Deep-sea pressure-resistant wear-resistant anticorrosive paint as well as preparation method and application thereof
By combining the sulfonated polyaniline-modified graphite carbon nitride with the Magnolol-based tetrafunctional epoxy resin, the corrosion and wear of marine steel structures in deep-sea environments is solved, and high adhesion and wear resistance are achieved and corrosion-resistant coatings meet the protection needs of high pressure and high wear in the deep sea.
Patent Information
- Application Number
- CN202411128989.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Marine steel structures are susceptible to electrochemical corrosion and erosion wear in marine environments. The existing epoxy resin coatings have high brittleness and poor impact and friction wear performance in high cross-linking density, making it difficult to meet the high pressure and high wear of deep-sea. Protection needs.
The graphite carbon nitride is modified by sulfonated polyaniline and combined with the Magnolol-based tetrafunctional epoxy resin to form a coating with high density and hardness, and a body-shaped intersection is formed by a polyetheramine curing agent. The structure increases the adhesion and wear resistance of the coating.
The prepared deep-sea pressure-resistant and wear-resistant anti-corrosion coating has excellent adhesion, wear resistance and erosion resistance. It can maintain protective effect for more than 60 days under the pressure of 6000 meters of deep sea water, and it has shown super-sea superspectrum tests. Long wear resistance.
Smart Images

Figure CN118931315A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings and metal protection, and specifically relates to a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating and a preparation method and application thereof. Background Art
[0002] With the development and utilization of marine resources, offshore equipment has been widely used in marine engineering. However, when offshore steel structures are in service in harsh marine environments, they will be subjected to electrochemical corrosion and erosion wear due to the impact of seawater, oxygen and solid particles in the splash zone. Offshore steel structures will deform and break after being impacted, making it easier for corrosive media to corrode the metal substrate. Therefore, in order to increase the service life of offshore equipment, spraying protective coatings is usually used for protection. The sprayed protective coatings should have the following characteristics in the process of resisting erosion, wear and corrosion: (1) Strong adhesion. The strong adhesion between the coating and the substrate can ensure that the coating will not fall off and fail during the erosion process; (2) Friction and wear resistance. The coating will produce friction and wear during the impact of seawater. Therefore, the coating has excellent friction and wear resistance, which can greatly improve the protective effect of the coating; (3) Excellent barrier properties. Seawater and mud will carry a large amount of corrosive media during the impact of the coating. The coating has excellent barrier properties, which can effectively inhibit the penetration of corrosive media into the coating and improve the protective effect of the protective substrate.
[0003] Epoxy resin is preferred as the main film-forming substance for anti-erosion coatings in marine environments, mainly because the epoxy resin molecular structure contains active epoxy groups, which can undergo cross-linking reactions with various types of curing agents to form a polymer with a multi-dimensional network structure. Epoxy coatings have the following advantages: ① strong adhesion, excellent adhesion to various substrates, and low curing shrinkage; ② excellent chemical resistance, especially alkali resistance; ③ good compatibility, can be miscible with various resins and additives, and the filler has good dispersion in epoxy resin; ④ the prepared coating is hard and has a certain toughness. At the same time, the relative molecular mass of epoxy resin is not high, which is conducive to the preparation of solvent-free coatings. However, pure epoxy coatings are brittle due to their high cross-linking density, and have poor impact resistance and friction and wear properties. Adding functional fillers is the most direct and effective way to improve the impact resistance and friction and wear properties of epoxy coatings.
[0004] Graphitic carbon nitride (g-C3N4) is a covalent compound with a hardness comparable to that of diamond. It is easy to manufacture, wear-resistant, non-toxic, and has strong physical and chemical stability. It is a two-dimensional material with good electron transport properties, which shows that g-C3N4 has great potential in the field of corrosion protection. However, g-C3N4 itself also has defects, such as small specific surface area and easy agglomeration. Summary of the invention
[0005] The object of the present invention is to provide a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating and a preparation method thereof. The present invention uses sulfonated polyaniline (SPANi) to modify graphite carbon nitride (g-C3N4) to obtain graphite carbon nitride modified with sulfonated polyaniline g-C3N4@SPANi, and adds it to epoxy resin as a functional wear-resistant and anti-corrosion filler to prepare a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating. In addition, the magnolol-based tetrafunctional epoxy resin prepared by the deacidification reaction of magnolol and epichlorohydrin has a large number of epoxy groups, and can form a body-shaped cross-linked structure after reacting with a polyetheramine curing agent, thereby improving the compactness of the paint film, and the paint film has strong adhesion after curing, good deep-sea high-pressure resistance, and high hardness. The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating provided by the present invention has a salt spray resistance of ≥4000h, a wear resistance of ≤30mg (GB / T 1768, 1000g / 500r), and a deep-sea 6000-meter seawater pressure resistance of ≥60d.
