Interior wall latex paint capable of releasing negative oxygen ions and preparation method thereof
By modifying tourmaline with conductive polymers and nano activated carbon, the negative oxygen ion release and formaldehyde purification capabilities of latex paint are improved, and the problem of traditional latex paint is solved, and a healthy and environmentally friendly interior wall latex paint is achieved.
Patent Information
- Application Number
- CN202411361045.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-27
AI Technical Summary
Traditional latex paint releases harmful gases, such as formaldehyde, during drying and curing, resulting in indoor air quality problems. In the prior art, there is a risk of radiocontamination when mixing tourmaline with rare earths to improve the efficiency of negative oxygen ion release.
Wet grinding and modification of conductive polymers, nanoactivated carbon and tourmaline powder is used to improve the negative oxygen ion release capacity of tourmaline, and the formaldehyde purification efficiency of latex paint is enhanced.
It significantly improves the negative oxygen ion release performance and formaldehyde purification efficiency of latex paint, realizes a healthy and environmentally friendly interior wall latex paint, and avoids the risk of radiation pollution.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of latex paint, in particular to an interior wall latex paint capable of releasing negative oxygen ions and a preparation method thereof. Background Art
[0002] Traditional latex paint releases harmful gases such as formaldehyde during the drying and curing process, which seriously affects the indoor air quality and poses potential harm to the health of residents. In order to solve the problem of traditional latex paint releasing harmful substances, some studies have proposed integrating tourmaline (also known as tourmaline ore) into latex paint, taking advantage of its ability to release negative oxygen ions, hoping to achieve the effect of purifying the air and decomposing harmful gases by generating negative oxygen ions.
[0003] However, the negative oxygen ion release efficiency of tourmaline in traditional latex paint is relatively low, resulting in unsatisfactory purification effect of harmful substances such as formaldehyde in the air. For this reason, there is a technology that mixes tourmaline with rare earth to greatly improve the negative oxygen ion release capacity, but rare earth is generally radioactive and may cause radioactive pollution when used indoors. Summary of the invention
[0004] The invention provides an interior wall latex paint capable of releasing negative oxygen ions and a preparation method thereof, so as to solve the technical problem that the traditional interior wall latex paint has poor purification ability for toxic gases such as formaldehyde.
[0005] In order to solve the above technical problems, in a first aspect, the present invention provides an interior wall latex paint capable of releasing negative oxygen ions, comprising the following raw material components in parts by weight:
[0006] 30 to 50 parts of water-based acrylic emulsion;
[0007] 20 to 30 parts of titanium dioxide;
[0008] 5 to 10 parts of tourmaline powder;
[0009] 1 to 3 parts of conductive polymer;
[0010] 1 to 2 parts of nano activated carbon;
[0011] 0.1 to 20 parts of additives;
[0012] 10 to 20 parts of filler;
[0013] 50 to 70 parts of water.
[0014] In some embodiments, the mass ratio of the conductive polymer, nano-activated carbon and tourmaline powder is 1:0.8:4.5.
[0015] In some embodiments, the conductive polymer is one or both of conductive polyaniline and polypyrrole.
[0016] In some embodiments, the conductive polyaniline is acid-doped polyaniline, or the polypyrrole is anion-doped polypyrrole.
[0017] Acid-doped polyaniline is a polyaniline obtained by doping aniline with proton acid during polymerization using hydrochloric acid, sulfuric acid, perchloric acid, dodecylsulfonic acid, dodecylbenzenesulfonic acid, camphorsulfonic acid, naphthalenesulfonic acid or 2,4-dinitronaphthol-7-sulfonic acid as doping agents. During the doping process of polyaniline, the number of its electrons does not change, but the doped proton acid decomposes to produce H+ and anions (such as Cl-, sulfate, phosphate, etc.) that enter the main chain and combine with the N atoms in the amine and imine groups to form polar and dipole delocalized to the P bond of the entire molecular chain, thereby forming a P-type doped polyaniline chain.
