Wafer cutting protective film
By using the TPU layer and the extension layer in the wafer cutting protective film and using the acrylate polymer adhesive layer, the problem of poor adhesion between the adhesive layer and the substrate layer in the prior art is solved, and the wafer cutting protection is improved The adhesive properties and structural stability of the film improve the preparation yield and production efficiency.
Patent Information
- Application Number
- CN202411147489.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
The adhesion of the adhesive layer and the substrate layer of the existing wafer cutting protective film is poor, resulting in poor cutting, which affects the wafer preparation yield and production efficiency.
The TPU layer is combined with the extension layer. The extension layer is composed of the first thermoplastic elastomer. By controlling the molecular weight and molecular distribution, combining the adhesive layer of the acrylate polymer, the adhesion ability and interface adhesion are improved, and the substrate layer and adhesion are optimized. composite performance of the layer.
It significantly improves the adhesive performance and structural stability of the wafer cutting protective film, prevents layering and degumming, and improves the preparation yield and production efficiency of the wafer.
Smart Images

Figure CN118931404A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of adhesives, and in particular, relates to a wafer cutting protective film. Background Art
[0002] Wafer cutting is an essential process in the semiconductor chip manufacturing process. It is a post-processing process after crystal column slicing. The whole wafer with the finished chip is divided into single chips according to the chip size. Since most semiconductor chips are silicon chips, which are brittle materials, the broken edges and corners will affect the strength of the chip, and the surface finish is easily damaged during the cutting process, which will affect the subsequent processes. In order to avoid the above problems, a protective film needs to be set in the wafer cutting process to play a certain protective role and improve the yield of the chip.
[0003] Currently, the existing wafer cutting protective film includes a substrate layer and a sticky layer. The substrate layer is generally made of polyvinyl chloride (PVC), polyolefin (PO), and thermoplastic polyurethane elastomer (TPU). Among them, the problem of plasticizer migration in PVC has been difficult to solve. It is also a carcinogen and is toxic to human health and the ecological environment. PO has a large shrinkage rate, low adhesion with glue, and poor stability. It is generally not suitable for wafer cutting. TPU has excellent comprehensive performance and is a new polymer environmentally friendly material between rubber and plastic. It is expected to replace the commonly used PVC and PO as the substrate layer. However, there is a difference in interface performance between TPU as a substrate layer and the sticky layer. The substrate layer and the sticky layer have poor adhesion, which results in the problem that the wafer cutting protective film is not firmly attached to the wafer and the protective effect fails, which seriously affects the wafer preparation yield. Summary of the invention
[0004] The purpose of the present invention is to provide a wafer cutting protective film, the adhesive layer of the wafer cutting protective film and the substrate layer have good bonding effect and interface adhesion, which is beneficial to improving the protection ability of the wafer cutting protective film to the wafer during the cutting process, thereby improving the preparation yield of the wafer.
[0005] According to the first aspect of the present invention, there is provided a wafer cutting protective film, comprising a substrate layer and a sticky layer, the substrate layer comprising a TPU layer and an extension layer, the TPU layer, the extension layer and the sticky layer being compounded in sequence; the TPU layer comprising a thermoplastic polyurethane elastomer; the extension layer comprising a first thermoplastic elastomer, the first thermoplastic elastomer comprising at least one of polyvinyl acetate and polycarbonate, the molecular weight of the first thermoplastic elastomer being 15,000 to 100,000; the sticky layer comprising an acrylate polymer, the weight average molecular weight of the acrylate polymer being Mw, the number average molecular weight of the acrylate polymer being Mn, the acrylate polymer satisfying: 1<Mw / Mn≤2.5, and Mw≥100,000.
[0006] Since the interface polarity of TPU as the substrate layer and the adhesive layer is greatly different, the substrate layer and the adhesive layer are prone to poor contact and delamination when directly attached. Therefore, the present invention sets an extension layer between the TPU layer and the adhesive layer, and uses a first thermoplastic elastomer as the extension layer. The extension layer has good compatibility with the TPU layer and the adhesive layer, so that the adhesive layer and the substrate layer maintain excellent bonding effect and interface adhesion. Based on this, by further controlling the molecular weight of the first thermoplastic elastomer and the molecular weight and distribution level of the acrylic polymer in the adhesive layer, the extension layer and the adhesive layer have excellent cohesion and good processing performance, which is conducive to further promoting the composite of the substrate layer and the adhesive layer, so that the wafer cutting protective film provided by the present invention has excellent bonding ability, mechanical properties and structural stability; in addition, the above-mentioned adhesive layer can improve the peeling strength of the wafer cutting protective film before UV viscosity reduction, and reduce the peeling strength and residue content after UV viscosity reduction, so as to avoid residual glue and residual monomers from contaminating the wafer.