[0006] Another object of the present invention is to provide an application of a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating for use in deep-sea engineering construction to improve long-term erosion resistance and corrosion resistance.
[0007] The specific technical solutions of the present invention are as follows:
[0008] The present invention provides a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating, the raw materials of which include sulfonated polyaniline-modified graphite carbon nitride;
[0009] The preparation method of the sulfonated polyaniline modified graphite carbon nitride is:
[0010] After aniline, o-aminobenzenesulfonic acid and graphite carbon nitride are uniformly mixed, hydrochloric acid solution is added under ice bath conditions, and after stirring, a catalyst is added to react to obtain sulfonated polyaniline modified graphite carbon nitride.
[0011] In the preparation method of sulfonated polyaniline modified graphite carbon nitride, the mass ratio of aniline, o-aminobenzenesulfonic acid and graphite carbon nitride is 1-2:1-2:2-3; the usage ratio of the total mass of aniline, o-aminobenzenesulfonic acid and graphite carbon nitride to the volume of hydrochloric acid solution is 2-3:1 g / mL, and the solubility of the hydrochloric acid solution is 1-1.5 mol / L; the stirring time is 30-60 min; the reaction time is 30-50 h under ice bath conditions at 0-5° C.; the amount of the catalyst is 0.5 / 100-1 / 100 of the total mass of aniline, o-aminobenzenesulfonic acid and graphite carbon nitride; the catalyst is ammonium persulfate; after the reaction is completed, the reaction is washed with deionized water and vacuum filtered to obtain the sulfonated polyaniline modified graphite carbon nitride.
[0012] The raw materials of the deep-sea pressure-resistant, wear-resistant and anti-corrosion coating also include modified epoxy resin;
[0013] The modified epoxy resin is a magnolol-based tetrafunctional epoxy resin;
[0014] The preparation method of the modified epoxy resin is:
[0015] The magnolia phenol and epichlorohydrin are uniformly mixed, a catalyst is added, a strong alkaline solution is dropped under heating conditions, stirred for reaction, and vacuum filtered to obtain magnolia phenol-based difunctional epoxy; the magnolia phenol-based difunctional epoxy is dropped into meta-chloroperbenzoic acid, reacted at room temperature, then heated to react, filtered, and washed with an alkaline solution to obtain the target product, magnolia phenol-based tetrafunctional epoxy resin.
[0016] In the preparation method of the modified epoxy resin, the mass ratio of magnolol to epichlorohydrin is 1:8-2:8, the amount of catalyst added is 1 / 1000-5 / 1000 of the total mass of magnolol and epichlorohydrin, and the catalyst is tributylamine; the mass of the strong alkali solution is 25%-35% of the total mass of magnolol and epichlorohydrin; the strong alkali solution is a 50wt% sodium hydroxide solution or potassium hydroxide solution; the heating condition refers to a temperature of 80-85°C; the stirring reaction refers to a temperature of 80-85°C The reaction time is 24 to 48 hours at 25°C; after the stirring reaction is completed, the mixture is washed with deionized water for 8 to 10 times, and rotary distilled at 60 to 80°C under a vacuum water pump for 3 to 5 hours to obtain magnolia phenol difunctional epoxy; the mass ratio of magnolia phenol difunctional epoxy to m-chloroperbenzoic acid is 1:1 to 1:1.5; the room temperature reaction time is 48 to 96 hours at 25°C; the temperature increase reaction refers to heating to 50°C and then reacting for 4 to 5 hours; the washing with an alkaline solution refers to washing with a low concentration 0.1 mol / L KOH solution for 8 to 10 times.