[0018] Anion-doped polypyrrole is obtained by doping halogen ions (such as chloride ions, bromide ions or iodide ions, etc.), organic anions (such as benzenesulfonic acid or p-toluenesulfonic acid, etc.) or inorganic anions (such as sulfate or phosphate, etc.) into polypyrrole molecules. During the doping process of polypyrrole, anions enter the molecular structure of polypyrrole, changing its original electron distribution and making it exhibit electronegativity.
[0019] In some embodiments, the auxiliary agent includes one or more of a film-forming auxiliary agent, a thickener, a dispersant, a leveling agent, a defoaming agent, a preservative and a pH adjuster.
[0020] The film-forming aid includes one or more of alcohol ester dodecahydrate, diethylene glycol butyl ether, dipropylene glycol methyl ether, ethylene glycol monobutyl ether, propylene glycol methyl ether acetate and propylene glycol monomethyl ether. The thickener includes one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, sodium carboxymethyl cellulose, fatty alcohol polyoxyethylene ether, alkylphenol polyoxyethylene ether and polyoxyethylene-polyoxypropylene copolymer.
[0021] In some embodiments, the filler includes one or more of calcium carbonate, kaolin, talc and diatomaceous earth.
[0022] In a second aspect, the present invention also provides a method for preparing an interior wall latex paint capable of releasing negative oxygen ions, comprising the following steps:
[0023] Step 1, adding conductive polymer and nano activated carbon to tourmaline powder for wet grinding modification to obtain a modified composite material;
[0024] Step 2, mixing titanium dioxide, additives, fillers and water, stirring at a stirring speed of 1800 rpm to 3000 rpm for 40 min to 60 min to obtain a mixture A;
[0025] Step 3, mixing the modified composite material with mixture A, stirring at a stirring speed of 300 rpm to 600 rpm for 30 min to 45 min to obtain mixture B;
[0026] Step 4: Mix the mixture B with the aqueous acrylic emulsion, and stir at a stirring speed of 500 rpm to 1000 rpm for 1 h to 3 h to obtain a latex paint.
[0027] In some embodiments, the step one comprises:
[0028] The conductive polymer, nano-activated carbon and tourmaline powder are mixed with water to form a slurry I with a concentration of 60% to 70%;
[0029] Add slurry I and grinding media to a low-speed stirring mill for cyclic grinding for 5 h to 8 h to obtain slurry II;
[0030] The slurry II and the grinding medium are added to a high-speed stirring mill for cyclic grinding for 3 hours to 5 hours, filtered and dried to obtain a modified composite material, wherein the grinding medium includes zirconium oxide or ceramic.
[0031] In some of the embodiments, the particle size of the tourmaline powder of the slurry II is 2 μm to 4 μm, and the particle size of the tourmaline powder of the modified composite material is 0.5 μm to 1.8 μm.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The present invention uses conductive polymer and nano activated carbon to perform wet grinding modification on tourmaline, utilizes the electromagnetic characteristics of the conductive polymer to activate the activity of the tourmaline, improves the ability of the tourmaline to release negative oxygen ions, utilizes the excellent adsorption capacity of the nano activated carbon to adsorb free formaldehyde and other toxic gases in the air, and improves the efficiency of purifying formaldehyde with negative oxygen ions. Therefore, a conductive polymer-nano activated carbon-tourmaline composite material is used as a negative oxygen ion releaser to improve the formaldehyde purification ability of latex paint, thereby achieving healthy and environmentally friendly interior wall latex paint. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0035] As used herein, the term "prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0036] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.