[0007] In summary, the wafer cutting protection film provided by the present invention can effectively protect the wafer from cutting, solve the problem of poor adhesion between the adhesive layer and the substrate layer in the prior art, and prevent the wafer cutting protection film from stratification and debonding. Moreover, since the thickness of the wafer is small and it is brittle and fragile, the wafer cutting protection film with high adhesion and excellent structural stability can effectively protect the wafer surface and prevent the wafer surface from being damaged, thereby improving the wafer preparation yield and production efficiency.
[0008] Preferably, the first thermoplastic elastomer includes polyvinyl acetate, which includes ethylene-vinyl acetate copolymer, and the content of vinyl acetate in the ethylene-vinyl acetate copolymer is 15wt% to 30wt%. The ethylene-vinyl acetate copolymer (EVA) with the above-mentioned specific vinyl acetate (VA) content has a suitable molecular weight and good film-forming properties, which is conducive to further promoting the compounding of the substrate layer and the adhesive layer, so that the mechanical properties and bonding effect of the wafer cutting protective film are improved.
[0009] Preferably, the preparation method of the substrate layer includes the following operations: compounding the TPU layer and the extension layer by a coextrusion process, thereby preparing the substrate layer; wherein the coextrusion temperature of the coextrusion process is 170-190°C; in the TPU layer, the melt index of the thermoplastic polyurethane elastomer under the test conditions of 190°C and 2.16kg is 28-35g / 10min; in the extension layer, the melt index of the first thermoplastic elastomer under the test conditions of 190°C and 2.16kg is 26-34g / 10min. By controlling the melt index of TPU and the first thermoplastic elastomer, it is beneficial to improve the processing performance of the TPU layer and promote the firm compounding of the TPU layer and the extension layer.
[0010] Preferably, the raw materials for preparing the acrylic ester polymer include ethylene-acrylate copolymer, homopolypropylene, styrene thermoplastic elastomer and ethylene-vinyl acetate copolymer; wherein, calculated by mass ratio, ethylene-acrylate copolymer: homopolypropylene: styrene thermoplastic elastomer: ethylene-vinyl acetate copolymer = 10-40: 25-45: 30-50: 5-20. By optimizing the formula of the viscous layer, the ethylene-acrylate copolymer, homopolypropylene, styrene thermoplastic elastomer and ethylene-vinyl acetate copolymer can play a synergistic role, so that the viscous layer formed thereby has a higher cohesive force, thereby enabling the wafer cutting protective film to reduce its interfacial peeling force after UV viscosity reduction while maintaining good initial adhesion and tensile strength, so as to facilitate peeling and removal.
[0011] Preferably, the styrene thermoplastic elastomer comprises polystyrene-polybutadiene-polystyrene (SBS).
[0012] Preferably, the raw materials of the adhesive layer also include a thermal initiator and a photoinitiator; the thermal initiator includes at least one of divinylbenzene, triallyl isocyanurate, diallyl bisphenol A, 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane, di-tert-butyl peroxide, benzoyl peroxide, and diisopropylbenzene hydroperoxide; the photoinitiator includes at least one of benzophenone, 4-phenylbenzophenone, 2-ethylhexyl-4-dimethylaminobenzoate, and ethyl-4-dimethylaminobenzoate.
[0013] Preferably, the raw materials of the adhesive layer also include an antioxidant, and the antioxidant includes at least one of antioxidant 1010, pentaerythritol tetra[β-propionate] ester, tris(2,4-di-tert-butylphenyl) phosphite, 4,4'-thiobis(6-tert-butyl-3-methylphenol), 2,4-di(n-octylthiomethylene)-6-methylphenol, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 2,6-di-tert-butyl-p-cresol, and glycol bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate.