[0017] Preferably, a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating provided by the present invention comprises the following raw materials in parts by mass: 28 to 33 parts of modified epoxy resin, 30 to 50 parts of sulfonated polyaniline-modified graphite carbon nitride, 10 to 20 parts of active diluent, 2 to 3 parts of silane coupling agent, 15 to 20 parts of polyetheramine curing agent, 15 to 30 parts of filler, and 1.5 to 2.5 parts of additive.
[0018] The active diluent is one or a combination of octyl glycidyl ether, phenyl glycidyl ether, and neopentyl glycol bisglycidyl ether.
[0019] The silane coupling agent is one or a combination of KH550, KH560 and KH570.
[0020] The polyetheramine curing agent was purchased from Shanghai Aladdin Company, with the brand name D230 and analytical grade;
[0021] The filler is one or a combination of aluminum polyphosphate, red iron oxide, and graphene, and the aluminum polyphosphate is aluminum tripolyphosphate.
[0022] The auxiliary agent is one or a combination of the anti-settling agent fumed silica, the dispersant EFKA4010, and the leveling agent BYK333.
[0023] The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating prepared by the present invention, which uses magnolia phenol-based tetrafunctional epoxy resin as the main film-forming substance, sulfonated polyaniline-modified graphite carbon nitride as the wear-resistant and anti-corrosion filler, and polyetheramine as the epoxy curing agent, can provide good anti-corrosion and anti-erosion performance for metal substrates. The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating provided by the present invention increases the surface roughness of graphite carbon nitride by chemically grafting sulfonated polyaniline on the surface of graphite carbon nitride. At the same time, the sulfonated polyaniline-modified graphite carbon nitride has good compatibility with epoxy resin, improves the density and toughness of the coating, and thus improves the anti-erosion performance of the composite coating.
[0024] The present invention provides a method for preparing a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating, which is specifically:
[0025] Add sulfonated polyaniline modified graphite carbon nitride, active diluent and filler to the modified epoxy resin, stir and disperse, then add auxiliary agent and silane coupling agent, stir, finally add polyetheramine curing agent, stir evenly, and obtain deep-sea pressure-resistant, wear-resistant and anti-corrosion coating.
[0026] The stirring dispersion refers to dispersion at 500-800 r / min for 10-15 min;
[0027] The stirring refers to stirring at 2000 r / min for 30 min.
[0028] The application of a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating provided by the present invention is used in deep-sea engineering construction. The specific application method is:
[0029] The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating is sprayed or coated on the metal substrate of marine engineering equipment with a paint film thickness of 100-500μm. It is used in deep-sea engineering construction to achieve long-term anti-corrosion and anti-erosion functions for the substrate.
[0030] Compared with the prior art, the present invention is a magnolol-based tetrafunctional epoxy resin prepared by the deacidification reaction of magnolol and epichlorohydrin, and the resin contains many epoxy groups, and can form a body cross-linked structure after reacting with a polyetheramine curing agent, thereby improving the compactness of the paint film, and the paint film has strong adhesion after curing, good deep-sea high-pressure resistance, and high hardness. Self-made sulfonated polyaniline-modified graphite carbon nitride is used as a wear-resistant and anti-corrosion filler, and sulfonated polyaniline can effectively inhibit the agglomeration of graphite carbon nitride. The wear-resistant and anti-corrosion filler has high hardness and good wear resistance. After sulfonated polyaniline is chemically grafted on the surface of graphite carbon nitride, the roughness of graphite carbon nitride can be increased, and the compatibility with epoxy resin is improved at the same time, and the anti-erosion performance and wear resistance of the composite coating are improved. The present invention uses glycidyl ether as an active diluent for the coating, and in the process of paint film curing, there is no solvent volatilization, VOC emissions are small, and it is safe and environmentally friendly. At the same time, the deep-sea special anti-erosion coating prepared by the present invention has salt spray resistance of ≥4000h, wear resistance of ≤30mg (GB / T1768, 1000g / 500r), and resistance to deep-sea 6000-meter seawater pressure of ≥60d. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Schematic diagram of the preparation of magnolol-based tetrafunctional epoxy resin;
