Microorganism-loaded porous additive as well as preparation method and application thereof

Through the technology of microorganisms loading porous additives, the problems of water loss of coal mine goaf sealing materials and untimely release of microorganisms are solved, and long-term sealing and safe production of coal mine goaf is achieved, and CO2 is sealed during the repair process. It complies with the dual carbon index, has good economic benefits and engineering application prospects.

CN118931512APending Publication Date: 2024-11-12CHINA UNIV OF MINING & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974417.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing coal mine goaf sealing materials have problems such as water loss and cracking, and the release of irritating gases and microorganisms in time, resulting in frequent coal spontaneous combustion accidents and safety production risks.

Method used

Microbial loaded porous additives are used to prepare microbial loaded gangue-based zeolite particles through mixing NaOH with coal gangue powder, impregnation of Bacillus bacterial solution, and powder coating technology to adjust the hydration state of the gel coating layer. Maintain the time to ensure that microorganisms release time and repair when cracks in inorganic sealing material appear.

Benefits of technology

Achieve long-term sealing of coal mine goafs, avoid secondary air leakage and ammonia pollution, improve microbial utilization, ensure safe production of coal mines, and seal CO2 during the mineralization and restoration process, comply with the dual carbon index and have good economic benefits and engineering application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931512A_ABST
    Figure CN118931512A_ABST
Patent Text Reader

Abstract

The invention discloses a microorganism-loaded porous additive and a preparation method and application thereof.The method comprises the steps that firstly, NaX zeolite is prepared from NaOH and coal gangue powder, then the NaX zeolite is soaked in bacillus liquid, and microorganism-loaded coal gangue-based zeolite particles are obtained after drying and grinding; a composite organic calcium salt and an adaptive gel coating material are used as powder coating materials, the microbe-loaded coal gangue-based zeolite particles are subjected to ball coating, ball forming and granulation in a powder coating mode after spraying wetting, the powder coating materials form a layer of gel hard shell on the surfaces of the microbe-loaded coal gangue-based zeolite particles, and the microbe-loaded porous additive is obtained after ball forming and drying. The prepared microorganism-loaded porous additive can seal and absorb a large amount of CO2 in the process of mineralizing and repairing cracks of the inorganic plugging material of the coal mine, and after different inorganic plugging materials are mixed, the release time of microorganisms can be kept consistent with the occurrence time of the cracks of the inorganic plugging material needing to be repaired by changing the proportion of the raw materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coal mine goaf blocking and fire prevention, and in particular to a microorganism-loaded porous additive and a preparation method and application thereof. Background Art

[0002] Spontaneous combustion of coal is the main natural disaster faced by coal mining in mines. With the continuous growth of coal production, the frequency of spontaneous combustion accidents in coal mine goafs has increased significantly, causing huge economic losses and a large number of casualties, and seriously damaging the surrounding natural environment. Leakage plugging technology is an effective means of preventing and controlling spontaneous combustion of coal in underground mines. By injecting leak plugging and fire extinguishing materials into the possible leakage areas underground, air is prevented from contacting the broken coal in the mine, and spontaneous combustion of coal is suppressed.

[0003] Coal mines mainly use inorganic plugging materials to plug air leakage and prevent fire in goaf areas, including solid slurry plugging materials, inorganic gel materials, high water quick-setting materials and foamed cement materials. These inorganic plugging materials all have the phenomenon of water loss and cracking, causing secondary air leakage problems, making it difficult to plug coal mine goaf areas for a long time.

[0004] In recent years, microbial induced calcium carbonate precipitation (MICP) technology has developed rapidly and has been widely used in soil reinforcement, heavy metal removal, rock repair and other fields. The use of microbial induced calcium carbonate precipitation to repair rock cracks effectively makes up for the limitations of traditional repair methods in engineering applications. The principle is that microorganisms, mainly bacteria, provide carbonate ions through their own metabolism and other reactions, and attract free calcium ions in the environment to combine with carbonate ions with their own negative charge, and use themselves as nucleation points to form calcium carbonate crystal precipitation to fill and repair the cracks.