[0014] Preferably, the molecular weight of ethylene-acrylate copolymer is 5,000 to 50,000, the molecular weight of homopolypropylene is 200,000 to 400,000, the molecular weight of styrene thermoplastic elastomer is 200,000 to 400,000, and the molecular weight of ethylene-vinyl acetate copolymer is 15,000 to 50,000. The above-mentioned ethylene-acrylate copolymer, styrene thermoplastic elastomer, and EVA with specific molecular weight provide good flexibility and bonding properties for the wafer cutting protective film; homopolypropylene provides good tensile strength and bonding properties for the wafer cutting protective film, and the molecular weight distribution of the adhesive layer formed by the above-mentioned components is uniform and the residual monomer content is small, which is conducive to further optimizing the bonding effect and peeling effect of the wafer cutting protective film, so that the risk of residual glue and small molecules precipitating to contaminate the wafer is reduced; in addition, the above-mentioned components have good compatibility, which is conducive to improving the processing performance of the wafer cutting protective film.
[0015] Preferably, the method for preparing the wafer cutting protective film includes the following operations: the TPU layer, the extension layer and the adhesive layer are compounded in sequence by a co-extrusion process, thereby preparing the wafer cutting protective film; the co-extrusion temperature of the co-extrusion process is 145-190°C; in the adhesive layer, the melt index of the acrylate polymer under the test conditions of 190°C and 2.16kg is 20-35g / 10min, and in the extension layer, the melt index of the first thermoplastic elastomer under the test conditions of 190°C and 2.16kg is 26-34g / 10min. By controlling the co-extrusion temperature of the co-extrusion process for preparing the wafer cutting protective film and the melt indexes of the acrylate polymer in the viscous layer and the first thermoplastic elastomer in the extension layer, it is beneficial to improve the processing performance of the viscous layer and the extension layer and promote the firm compounding of the viscous layer and the extension layer.
[0016] Preferably, the raw materials for preparing the acrylic ester polymer include acrylic ester soft monomer, acrylic ester hard monomer, ethylene-vinyl acetate copolymer, hydroxyl-containing acrylic ester monomer and isocyanate; wherein, calculated by weight fraction ratio, butyl methacrylate: methyl methacrylate: ethylene-vinyl acetate copolymer: hydroxyl-containing acrylic ester monomer: isocyanate = 30-60: 10-30: 2-10: 5-20: 2-10. By reasonably setting the formula of the adhesive layer, it is helpful to ensure that the adhesive layer has a good molecular weight and its distribution, and the adhesive layer forms a three-dimensional network cross-linked structure, giving the wafer cutting protective film good bonding performance and peeling effect.
[0017] Preferably, the hydroxyl-containing acrylate monomer includes hydroxybutyl acrylate.
[0018] Preferably, the isocyanate comprises a diisocyanate.
[0019] Preferably, the isocyanate includes diisocyanate. The diisocyanate has a suitable reactivity, which is beneficial to maintaining a firm bond between the adhesive layer and the TPU layer while reducing the interfacial peeling force after UV viscosity reduction.
[0020] Preferably, the diisocyanate includes at least one of trimethylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate trimer.
[0021] Preferably, the preparation method of the wafer cutting protective film includes the following operations: mixing the raw materials for preparing the acrylate polymer and heating the temperature to 50-80°C to obtain an adhesive stock solution; then coating the adhesive stock solution onto a release film and drying it to obtain an adhesive film; then transferring the adhesive film to the substrate layer to obtain a wafer cutting protective film.
[0022] Preferably, the thickness of the wafer cutting protection film is 50-120 μm, and the thickness of the adhesive layer is ≤30 μm. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the structure of the wafer cutting protection film prepared in Examples 1 to 10 and Comparative Examples 2 to 5.
[0024] Figure 2 Schematic diagram of the structure of the wafer cutting protection film prepared in Examples 11 to 12.
[0025] Figure 3 This is a schematic diagram of the structure of the wafer cutting protection film prepared in Comparative Example 1.
[0026] In the above drawings, the correspondence between the technical features and the drawing marks is: 1 TPU layer, 2 extension layer, 3 adhesive layer, 4 release layer. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0028] Example 1
[0029] This embodiment provides a wafer cutting protection film, and the preparation method thereof includes the following operations:
[0030] 1. Prepare the raw materials as follows:
[0031] Raw materials for TPU layer: TPU granules, the brand of TPU granules is PearlbondTM 1160, melt index (according to ISO 1133 test standard) at 190°C and 2.16kg is 30g / 10min, and tensile strength is 30MPa;
[0032] The raw material of the extension layer: EVA granules, the brand of EVA granules is COSMOTHENE TM VF024N00, the melt index (according to ISO 1133 test standard) under the test conditions of 190°C and 2.16kg is 28g / 10min, and the VA content is 28wt%;
[0033] Raw materials for the viscous layer: The raw materials for the viscous layer are shown in Table 1 below.