[0032] Figure 2 Schematic diagram of the preparation of sulfonated polyaniline-modified graphite carbon nitride composite epoxy coating: (a) shows the preparation process of sulfonated polyaniline-modified graphite carbon nitride, (b) shows the polymerization reaction of generating sulfonated polyaniline; in the figure, m:n=1:1~2;
[0033] Figure 3 This is an electron transmission electron microscopy photograph of sulfonated polyaniline-modified graphite carbon nitride prepared in Example 1;
[0034] Figure 4 Infrared spectra of sulfonated polyaniline-modified graphite carbon nitride, polyaniline, and graphite carbon nitride prepared in Example 1;
[0035] Figure 5 This is a photo of the deep-sea pressure-resistant, wear-resistant and anti-corrosion coating prepared in Example 2 after being coated on a carbon steel surface and subjected to neutral salt spray for 4000 hours;
[0036] Figure 6 These are photos of on-site construction and finished product of preparing deep-sea pressure-resistant, wear-resistant and anti-corrosion coating in Example 2 and applying it on offshore wind power steel pipe piles and cages. The coating thickness is 500 microns. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0039] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0040] Example 1
[0041] A method for preparing a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating comprises the following steps:
[0042] 1) Preparation of magnolol-based tetrafunctional epoxy resin:
[0043] Mix 10.0g magnolia phenol and 80.0g epichlorohydrin in a three-necked flask and mix well. At the same time, add 0.09g tributylamine as a catalyst, maintain the water bath temperature at 80°C, then drop 28.0g of 50wt% NaOH solution, stir at 200r / min for 24h, wash with deionized water 10 times, and rotary evaporate for 5h under a vacuum water pump at 60°C to obtain magnolia phenol-based difunctional epoxy resin. Drop 100.0g of m-chloroperbenzoic acid into 80g magnolia phenol-based difunctional epoxy resin, keep the room temperature for 48h, heat to 50°C and react for another 5h, filter, wash 10 times with 0.1mol / L KOH solution, and obtain the target product magnolia phenol-based tetrafunctional epoxy resin. See the preparation diagram. Figure 1 .
[0044] 2) Preparation of sulfonated polyaniline modified graphite carbon nitride:
[0045] First, 15.1g aniline, 16.5g o-aminobenzenesulfonic acid and 21.6g graphite carbon nitride were mixed evenly in a three-necked flask, and 25mL 1mol / L hydrochloric acid solution was added in an ice bath, and the mixture was slowly stirred for 60min. Then, 0.28g ammonium persulfate catalyst was added, and the reaction was continued for 48h. Then, the mixture was washed with deionized water for 5 times and vacuum filtered to obtain sulfonated polyaniline modified graphite carbon nitride. See the preparation diagram for details. Figure 2 ; Figure 3The electron projection electron micrograph of sulfonated polyaniline-modified graphite carbon nitride was prepared. As can be seen from the figure, the graphite carbon nitride has a two-dimensional layered structure, the flake diameter is about 1 to 2 μm, and it is in a uniformly dispersed state, indicating that sulfonated polyaniline can effectively inhibit the agglomeration of graphite carbon nitride.
[0046] Figure 4 The infrared spectra of sulfonated polyaniline-modified graphite carbon nitride, commercially available polyaniline, and graphite carbon nitride prepared in Example 1 are shown in Figure 1. For pure graphite carbon nitride (g-C3N4), 1244 cm -1 It is the CN stretching vibration absorption peak, 812cm -1 is the in-plane bending vibration absorption peak of CH, 1476 cm -1 is the NH stretching vibration absorption peak; for pure polyaniline (PANi), 1244 cm -1 and 1476cm -1 The stretching vibration of CN bond and NH bond is 3467 cm -1 The peak at 616 cm-1 is the OH stretching vibration. For sulfonated polyaniline modified graphite carbon nitride (g-C3N4@SPANi), a new characteristic peak appears, with a peak at 616 cm-1. -1 、1146cm -1 and 1303cm -1 They correspond to CS stretching vibration, SO stretching vibration and S=O stretching vibration, respectively, indicating that the sulfonic acid groups have been successfully grafted to the polyaniline chains and adsorbed on the surface of graphitic carbon nitride.