[0005] In current technology, when using microorganisms to induce calcium carbonate precipitation to repair cracks in plugging materials, urea is added as a carbon source to produce carbonate ions. Excessive use of nitrogen-containing compounds will cause soil compaction, and the reaction process will produce a large amount of irritating gases such as ammonia, causing underground gas pollution and affecting coal mine safety production. At the same time, directly mixing the microbial mixed repair liquid into the plugging material for repair will limit the living environment of the microorganisms and make it difficult to achieve the theoretical repair effect. Some technologies use microcapsules or porous carriers to load microorganisms to ensure the living environment of microorganisms, but they will cause problems such as failure to release microorganisms in time and too fast release of microorganisms during stirring and transportation. Therefore, it is necessary to seek a new microbial-loaded porous additive and its preparation method to solve the above problems. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a microbial-loaded porous additive for self-repair of cracks in coal mine plugging materials and its application. After the prepared microbial-loaded porous additive is mixed with different inorganic plugging materials, the raw material ratio can be changed to make the microbial release time consistent with the appearance time of the cracks in the inorganic plugging materials to be repaired, thereby improving the utilization rate of the microorganisms while ensuring the living environment of the microorganisms. At the same time, no irritating gases such as ammonia will be generated during the process of microbial mineralization repair of cracks, thereby ensuring safe production underground in coal mines.

[0007] To achieve the above object, the present invention is implemented by the following technical scheme: a method for preparing a microorganism-loaded porous additive material, the preparation method comprising the following steps:

[0008] S1: NaOH and coal gangue powder are mixed and melted at 600-800°C for 1-2 hours and heated in an ultrasonic water bath for 5-8 hours, washed with deionized water, and vacuum dried for 1-2 hours to obtain NaX zeolite.

[0009] S2: soaking the NaX zeolite in a Bacillus bacterial solution for 20-30 minutes under a vacuum environment, loading the Bacillus bacteria into the NaX zeolite structure to obtain a microorganism-loaded coal gangue-based zeolite;

[0010] S3: drying the microorganism-loaded coal gangue-based zeolite obtained in step S2 in a forced air drying oven for 0.25-0.5 h, grinding the obtained microorganism-loaded coal gangue-based zeolite and passing it through a 7-16 mesh sieve to obtain microorganism-loaded coal gangue-based zeolite particles;

[0011] S4: using composite organic calcium salt and adaptive gel coating material as powder coating material, wherein the adaptive gel coating material is composed of nano-lignin, chitosan lactate, and sodium alginate in a mass ratio of 1:(3-8):(5-11); coating and granulating the microorganism-loaded gangue-based zeolite particles obtained in step S3 by spraying and wetting, and the powder coating material forms a gel hard shell on the surface of the microorganism-loaded gangue-based zeolite particles, and drying after balling to obtain the microorganism-loaded porous additive. .

[0012] Preferably, in step S1, the mass ratio of the NaOH to the coal gangue powder is 1:(1-1.25); the coal gangue powder is prepared by calcining at a high temperature above 800°C, grinding, and passing through a 120-200 mesh sieve.

[0013] Preferably, in step S2, the mass ratio between the Bacillus species and the NaX zeolite is 1:(3-7).

[0014] Preferably, in step S2, the Bacillus bacterial solution is a mixed bacterial solution, including at least two of Bacillus pasteurianus, Bacillus subtilis, Bacillus cohnii, Bacillus alkali, Bacillus halophilus, and Bacillus thuringiensis.

[0015] Preferably, in step S4, the mass ratio between the adaptive gel coating material and the composite organic calcium salt is 1:(1.5-3); the mass ratio between the powder coating material and the microorganism-loaded coal gangue-based zeolite particles is 1:(3-6).

[0016] Preferably, in step S4, the composite organic calcium salt includes at least two of calcium acetate, calcium lactate, sugar alcohol calcium or EDTA chelated calcium.

[0017] Preferably, in step S4, the thickness of the gel hard shell is 0.05-0.1 mm.

[0018] In order to achieve the above object, the present invention also provides a microorganism-loaded porous additive prepared by the above preparation method.

[0019] To achieve the above objectives, the present invention also provides the use of the microbial-loaded porous additive prepared by the above preparation method in the preparation of coal mine plugging materials for crack self-repair. The specific application process is: during the stirring process of preparing the coal mine inorganic plugging material, the microbial-loaded porous additive is added in a proportion of 1-2% by external doping.

[0020] Furthermore, the adaptive gel coating material in the microbial-loaded porous additive can maintain the hydration state for a period of 24-72 hours by adjusting the ratio of nano-lignin, chitosan lactate and sodium alginate, which is consistent with the crack appearance time of the mixed coal mine inorganic plugging material.