[0034] 2. The raw materials of the TPU layer, the extension layer, and the adhesive layer are dried separately, and then the raw materials of the adhesive layer are blended. Subsequently, the raw materials of the TPU layer, the extension layer, and the blended adhesive layer are put into a screw extruder (the die temperature is controlled at 180-190°C, the screw aspect ratio is 30:1, and the screw speed is 70rpm) and heated to a molten state (segmented melting, the segmented melting temperatures are controlled at 145-155°C, 155-165°C, 165-175°C, and 175-190°C, respectively), and then co-extruded, cast, and compositely molded in layer order to obtain the wafer cutting protective film of this embodiment.
[0035] The schematic diagram of the structure of the wafer cutting protection film of this embodiment is as follows Figure 1 As shown, its structure includes a TPU layer 1, an extension layer 2, and an adhesive layer 3 in the thickness direction, wherein the TPU layer includes a thermoplastic polyurethane elastomer, the extension layer includes EVA (molecular weight is 80000), the adhesive layer includes an acrylate polymer (the acrylate polymer satisfies: Mw / Mn is 1.8, Mw is 165000), the substrate layer is composed of the TPU layer 1 and the extension layer 2, the thickness of the substrate layer is 65μm, and the thickness of the adhesive layer is 20μm.
[0036] Table 1. Raw materials for the adhesive layer of Example 1
[0037]
[0038] Example 2
[0039] This embodiment refers to Example 1 to prepare a wafer cutting protective film. The difference between this embodiment and Example 1 is that in the process of preparing the wafer cutting protective film, the same weight of polycarbonate is used to replace EVA to prepare the extension layer. Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0040] Example 3
[0041] This embodiment prepares a wafer cutting protection film with reference to the embodiment 1. The difference between this embodiment and the embodiment 1 is that the content of vinyl acetate (VA) in the EVA used in the extension layer of this embodiment is 12%. Except for the above difference, the materials and process operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0042] Example 4
[0043] This embodiment refers to Example 1 to prepare a wafer cutting protection film. The difference between this embodiment and Example 1 is that the content of vinyl acetate (VA) in EVA used in the raw material of the extension layer in this embodiment is 35%. Except for the above difference, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0044] Example 5
[0045] This embodiment refers to Example 1 to prepare a wafer cutting protective film. The difference between this embodiment and Example 1 is that among the raw materials of the TPU layer used in this embodiment, the melt index of TPU under the test conditions of 190°C and 2.16kg (according to ISO 1133 test standard) is 25g / 10min. Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0046] Example 6
[0047] This embodiment refers to Example 1 to prepare a wafer cutting protective film. The difference between this embodiment and Example 1 is that among the raw materials of the TPU layer used in this embodiment, the melt index of TPU under the test conditions of 190°C and 2.16kg (according to ISO 1133 test standard) is 39g / 10min. Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0048] Example 7
[0049] This embodiment refers to Example 1 to prepare a wafer cutting protective film. The difference between this embodiment and Example 1 is that in the raw materials of the adhesive layer used in this embodiment, ethylene-acrylate copolymer is 40 parts by weight and homopolypropylene is 10 parts by weight; the acrylate polymer in the adhesive layer prepared in this embodiment satisfies: Mw / Mn is 1.1 and Mw is 124000. Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in Example 1.
[0050] Example 8
[0051] This embodiment is used to prepare a wafer cutting protective film with reference to the embodiment 1. The difference between this embodiment and the embodiment 1 is that in the raw materials of the adhesive layer used in this embodiment, the ethylene-acrylate copolymer is 10 parts by weight and the homopolypropylene is 40 parts by weight; the acrylate polymer in the adhesive layer prepared in this embodiment satisfies: Mw / Mn is 2.0 and Mw is 202000. Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0052] Example 9
[0053] This embodiment refers to the embodiment 1 to prepare a wafer cutting protective film. The difference between this embodiment and the embodiment 1 is that in the raw material of the adhesive layer used in this embodiment, the molecular weight of the ethylene-ethyl acrylate copolymer is 55000; the acrylic acid ester polymer in the adhesive layer prepared in this embodiment satisfies: Mw / Mn is 2.5, and Mw is 221000. Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0054] Example 10
[0055] This embodiment provides a wafer cutting protection film, and the preparation method thereof includes the following operations:
[0056] 1. Prepare the raw materials as follows:
[0057] Raw materials for the TPU layer: TPU pellets, the grade of TPU pellets is Ultralast TM ME930, melt index (according to ISO 1133 test standard) at 190°C and 2.16kg is 28g / 10min, and tensile strength is 32MPa;
[0058] The raw material of the extension layer: EVA granules, the brand of EVA granules is ATEVA TM 1641, the melt index (according to ISO 1133 test standard) under the test conditions of 190°C and 2.16kg is 28g / 10min, and the VA content is 16wt%;
[0059] Raw materials for the viscous layer: The raw materials for the viscous layer are shown in Table 2 below.