[0047] 3) Preparation of deep-sea pressure-resistant, wear-resistant and anti-corrosion coatings
[0048] 30g of wear-resistant and anti-corrosion filler sulfonated polyaniline modified graphite carbon nitride, 6g of octyl glycidyl ether and 4g of phenyl glycidyl ether were added to 30g of magnolia phenol-based tetrafunctional epoxy resin in sequence, and stirred evenly at 500r / min. Then, 25g of aluminum tripolyphosphate and 1g of graphene powder were added, and dispersed at 800r / min for 15min. Then, 0.5g of anti-settling agent fumed silica, 1.5g of dispersant EFKA4010 and 2.5g of silane coupling agent KH560 were added, and stirred at 2000r / min for 30min. The mixture was ground to a fineness of 50μm, and finally 18g of polyetheramine curing agent (the polyetheramine curing agent was purchased from Shanghai Aladdin Company, brand D230, analytically pure) was added and stirred evenly to obtain a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating.
[0049] The basic performance characteristics of the deep-sea pressure-resistant, wear-resistant and anti-corrosion coating prepared above are as follows:
[0050] The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating was sprayed onto a carbon steel plate (substrate sandblasting Sa2.5 level) using compressed air, and cured at room temperature of 25°C for 24 hours, and the film thickness was controlled to be 100±5μm to obtain an anti-erosion coating. The adhesion, hardness, impact resistance, anti-erosion performance, resistance to simulated deep-sea 6000m seawater pressure, salt spray performance and wear resistance of the coating prepared in Example 1 are shown in Table 1.
[0051] Example 2
[0052] A method for preparing a deep-sea pressure-resistant, wear-resistant and anti-corrosion coating comprises the following steps:
[0053] The coating is basically the same as Example 1, except that 40 g of sulfonated polyaniline-modified graphite carbon nitride and 15 g of aluminum tripolyphosphate are added when preparing the coating, and the other parameters remain unchanged. The adhesion, hardness, impact resistance, erosion resistance, resistance to simulated deep sea 6000 m seawater pressure, salt spray performance and wear resistance of the coating prepared in Example 2 are shown in Table 1.
[0054] Figure 5 This is a photo of the deep-sea pressure-resistant, wear-resistant and anti-corrosion coating prepared in Example 2 after being coated on a carbon steel surface and subjected to neutral salt spray for 4000 hours. After 4000 hours of salt spray, the coating prepared in Example 2 had no corrosion, no shedding and no blistering, and the paint film had good adhesion on the carbon steel substrate, indicating that the homemade coating had good anti-corrosion performance on the carbon steel substrate.
[0055] Figure 6 These are photos of on-site construction and finished product of the deep-sea pressure-resistant, wear-resistant and anti-corrosion coating prepared in Example 2 and applied to offshore wind power steel pipe piles and cages. The coating has good construction performance, and the adhesion of the paint film on the steel pipe pile substrate after curing is tested to reach 15.8MPa.
[0056] Comparative Example 1
[0057] According to the method described in Example 1, the difference is that the 30g magnolol-based tetrafunctional epoxy resin prepared in Example 1 is replaced by the commercially available epoxy resin E51 (the epoxy resin is purchased from Shandong Deyuan Epoxy Technology Co., Ltd.), and the others remain unchanged. The adhesion, hardness, impact resistance, erosion resistance, resistance to simulated deep sea 6000 meters seawater pressure, salt spray performance and wear resistance of the coating of this comparative example 1 are shown in Table 1.
[0058] Comparative Example 2
[0059] The method described in Example 1 is used, except that the wear-resistant and anti-corrosion filler sulfonated polyaniline-modified graphite carbon nitride is not added, the amount of aluminum tripolyphosphate added is increased to 55 g, and the other parameters remain unchanged. The adhesion, hardness, impact resistance, erosion resistance, resistance to simulated deep sea 6000 meters seawater pressure, salt spray performance and wear resistance of the coating prepared in Comparative Example 2 are shown in Table 1.