[0021] The repair mechanism of the present invention is to utilize the organic salt respiration of Bacillus mixed bacteria to decompose complex organic calcium salts to produce carbonate and calcium ions, and use coal gangue-based zeolite as nucleation points to generate calcium carbonate crystal precipitation to carry out continuous mineralization repair of cracks.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention not only solves the problem of secondary air leakage in coal mine goaf caused by cracking of inorganic plugging materials due to water loss, but also overcomes the problem that existing microbial mineralization repair agents produce a large amount of irritating gases such as ammonia and are difficult to release microorganisms for repair at the same time as the cracks are generated. In addition, the microbial-loaded porous additive prepared by the present invention can seal and absorb a large amount of CO in the process of mineralization repair of cracks in inorganic plugging materials in coal mines. 2 , making full use of the space in the coal mine goaf is conducive to achieving the dual carbon indicators of coal mines, saving energy and reducing emissions, and has good economic benefits and engineering application prospects.

[0024] 2. The present invention creatively applies an adaptive gel coating composed of sodium alginate, chitosan lactate, and nano-lignin to microorganism-loaded coal gangue-based zeolite. The prepared microorganism-loaded porous additive exists in the form of dry spheres, wherein the inner layer of coal gangue-based zeolite skeleton can provide a suitable living environment for microorganisms, and prevent the gel from losing water and collapsing, resulting in voids inside the inorganic plugging material, affecting its mechanical properties; during the spraying and powder coating process of the outer layer of the adaptive gel coating, the gel raw material dissolves and undergoes a cross-linking reaction to form a gel cross-linked structure, which will not be affected by the loss of bound water after drying, and can be stored for a long time in a dry environment. When used, it can absorb water and recover by adding water and mixing, and re-form a water-retaining gel coating layer to wrap the coal gangue-based zeolite skeleton to ensure that the loaded microorganisms will not be separated during mixing and stirring and pipeline transportation.

[0025] 3. When the microbial-loaded porous additive of the present invention is applied to inorganic plugging materials, it is only necessary to adjust the proportion of the raw materials of the adaptive gel coating layer, so as to adjust the maintenance time of the hydration state of the adaptive gel to be consistent with the time of the appearance of cracks in the inorganic plugging materials, and mix it in the inorganic plugging materials of the coal mine in proportion and transport it to the target goaf. In a short period of time before and after the inorganic plugging materials lose water and crack, the outer layer adaptive gel of the microbial-loaded porous additive no longer maintains a hydrated state, and releases the loaded microorganisms to continuously repair the cracks in the inorganic plugging materials, thereby avoiding the problem of decreased activity due to premature release of microorganisms and low utilization rate due to difficulty in release, thereby ensuring long-term plugging of coal mine goafs. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The figure is a bar graph showing the change of the plugging efficiency of the inorganic plugging material with time before and after the addition of the microorganism-loaded porous additive prepared in Example 1;

[0027] Figure 2 The figure is a bar graph showing the change of plugging efficiency of the inorganic plugging material with time before and after adding the microorganism-loaded porous additive prepared in Example 2;

[0028] Figure 3 The figure is a bar graph showing the change of the plugging efficiency of the inorganic plugging material with time before and after the addition of the microorganism-loaded porous additive prepared in Example 3;

[0029] Figure 4 The figure is a bar graph showing the change of the plugging efficiency of the inorganic plugging material with time before and after the addition of the microorganism-loaded porous additive prepared in Example 4;

[0030] Figure 5 Response surface diagram of the effect of different components of the adaptive gel coating layer on the hydration retention time, (a) nanolignin and chitosan lactate, (b) nanolignin and sodium alginate, (c) sodium alginate and chitosan lactate. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] Example 1

[0033] A method for preparing a microorganism-loaded porous additive comprises the following steps:

[0034] S1: 5g NaOH and 6g coal gangue powder were mixed and melted at 800°C for 2h and heated in an ultrasonic water bath for 7h, washed with deionized water, and vacuum dried for 2h to obtain NaX zeolite; the coal gangue powder was prepared by high-temperature calcination at 800°C, grinding, and passing through a 200-mesh sieve;

[0035] S2: 10 g of NaX zeolite was immersed in 200 ml of Bacillus bacterial solution for 20 min under vacuum environment, and the Bacillus strain was loaded in the NaX zeolite structure to obtain microorganism-loaded coal gangue-based zeolite; the dry weight of bacteria in the Bacillus bacterial solution was measured to be 10-15 mg / ml, and 200 ml of the Bacillus bacterial solution contained 2-3 g of Bacillus, and the Bacillus bacterial solution was a mixed bacterial solution of Bacillus subtilis and Bacillus thuringiensis;