[0060] 2. The raw materials of the TPU layer and the raw materials of the extension layer are dried respectively, and then the raw materials of the TPU layer and the raw materials of the extension layer are put into a screw extruder (the die temperature is controlled at 180-190°C, the screw aspect ratio is 30:1, and the screw speed is 70rpm) and heated to a molten state (segmented melting, the segmented melting temperatures are controlled at 145-155°C, 155-165°C, 165-175°C, and 175-190°C, respectively), and then co-extruded and cast according to the interlayer order and compositely molded to obtain a substrate layer;
[0061] 3. Blend the raw materials of the above-mentioned viscous layer to form a mixed liquid, then take out 10wt% of the mixed liquid and heat it to 50-80℃ and keep it warm for 0.5-1.5 hours, then slowly add the remaining mixed liquid, and keep it warm for 2-4 hours after the addition is completed to obtain an adhesive stock solution; then, apply the adhesive stock solution to the release film, dry and remove the solvent to obtain an adhesive film; then, transfer the adhesive film to the substrate layer, roll it up, and mature it, thereby obtaining the wafer cutting protective film of this embodiment.
[0062] The schematic diagram of the structure of the wafer cutting protection film of this embodiment is as follows Figure 2 As shown, its structure includes TPU layer 1, extension layer 2, adhesive layer 3, and release layer 4 in the thickness direction, wherein the TPU layer includes thermoplastic polyurethane elastomer, the extension layer includes EVA (molecular weight is 18000), the adhesive layer includes acrylate polymer (the acrylate polymer satisfies: Mw / Mn is 1.4, Mw is 130000), the substrate layer is composed of TPU layer 1 and extension layer 2, the thickness of the substrate layer is 65μm, and the thickness of the adhesive layer is 20μm.
[0063] Table 2. Raw materials for the adhesive layer of Example 11
[0064]
[0065]
[0066] Embodiment 11
[0067] This embodiment refers to the embodiment 10 to prepare the wafer cutting protection film. The difference between this embodiment and the embodiment 10 is that in the process of preparing the wafer cutting protection film, the adhesive layer is prepared by replacing trimethylene diisocyanate with ethyl isocyanate acrylate in the same weight portion. Except for the above difference, the materials and process operations used in this embodiment are strictly consistent with those in the embodiment 10.
[0068] Comparative Example 1
[0069] This comparative example refers to Example 1 to prepare a wafer cutting protective film. The difference between this comparative example and Example 1 is that in the process of preparing the wafer cutting protective film, this comparative example does not set an extension layer 2. In addition to the above differences, the materials and process operations used in this comparative example are strictly consistent with those in Example 1.
[0070] The structural schematic diagram of the wafer cutting protection film of this comparative example is as follows Figure 3 As shown, its structure includes a TPU layer 1 and an adhesive layer 3 in sequence in the thickness direction, wherein the substrate layer is composed of the TPU layer 1, the thickness of the substrate layer is 65 μm, and the thickness of the adhesive layer is 20 μm.
[0071] Comparative Example 2
[0072] This comparative example refers to Example 1 to prepare a wafer cutting protective film. The difference between this comparative example and Example 1 is that the molecular weight of EVA in the raw material of the extension layer used in this comparative example is 10000. In addition to the above differences, the materials and process operations used in this comparative example are strictly consistent with those in Example 1.
[0073] Comparative Example 3
[0074] This comparative example prepares a wafer cutting protective film with reference to Example 1. The difference between this comparative example and Example 1 is that the molecular weight of EVA in the raw material of the extension layer used in this comparative example is 120000. Except for the above difference, the materials and process operations used in this comparative example are strictly consistent with those in Example 1.
[0075] Comparative Example 4
[0076] This comparative example refers to Example 1 to prepare a wafer cutting protective film. The difference between this comparative example and Example 1 is that this comparative example adjusts the raw materials and the ratio of the adhesive layer so that the acrylic ester polymer in the prepared adhesive layer satisfies: Mw / Mn is 2.0, and Mw is 80000. Except for the above differences, the materials and process operations used in this comparative example are strictly consistent with those in Example 1.