[0060] Comparative Example 3
[0061] According to the method described in Example 1, the difference is that the wear-resistant and anti-corrosion filler sulfonated polyaniline modified graphite carbon nitride is not added, the wear-resistant and anti-corrosion filler is 30g of commercially available graphite carbon nitride, and the other parameters remain unchanged. The adhesion, hardness, impact resistance, erosion resistance, resistance to simulated deep sea 6000 meters seawater pressure, salt spray performance and wear resistance of the coating prepared in this comparative example 3 are shown in Table 1.
[0062] Comparative Example 4
[0063] According to the method described in Example 1, the difference is that the wear-resistant and anti-corrosion filler sulfonated polyaniline modified graphite carbon nitride is not added, and the magnolol-based tetrafunctional epoxy resin prepared in Example 1 is not added; instead, 30g of commercially available graphite carbon nitride and 30g of commercially available epoxy resin E51 (the epoxy resin is purchased from Shandong Deyuan Epoxy Technology Co., Ltd.) are added, and the others remain unchanged. The adhesion, hardness, impact resistance, erosion resistance, resistance to simulated deep sea 6000 meters seawater pressure, salt spray performance and wear resistance of the coating prepared in this comparative example 4 are shown in Table 1.
[0064] Table 1 Comprehensive physical properties of paint films on carbon steel surfaces sprayed with paints in various embodiments and comparative examples
[0065]
[0066] Note 1: The SSRT / Constantload / Low CycleFatigue test system of Cortest Company was used to simulate the high-pressure seawater environment. The pressure was controlled at (60.0±0.1)MPa. The corrosive medium was 3.5wt% NaCl solution. The temperature in the chamber was maintained at 4±1℃ by a circulating temperature control system. The coating samples were taken out every 10 days to observe whether the paint film failed or corroded. If the coating did not fail, the high-pressure test was continued.
[0067] Note 2: Erosion resistance test method: The erosion resistance of the coating is tested using a solid / liquid / gas three-phase flow erosion wear tester. The erosion agent is composed of SiC particles and water in a mass ratio of 1:4 (where SiC is spherical with a diameter of 100μm to 150μm), the jet velocity is 2.36m / s (gas pressure is 0.2MPa), the impact angle is 90°, and the coating sample erosion time is 30min. Record the mass difference before and after erosion.
[0068] By comparing the test results of Example 1 and Example 2, it is shown that the content of sulfonated polyaniline modified graphite carbon nitride is proportional to the wear resistance and erosion resistance of the paint film. As the content of sulfonated polyaniline modified graphite carbon nitride in the formulation components increases, the hardness of the cured coating increases, and the wear resistance and erosion resistance are enhanced.
[0069] By comparing the test results of Example 1 and Comparative Example 1, it is shown that the self-made magnolia phenol-based tetrafunctional epoxy resin is the main film-forming substance, which can significantly improve the hardness, deep sea water pressure corrosion resistance and salt spray resistance of the paint film on carbon steel. The main reason is that the magnolia phenol-based tetrafunctional epoxy resin contains many epoxy functional groups, which can form a three-dimensional cross-linked structure after reacting with the polyetheramine curing agent, thereby improving the density and wear resistance of the paint film.
[0070] By comparing the test results of Example 1 and Comparative Example 2, it is shown that the use of sulfonated polyaniline-modified graphite carbon nitride as a wear-resistant and anti-corrosion filler can improve the hardness, wear resistance and erosion resistance of the paint film.
[0071] By comparing the test results of Example 1 and Comparative Example 3, it is shown that adding commercially available graphite carbon nitride (without chemical modification) to epoxy resin leads to a decrease in the salt spray resistance, deep sea pressure resistance, impact resistance and erosion resistance of the paint film.
[0072] By comparing the test results of Example 1, Comparative Example 3 and Comparative Example 4, it is shown that the magnolia phenol-based tetrafunctional epoxy resin has better salt spray resistance and adhesion than the commercially available epoxy resin E51, and the use of sulfonated polyaniline-modified graphite carbon nitride as a wear-resistant and anti-corrosion filler can improve the wear resistance and erosion resistance of the paint film. Therefore, the use of magnolia phenol-based tetrafunctional epoxy resin and sulfonated polyaniline-modified graphite carbon nitride can synergistically enhance the erosion resistance and deep sea pressure resistance of the paint film.