[0036] S3: drying 12 g of the microorganism-loaded coal gangue-based zeolite obtained in step S2 for 0.5 h, grinding it, and passing it through a 10-mesh sieve to obtain microorganism-loaded coal gangue-based zeolite particles;

[0037] S4: Using a composite organic calcium salt composed of 1.5g calcium lactate and 0.5g calcium acetate and 1.2g adaptive gel coating material as a coating material, wherein the adaptive gel coating material is composed of 0.09g nano-lignin, 0.66g chitosan lactate, and 0.45g sodium alginate; spraying and wetting the microorganism-loaded gangue-based zeolite particles obtained in step S3, and then placing them in an iron plate filled with the coating material, shaking the plate to coat the powder, taking it out and weighing it, and repeating the coating process for multiple times until the required weight is reached; at this time, the coating material forms a layer of gel hard shell on the surface of the microorganism-loaded gangue-based zeolite, and the microorganism-loaded porous additive is obtained by drying after being balled.

[0038] 900 g of yellow mud and 150 g of sand were mixed evenly, 450 g of water was poured in and stirred for 2 minutes, and then the microorganism-loaded porous additive was added in a proportion of 1% of the total mass to prepare a coal mine yellow mud solid slurry plugging material.

[0039] Depend on Figure 1As shown in the figure, cracks in the coal mine yellow mud-based plugging material without the addition of microbial loaded porous additives appeared within 4-24 hours after preparation. According to the results of the response surface curve experiment, the hydration state retention time of the adaptive gel-coated material composed of 0.09g nano-lignin, 0.66g chitosan lactate, and 0.45g sodium alginate was 20-22h. Therefore, the microbial loaded porous additive prepared by the material component can release microorganisms in time to repair the cracks after the coal mine yellow mud-based plugging material cracks, thereby slowing down the rate of decrease in the plugging efficiency of the plugging material.

[0040] Example 2

[0041] The preparation method of this embodiment is the same as that of Embodiment 1, except that the adaptive gel coating material in step S4 is composed of 0.08 g of nano-lignin, 0.24 g of chitosan lactate, and 0.88 g of sodium alginate.

[0042] 630 g of fly ash and 270 g of slag were mixed evenly, 15 g of NaOH, 300 g of water glass and 285 g of water were poured in and stirred for 2 minutes, and then the microorganism-loaded porous additive was added in a proportion of 1% of the total mass to prepare a coal mine fly ash-based gel plugging material.

[0043] Depend on Figure 2 As shown in the figure, cracks in the coal fly ash-based gel plugging material without the addition of microbial loaded porous additives appeared within 48-72 hours after preparation. According to the results of the response surface curve experiment, the hydration state of the adapted gel-coated material composed of 0.08g nano-lignin, 0.24g chitosan lactate, and 0.88g sodium alginate was maintained for 50-52h. Therefore, the microbial loaded porous additive prepared by the material components can release microorganisms in time to repair the cracks after the coal fly ash-based gel plugging material cracks, thereby slowing down the rate of decrease in the plugging efficiency of the plugging material.

[0044] Example 3

[0045] The preparation method of this embodiment is the same as that of Embodiment 1, except that the adaptive gel coating material in step S4 is composed of 0.08 g of nano-lignin, 0.48 g of chitosan lactate, and 0.64 g of sodium alginate.

[0046] 825g of fly ash and 75g of slag were mixed evenly, 600g of foaming liquid with a foaming agent concentration of 2% was poured into it and stirred for 2 minutes, and then the microbial loaded porous additive was added in a proportion of 1% of the total mass to prepare a coal mine sulphoaluminate cement-based quick-setting plugging material.

[0047] Depend on Figure 3As shown in the figure, cracks in the coal mine sulphoaluminate cement-based quick-setting plugging material without the addition of microbial-loaded porous additives appeared within 24-48 hours after preparation. According to the results of the response surface curve experiment, the hydration state retention time of the adaptive gel-coated material composed of 0.08g nano-lignin, 0.48g chitosan lactate, and 0.64g sodium alginate was 40-43h. Therefore, the microbial-loaded porous additive prepared by the material component can release microorganisms in time to repair the cracks after the coal mine sulphoaluminate cement-based quick-setting plugging material cracks, thereby slowing down the rate of decrease in the plugging efficiency of the plugging material.