[0077] Comparative Example 5
[0078] This comparative example refers to Example 1 to prepare a wafer cutting protective film. The difference between this comparative example and Example 1 is that this comparative example adjusts the raw materials and the ratio of the adhesive layer so that the acrylic ester polymer in the prepared adhesive layer satisfies: Mw / Mn is 3.0, and Mw is 120000. In addition to the above differences, the materials and process operations used in this comparative example are strictly consistent with those in Example 1.
[0079] Test Example 1
[0080] 1. Participants
[0081] The wafer cutting protection films prepared in Examples 1 to 11 and Comparative Examples 1 to 5 were used as test objects in this test example.
[0082] 2. Test items and test methods:
[0083] (1) Peeling force before UV irradiation: Referring to the test method in GB / T 2792-2014 Test method for peeling strength of adhesive tape, the test object was cut into a size of 24mm*150mm, and the release layer of the test object was peeled off, and the adhesive layer was attached to the steel plate, and rolled back and forth with a 1kg rubber roller three times, and placed in an environment of 23±1℃ and 50±5%RH for 20min. Then, the test object was peeled off from the steel plate at a peeling speed of 300mm / min and a peeling angle of 180°, and the peeling force of the test object before UV irradiation was recorded.
[0084] (2) Peel strength after UV irradiation: Referring to the test method in GB / T 2792-2014 Test method for peel strength of adhesive tape, the test object was cut into a size of 24 mm*150 mm, and the release layer of the test object was peeled off, and the adhesive layer was attached to the steel plate. A 1 kg rubber roller was used to roll back and forth three times. After being placed in an environment of 23±1°C and 50±5% RH for 20 min, the test object was tested at a pressure of 250 mJ / cm 2 After UV irradiation, the test object was placed for 30 minutes. Then, the test object was peeled off from the steel plate at a peeling speed of 300 mm / min and a peeling angle of 180°, and the peeling force of the test object after UV irradiation was recorded.
[0085] (3) Tensile strength and elongation at break: refer to the test method in GB / T 30776-2014 Test method for tensile strength and elongation at break of adhesive tape for rating.
[0086] (4) Wafer defect rate: The test object was attached to the wafer surface, cut and expanded, and then irradiated with 250 mJ / cm 2 UV light irradiation, placed for 30 minutes, to obtain wafer samples. Repeat the preparation of 10,000 wafer samples. When the wafer samples have cracks, scratches, breakage or residual glue on the surface, they are identified as defective and marked as defective.
[0087] 3. Test results and analysis
[0088] Table 3. Test results of Examples 1 to 11 and Comparative Examples 1 to 5
[0089]
[0090] The test results are shown in Table 1. By comparing the performance test results corresponding to Example 1 and Comparative Example 1, it can be found that the tensile strength and elongation at break of the wafer cutting protective film prepared in Comparative Example 1 are lower than those in Example 1, the wafer defect rate is higher than that in Example 1, and debonding occurs before UV. The reason is that the wafer cutting protective film of Comparative Example 1 is not provided with an extension layer. Due to the large difference in the interface polarity between the TPU layer and the adhesive layer, direct bonding is prone to poor contact and delamination between the substrate layer and the adhesive layer, thereby deteriorating the bonding performance and mechanical properties of the protective film, which is not conducive to effectively protecting the wafer surface and increasing the wafer defect rate.
[0091] By comparing the performance test results corresponding to Example 1 and Comparative Examples 2-3, it can be found that the tensile strength, elongation at break, and pre-UV peeling force of the wafer cutting protective film prepared in Comparative Examples 2-3 are lower than those in Example 1, and the wafer defect rate is higher than that in Example 1. The reason is that the molecular weight of the first thermoplastic elastomer EVA in the extension layer of Comparative Examples 2-3 exceeds 15,000 to 100,000, which reduces the cohesive force of the extension layer and is not conducive to its composite with the TPU layer and the adhesive layer, thereby deteriorating the bonding performance and mechanical properties of the protective film, which is not conducive to effectively protecting the wafer surface and increases the wafer defect rate.