[0073] In the present invention, the magnolol-based tetrafunctional epoxy resin has a high epoxy value, a high crosslinking density after reacting with a curing agent, and an increased strength. When compounded with sulfonated polyaniline-modified graphite carbon nitride, the overall erosion resistance and wear resistance of the coating are improved. The comparative experimental results of the embodiments and comparative examples show the synergistic effect of the above raw materials.
[0074] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A deep-sea pressure-resistant, wear-resistant and anti-corrosion coating, characterized in that: The raw materials of the sea pressure-resistant, wear-resistant and anti-corrosion coating include sulfonated polyaniline-modified graphite carbon nitride; The preparation method of the sulfonated polyaniline modified graphite carbon nitride is: After aniline, o-aminobenzenesulfonic acid and graphite carbon nitride are uniformly mixed, hydrochloric acid solution is added under ice bath condition, after stirring, a catalyst is added and reacted to obtain sulfonated polyaniline modified graphite carbon nitride.
2. The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating according to claim 1 is characterized in that: The mass ratio of aniline, o-aminobenzenesulfonic acid and graphite carbon nitride is 1-2:1-2:2-3; the amount of the catalyst is 0.5 / 100-1 / 100 of the total mass of aniline, o-aminobenzenesulfonic acid and graphite carbon nitride.
3. The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating according to claim 1 or 2, characterized in that: The stirring time is 30 to 60 minutes; the reaction time is 30 to 50 hours under ice bath conditions at 0-5°C.
4. The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating according to claim 1 or 2, characterized in that: The catalyst is ammonium persulfate.
5. The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating according to claim 1, characterized in that: The raw materials of the deep-sea pressure-resistant, wear-resistant and anti-corrosion coating also include modified epoxy resin; the modified epoxy resin is magnolol-based tetrafunctional epoxy resin.
6. The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating according to any one of claims 1 to 5, characterized in that: The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating comprises the following raw materials in parts by weight: 28 to 33 parts of modified epoxy resin, 30 to 50 parts of sulfonated polyaniline-modified graphite carbon nitride, 10 to 20 parts of active diluent, 2 to 3 parts of silane coupling agent, 15 to 20 parts of polyetheramine curing agent, 15 to 30 parts of filler and 1.5 to 2.5 parts of auxiliary agent.
7. The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating according to claim 6, characterized in that: The active diluent is one or a combination of octyl glycidyl ether, phenyl glycidyl ether, and neopentyl glycol bisglycidyl ether.
8. The deep-sea pressure-resistant, wear-resistant and anti-corrosion coating according to claim 6 or 7, characterized in that: The polyetheramine curing agent is D230 polyetheramine curing agent.
9. A method for preparing the deep-sea pressure-resistant, wear-resistant and anti-corrosion coating according to any one of claims 1 to 8, characterized in that: The preparation method is: Add sulfonated polyaniline modified graphite carbon nitride, active diluent and filler to the modified epoxy resin, stir and disperse, then add auxiliary agent and silane coupling agent, stir, finally add polyetheramine curing agent, stir evenly, and obtain deep-sea pressure-resistant, wear-resistant and anti-corrosion coating.
10. An application of the deep-sea pressure-resistant, wear-resistant and anti-corrosion coating according to any one of claims 1 to 8, characterized in that: Used for deep sea engineering construction.
Citation Information
Patent Citations
Aminated GO / sulfonated polyaniline modified waterborne epoxy resin anticorrosive coating
CN113583544A
Phytic acid doped carbon nitride-polyaniline nano composite material and preparation method thereof as well as intumescent fire retardant coating and preparation method thereof
CN114409897A
Graphene oxide modified bio-based epoxy anticorrosive paint as well as preparation method and application thereof
CN117844336A
Cited By
Functional filler and preparation method thereof, deep-sea pressure-resistant anti-erosion heavy-duty anticorrosive paint and application
CN120158116A
Functional filler and preparation method thereof, deep-sea pressure-resistant, erosion-resistant, heavy-duty anti-corrosion coating and application thereof
CN120158116B