[0037] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention have no restrictions on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number is obviously intended to be in the singular form.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0039] Example 1
[0040] An interior wall latex paint capable of releasing negative oxygen ions comprises the following raw material components in parts by weight:
[0041] 30 parts of water-based pure acrylic emulsion;
[0042] 20 parts of titanium dioxide;
[0043] Tourmaline powder 5.6 parts;
[0044] 1.2 parts of hydrochloric acid doped polyaniline;
[0045] 1 part of nano activated carbon;
[0046] Alcohol ester 12 0.3 parts;
[0047] 0.2 parts of hydroxyethyl cellulose;
[0048] 5 parts of talcum powder;
[0049] 5 parts of light calcium carbonate;
[0050] 50 parts water;
[0051] The preparation method comprises the following steps:
[0052] Step 1: Mix the conductive polymer, nano-activated carbon and tourmaline powder with water to a slurry I with a concentration of 60%; add the slurry I and the grinding medium to a low-speed stirred mill for cyclic grinding for 5 hours to 8 hours until the particle size of the tourmaline powder is within 2 μm to 4 μm, to obtain slurry II; add the slurry II and the grinding medium to a high-speed stirred mill for cyclic grinding for 3 hours to 5 hours until the particle size of the tourmaline powder is 1.8 μm, filter and dry to obtain a modified composite material;
[0053] Step 2, titanium dioxide, additives, fillers and water are mixed, and stirred at a stirring speed of 1800 rpm for 60 minutes to obtain a mixture A;
[0054] Step 3, mixing the modified composite material with mixture A, stirring at a stirring speed of 300 rpm for 45 minutes to obtain mixture B;
[0055] Step 4: Mix the mixture B with the aqueous acrylic emulsion, and stir at a stirring speed of 500 rpm for 3 hours to obtain a latex paint.
[0056] Example 2
[0057] An interior wall latex paint capable of releasing negative oxygen ions comprises the following raw material components in parts by weight:
[0058] 50 parts of water-based pure acrylic emulsion;
[0059] 30 parts of titanium dioxide;
[0060] Tourmaline powder 10 parts;
[0061] Chloride ion doped polypyrrole 2.2 parts;
[0062] 1.8 parts of nano activated carbon;
[0063] 1.5 parts of alcohol ester 12;
[0064] 1 part of hydroxyethyl cellulose;
[0065] 10 parts of heavy calcium carbonate;
[0066] 10 parts of kaolin;
[0067] 70 parts of water;
[0068] The preparation method comprises the following steps:
[0069] Step 1: Mix the conductive polymer, nano-activated carbon and tourmaline powder with water to a slurry I with a concentration of 70%; add the slurry I and the grinding medium to a low-speed stirred mill for cyclic grinding for 5 hours to 8 hours until the particle size of the tourmaline powder is within 2 μm to 4 μm, to obtain slurry II; add the slurry II and the grinding medium to a high-speed stirred mill for cyclic grinding for 3 hours to 5 hours until the particle size of the tourmaline powder is 0.5 μm, filter and dry to obtain a modified composite material;
[0070] Step 2, mixing titanium dioxide, additives, fillers and water, stirring at a stirring speed of 3000 rpm for 40 minutes to obtain a mixture A;
[0071] Step 3, mixing the modified composite material with mixture A, stirring at a stirring speed of 600 rpm for 30 min to obtain mixture B;
[0072] Step 4: Mix the mixture B with the aqueous acrylic emulsion, and stir at a stirring speed of 1000 rpm for 3 hours to obtain a latex paint.