[0092] By comparing the performance test results corresponding to Example 1 and Comparative Examples 4-5, it can be found that the tensile strength and elongation at break of the wafer cutting protective film prepared in Comparative Examples 4-5 are lower than those in Example 1, and the post-UV peeling force and wafer defect rate are higher than those in Example 1. The reason is that the molecular weight of the acrylate polymer in the adhesive layer of Comparative Example 4 is lower than 100,000, and the Mw / Mn of the acrylate polymer in the adhesive layer of Comparative Example 5 is higher than 2.5. The wafer cutting protective film has good peeling strength before UV viscosity reduction, but residual glue and residual monomers are prone to appear in the adhesive layer after UV viscosity reduction, which increases the peeling strength after UV viscosity reduction, thereby deteriorating the adhesive performance and mechanical properties of the protective film, which is not conducive to effectively protecting the wafer surface and increases the wafer defect rate.
[0093] The performance test results of Example 1 are compared with those of Examples 3 to 4. As shown in Table 1, under the same conditions of other materials and operations for preparing the wafer cutting protective film, the VA content in the EVA in the extension layer of Example 3 is less than 15wt%, and the elongation at break and the peeling force before UV of the protective film thus prepared are lower than those of Example 1, and the peeling force and wafer defect rate after UV are higher than those of Example 1; the VA content in the EVA in the extension layer of Example 4 is higher than 30wt%, and the tensile strength and the peeling force before UV of the protective film thus prepared are lower than those of Example 1, and the peeling force and wafer defect rate after UV are higher than those of Example 1. This shows that, relative to Examples 2 to 3, Example 1 controls the content of vinyl acetate (VA) in ethylene-vinyl acetate copolymer (EVA) so that the extension layer has a suitable molecular weight and good film-forming properties, which is conducive to further promoting the composite of the substrate layer and the adhesive layer, improving the mechanical properties and bonding effect of the wafer cutting protective film, and reducing the wafer defect rate.
[0094] The performance test results of Example 1 are compared with those of Examples 5 to 6. As shown in Table 1, under the same conditions of other materials and operations for preparing the wafer cutting protective film, the melt index of TPU in the TPU layer of Example 5 is lower than 28g / 10min, and the elongation at break of the protective film prepared thereby is lower than that of Example 1, and the wafer defect rate is higher than that of Example 1; the melt index of TPU in the TPU layer of Example 6 is higher than 35g / 10min, and the tensile strength of the protective film prepared thereby is lower than that of Example 1, and the wafer defect rate is higher than that of Example 1. This shows that, compared with Examples 5 to 6, Example 1 is beneficial to improving the processing performance and mechanical properties of the TPU layer by controlling the melt index of the TPU in the TPU layer and the first thermoplastic elastomer in the extension layer, and promoting the firm compounding of the TPU layer and the extension layer, so that the mechanical properties and bonding effect of the wafer cutting protective film are improved, and the wafer defect rate is reduced.
[0095] The performance test results of Example 1 are compared with those of Examples 7 to 9. As shown in Table 1, under the same conditions of other materials and operations for preparing the wafer cutting protective film, the molecular weight of the acrylate polymer in the adhesive layer of Example 9 is high and the distribution is relatively uneven, so the tensile strength, elongation at break, and peeling force before UV of the protective film prepared thereby are lower than those of Example 1, while the peeling force after UV and the wafer defect rate are higher than those of Examples 1, 7 to 8. This shows that, relative to Example 9, Examples 1, 7 to 8 can improve the peeling strength before UV viscosity reduction and reduce the peeling strength and residue content after UV viscosity reduction by controlling the molecular weight and distribution of the acrylate polymer in the adhesive layer while ensuring the good mechanical properties of the wafer cutting protective film, thereby avoiding contamination of the wafer by residual adhesive and residual monomer, improving the mechanical properties and bonding effect of the wafer cutting protective film, and reducing the wafer defect rate.
[0096] The performance test results of Example 10 and Example 11 are compared. As shown in Table 1, under the same conditions of other materials and operations for preparing the wafer cutting protective film, Example 11 uses monoisocyanate (isocyanate ethyl acrylate) to prepare the adhesive layer, and the tensile strength, elongation at break and pre-UV peeling force of the protective film prepared thereby are lower than those of Example 10, and the post-UV peeling force and wafer defect rate are higher than those of Example 10. This shows that, relative to Example 11, Example 10 uses diisocyanate to prepare the adhesive layer, and the reaction activity of the diisocyanate is appropriate, which is conducive to maintaining a firm bond between the adhesive layer and the TPU layer while reducing its interfacial peeling force after UV viscosity reduction, thereby improving the mechanical properties and bonding effect of the wafer cutting protective film and reducing the wafer defect rate.
[0097] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.
