoamer, and silicone defoamer; and / or, the thickener comprises hydroxyethyl cellulose; And / or, the fungicide comprises at least one of pyrimidine copper zinc thiocarbamide and zinc oxide; And / or, the preservative includes at least one of 5-chloro-2-methyl-4-isothiazoline-3-one and 2-methyl-4-isothiazoline-3-one; and / or, the mildew inhibitor comprises methyl 2-benzimidazolecarbamate; and / or, the pH adjuster comprises 2-amino-2-methyl-1-propanol; And / or, the antifreeze-thaw aid includes propylene glycol; and / or, the film-forming aid comprises dodecyl alcohol ester; And / or, the functional additive includes a non-ionic polyurethane leveling modifier.

8. The method for preparing the coating according to any one of claims 1 to 7, characterized in that: The following steps are involved: The coating is prepared by mixing various raw material components.

9. The preparation method according to claim 8, characterized in that: The following steps are involved: (1) dissolving the dispersant and wetting agent in water, adding the thickener, and then adding the pH adjuster and filler, and mixing to obtain a premix; (2) Mixing the remaining components with the premix obtained in step (1) to prepare the coating.

10. Use of the coating according to any one of claims 1 to 7 in the field of construction.

Citation Information

Patent Citations

  • Hollow hiding coating as well as preparation method and application thereof

    CN102775861A

  • Coating

    CN104725970A

  • Preparation method of hollow micro-sphere emulsion with covering power for water-based cowboy adhesive cement

    CN107056977A

  • Heat insulation additive for building coating and preparation method

    CN109161246A

  • High-temperature-resistant high-water-resistance heat-insulation reflective coating and preparation method thereof

    CN111534180A