[0073] Example 3
[0074] An interior wall latex paint capable of releasing negative oxygen ions comprises the following raw material components in parts by weight:
[0075] 40 parts of water-based pure acrylic emulsion;
[0076] 25 parts of titanium dioxide;
[0077] 9 parts of tourmaline powder;
[0078] 2 parts of conductive polymer;
[0079] 1.6 parts of nano activated carbon;
[0080] Alcohol ester 12 1 part;
[0081] 0.8 parts of hydroxyethyl cellulose;
[0082] 7 parts of talcum powder;
[0083] 8 parts of kaolin;
[0084] 60 parts of water;
[0085] The preparation method comprises the following steps:
[0086] Step 1: Mix the conductive polymer, nano-activated carbon and tourmaline powder with water to a slurry I with a concentration of 65%; add the slurry I and the grinding medium to a low-speed stirred mill for cyclic grinding for 5 hours to 8 hours until the particle size of the tourmaline powder is within 2 μm to 4 μm, to obtain slurry II; add the slurry II and the grinding medium to a high-speed stirred mill for cyclic grinding for 3 hours to 5 hours until the particle size of the tourmaline powder is 1 μm, filter and dry to obtain a modified composite material;
[0087] Step 2, mixing titanium dioxide, additives, fillers and water, and stirring at a stirring speed of 2500 rpm for 50 minutes to obtain a mixture A;
[0088] Step 3, mixing the modified composite material with mixture A, stirring at a stirring speed of 500 rpm for 35 minutes to obtain mixture B;
[0089] Step 4: Mix the mixture B with the aqueous acrylic emulsion, and stir at a stirring speed of 600 rpm for 2.5 hours to obtain a latex paint.
[0090] Comparative Example 1
[0091] The difference from Example 3 is that no conductive polymer is added in Comparative Example 1;
[0092] Comparative Example 2
[0093] The difference from Example 3 is that no nano activated carbon is added in Comparative Example 2;
[0094] Comparative Example 3
[0095] The difference from Example 3 is that no conductive polymer and nano-activated carbon are added in Comparative Example 3;
[0096] Comparative Example 4
[0097] The difference from Example 3 is that the particle size of the tourmaline powder of the modified composite material of Comparative Example 4 is 0.01 μm.
[0098] According to the construction industry standard JC / T1016-2006 "Test Method for Negative Ion Generation of Materials", the negative oxygen ion release performance of the interior wall latex paints of Examples 1 to 3 and Comparative Examples 1 to 4 was tested. According to JC / T1074-2008 "Purification Performance of Indoor Air Purification Function Coating Materials", the formaldehyde purification efficiency of the above interior wall latex paints was tested.
[0099] Sample <![CDATA[Negative oxygen ion release amount (pcs / cm 3 )]]> Formaldehyde purification efficiency (%) Example 1 5360 >99 Example 2 5770 >99 Example 3 5910 >99 Comparative Example 1 1980 86 Comparative Example 2 3340 88 Comparative Example 3 720 77 Comparative Example 4 5240 99
[0100] From the test results in the above table, it can be seen that the negative oxygen ion release of the interior wall latex paint of Examples 1 to 3 is 5300 / cm 3As shown above, the formaldehyde purification efficiency is greater than 99%. It is obvious that the addition of conductive polymer-nano activated carbon-tourmaline modified composite materials can make the interior wall latex paint have excellent negative oxygen ion release performance. Comparative Example 1 does not add conductive polymer, and its negative oxygen ion release is significantly reduced. Comparative Example 2 does not add nano activated carbon, and its negative oxygen ion release is more significantly reduced. However, the formaldehyde purification efficiency of Comparative Examples 1 and 2 is equivalent. It may be that Comparative Example 2 does not add nano activated carbon, which makes it unable to adsorb free formaldehyde gas in the air for purification, while Comparative Example 1 does not add conductive polymer, which may cause it to reach the purification upper limit of negative oxygen ion concentration; Comparative Example 3 does not add conductive polymer and nano activated carbon, and its negative oxygen ion release and formaldehyde purification efficiency are significantly reduced; Comparative Example 4 has a reduced negative oxygen ion release, which may be due to the smaller tourmaline particle size, which weakens its spontaneous polarization performance, thereby weakening its negative oxygen ion release performance.