Claims
1. A wafer cutting protective film, characterized in that: It comprises a base material layer and an adhesive layer, wherein the base material layer comprises a TPU layer and an extension layer, and the TPU layer, the extension layer and the adhesive layer are compounded in sequence; The TPU layer includes a thermoplastic polyurethane elastomer; The extension layer includes a first thermoplastic elastomer, the first thermoplastic elastomer includes at least one of polyvinyl acetate and polycarbonate, and the molecular weight of the first thermoplastic elastomer is 15,000 to 100,000; The adhesive layer includes an acrylate polymer, with the weight average molecular weight of the acrylate polymer being Mw, and the number average molecular weight of the acrylate polymer being Mn. The acrylate polymer satisfies: 1<Mw / Mn≤2.5, and Mw≥100,000.
2. The wafer cutting protection film according to claim 1, characterized in that: The first thermoplastic elastomer includes polyvinyl acetate, and the polyvinyl acetate includes ethylene-vinyl acetate copolymer. The content of vinyl acetate in the ethylene-vinyl acetate copolymer is 15wt% to 30wt%.
3. The wafer cutting protection film according to claim 1, characterized in that: The method for preparing the substrate layer comprises the following operations: compounding the TPU layer and the extension layer by a co-extrusion process, thereby preparing the substrate layer; wherein the co-extrusion temperature of the co-extrusion process is 170-190° C.; In the TPU layer, the melt index of the thermoplastic polyurethane elastomer under the test conditions of 190°C and 2.16kg is 28-35g / 10min; in the extension layer, the melt index of the first thermoplastic elastomer under the test conditions of 190°C and 2.16kg is 26-34g / 10min.
4. The wafer cutting protection film according to claim 1, characterized in that: The raw materials for preparing the acrylic ester polymer include ethylene-acrylic ester copolymer, homopolypropylene, styrene thermoplastic elastomer and ethylene-vinyl acetate copolymer; wherein, calculated by mass ratio, the ethylene-acrylic ester copolymer: the homopolypropylene: the styrene thermoplastic elastomer: the ethylene-vinyl acetate copolymer = 10-40: 25-45: 30-50: 5-20.
5. The wafer cutting protection film according to claim 4, characterized in that: The molecular weight of the ethylene-acrylate copolymer is 5,000 to 50,000, the molecular weight of the homopolypropylene is 200,000 to 400,000, the molecular weight of the styrene thermoplastic elastomer is 50,000 to 150,000, and the molecular weight of the ethylene-vinyl acetate copolymer is 15,000 to 50,000.
6. The wafer cutting protection film according to claim 4 or 5, characterized in that: The method for preparing the wafer cutting protective film comprises the following operations: the TPU layer, the extension layer and the adhesive layer are compounded in sequence by a co-extrusion process, thereby preparing the wafer cutting protective film; the co-extrusion temperature of the co-extrusion process is 145-190° C.; In the adhesive layer, the melt index of the acrylic polymer under the test conditions of 190°C and 2.16kg is 20-35g / 10min, and in the extension layer, the melt index of the first thermoplastic elastomer under the test conditions of 190°C and 2.16kg is 26-34g / 10min.
7. The wafer cutting protection film according to claim 1, characterized in that: The raw materials for preparing the acrylic ester polymer include acrylic ester soft monomer, acrylic ester hard monomer, ethylene-vinyl acetate copolymer, hydroxyl-containing acrylic ester monomer and isocyanate; wherein, calculated by weight ratio, the butyl methacrylate: methyl methacrylate: the ethylene-vinyl acetate copolymer: the hydroxyl-containing acrylic ester monomer: the isocyanate = 30-60: 10-30: 2-10: 5-20: 2-10.
8. The wafer cutting protection film according to claim 7, characterized in that: The isocyanate includes diisocyanate.
9. The wafer cutting protection film according to claim 7 or 8, characterized in that: The preparation method of the wafer cutting protective film includes the following operations: mixing the raw materials for preparing the acrylic ester polymer and heating the mixture to 50-80° C. to obtain an adhesive stock solution; then coating the adhesive stock solution onto a release film and drying the adhesive film; and then transferring the adhesive film onto the substrate layer to obtain a wafer cutting protective film.
10. The wafer cutting protection film according to claim 1, characterized in that: The wafer cutting protection film has a thickness of 50 to 120 μm, and the adhesive layer has a thickness of ≤30 μm.
Citation Information
Cited By
Wafer grinding protective adhesive film and preparation method thereof
CN119684918A
Release film and oxide solid electrolyte membrane
TWI917138B