[0101] The present invention uses conductive polymer and nano activated carbon to wet-grind tourmaline for modification, utilizes the electromagnetic characteristics of the conductive polymer to improve the ability of tourmaline to release negative oxygen ions, utilizes the excellent adsorption capacity of the nano activated carbon to adsorb free formaldehyde and other toxic gases in the air, and improves the efficiency of purifying formaldehyde with negative oxygen ions. Therefore, a conductive polymer-nano activated carbon-tourmaline composite material is used as a negative oxygen ion releaser to improve the formaldehyde purification ability of latex paint, thereby achieving healthy and environmentally friendly interior wall latex paint.
[0102] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0103] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. An interior wall latex paint capable of releasing negative oxygen ions, characterized in that: The raw material components include the following parts by weight: 30 to 50 parts of water-based acrylic emulsion; 20 to 30 parts of titanium dioxide; 5 to 10 parts of tourmaline powder; 1 to 3 parts of conductive polymer; 1 to 2 parts of nano activated carbon; 0.1 to 20 parts of additives; 10 to 20 parts of filler; 50 to 70 parts of water.
2. The interior wall latex paint capable of releasing negative oxygen ions as claimed in claim 1, characterized in that: The mass ratio of the conductive polymer, nano-activated carbon and tourmaline powder is 1:0.8:4.
5.
3. The interior wall latex paint capable of releasing negative oxygen ions as claimed in claim 1 or 2, characterized in that: The conductive polymer is one or both of conductive polyaniline and polypyrrole.
4. The interior wall latex paint capable of releasing negative oxygen ions as claimed in claim 3, characterized in that: The conductive polyaniline is acid-doped polyaniline, or the polypyrrole is anion-doped polypyrrole.
5. The interior wall latex paint capable of releasing negative oxygen ions as claimed in claim 1, characterized in that: The auxiliary agent includes one or more of a film-forming auxiliary agent, a thickener, a dispersant, a leveling agent, a defoaming agent, a preservative and a pH regulator.
6. The interior wall latex paint capable of releasing negative oxygen ions as claimed in claim 1, characterized in that: The filler includes one or more of calcium carbonate, kaolin, talc and diatomaceous earth.
7. A method for preparing an interior wall latex paint capable of releasing negative oxygen ions as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1, adding conductive polymer and nano activated carbon to tourmaline powder for wet grinding modification to obtain a modified composite material; Step 2, mixing titanium dioxide, additives, fillers and water, stirring at a stirring speed of 1800 rpm to 3000 rpm for 40 min to 60 min to obtain a mixture A; Step 3, mixing the modified composite material with mixture A, stirring at a stirring speed of 300 rpm to 600 rpm for 30 min to 45 min to obtain mixture B; Step 4: Mix the mixture B with the aqueous acrylic emulsion, and stir at a stirring speed of 500 rpm to 1000 rpm for 1 h to 3 h to obtain a latex paint.
8. The preparation method according to claim 7, characterized in that: The step one comprises: The conductive polymer, nano-activated carbon and tourmaline powder are mixed with water to form a slurry I with a concentration of 60% to 70%; Add slurry I and grinding media to a low-speed stirring mill for cyclic grinding for 5 h to 8 h to obtain slurry II; The slurry II and the grinding medium are added to a high-speed stirring mill for cyclic grinding for 3 hours to 5 hours, and then filtered and dried to obtain a modified composite material.
9. The preparation method according to claim 8, characterized in that: The particle size of the tourmaline powder of the slurry II is 2 μm to 4 μm, and the particle size of the tourmaline powder of the modified composite material is 0.5 μm to 1.8 μm.
Citation Information
Patent Citations
Architectural interior anion waterproof putty powder and preparation method thereof
CN101225261A
Tourmalineline environmental protection emulsion paint and preparation method thereof
CN101781501A
Antistatic antibacterial odor removal coating adhesive for luggage fabric and preparation and application thereof
CN102877305A
Novel environment-friendly coating material and preparation method thereof
CN107118648A
Environment-friendly formaldehyde-removing wall decoration material and preparation method thereof