[0048] Example 4

[0049] The preparation method of this embodiment is the same as that of Embodiment 1, and the adaptive gel coating material in step S4 is composed of 0.065 g of nano-lignin, 0.455 g of chitosan lactate, and 0.68 g of sodium alginate.

[0050] 750g of fly ash and 225g of sand were mixed evenly, 75g of concrete admixture and 675g of water were poured in and stirred for 2 minutes, and then the microorganism-loaded porous additive was added in a proportion of 1% of the total mass to prepare a coal mine foamed cement porous plugging material.

[0051] Depend on Figure 4 As shown in the figure, cracks in the porous sealing material of coal mine foamed cement without adding microbial loaded porous additives appeared within 24-48 hours after preparation. According to the results of response surface curve experiment, the hydration state of the adaptive gel coating material composed of 0.065g nano-lignin, 0.455g chitosan lactate and 0.68g sodium alginate was maintained for 45-48h. Therefore, the microbial loaded porous additive prepared by the material components can release microorganisms in time to repair the cracks of the porous sealing material of coal mine foamed cement after cracking, thereby slowing down the rate of decrease in the plugging efficiency of the plugging material.

[0052] A plugging air simulation test device is used to test the airtightness of different plugging materials after mixing with microbial-loaded porous additives. The device is mainly composed of an air compressor, a pressure regulating valve, a rotor flowmeter, a pressure gauge, and a sticker test pipe with a length of 450mm and a diameter of 200mm. Stones with a height of 250mm and a particle size of 10-30mm are laid inside the device in advance; the pressure gauge is connected to the air outlet at the bottom of the pipe. If the pressure at the air outlet at the bottom of the pipe is equal to the pressure of the pressure regulating valve, it indicates that the air tightness of the device is good and the test can be started. During the test, the plugging slurry is injected into the pipeline. When the slurry height reaches the 50mm grouting line above the stone, the grouting is stopped. The regulating valve is adjusted to the test pressure after 4h, 24h, 48h, and 72h of grouting, and the test flow rate Q is preset through the flowmeter. 1 When the pressure indicator at the bottom of the pipeline changes, read the flow meter flow rate and record it as the leakage flow rate Q2 , the plugging efficiency calculation formula is as follows.

[0053] η=(Q 1 -Q 2 ) / Q 1 ×100%

[0054] Wherein, η is the plugging efficiency, %; Q 1 is the preset flow rate, L / min; Q 2 is the air leakage flow rate, L / min.

[0055] from Figure 1-4 From the bar graph of the plugging efficiency of each embodiment and the original plugging material changing with time, it can be seen that after the addition of the microbial-loaded porous additive, the plugging efficiency of each inorganic plugging material is greatly reduced due to the change of time. This is because while the inorganic plugging materials lose water and produce cracks, the external adaptive gel coating layer of the microbial-loaded porous additive is released from the hydration state, releasing the internally loaded microorganisms to carry out continuous mineralization repair of the cracks, which greatly alleviates the problem of decreased plugging efficiency caused by water loss and rupture.

[0056] Figure 5 The influence of the three components of the adaptive gel coating material on the hydration retention time at different proportions is shown. It can be found that chitosan lactate has the least effect on the hydration retention time of the gel coating layer. When its proportion increases, the hydration retention time is shortened; sodium alginate and nano-lignin interact with each other. When the proportion of nano-lignin is large, the sodium alginate content is proportional to the hydration retention time. When the proportion of nano-lignin is relatively reduced, the sodium alginate content is inversely proportional to the hydration retention time; the influence of nano-lignin on the hydration retention time is the same as that of sodium alginate.

[0057] The above test results show that the microorganism-loaded porous additive of the present invention has a relatively simple manufacturing process and can self-repair cracks in various inorganic plugging materials for mining, ensuring long-term sealing of coal mine goafs; at the same time, the adaptive gel coating layer can release loaded microorganisms in time for repair, thereby improving the utilization efficiency and utilization time of microorganisms. In addition, the present invention can not only improve the sealing performance of coal mine plugging materials, but also seal carbon dioxide underground in mining areas.

Claims

1. A method for preparing a microorganism-loaded porous additive, characterized in that: The following steps are involved: S1: NaOH and coal gangue powder are mixed and melted at 600-800°C for 1-2 hours and heated in an ultrasonic water bath for 5-8 hours, washed with deionized water, and vacuum dried for 1-2 hours to obtain NaX zeolite. S2: soaking the NaX zeolite in a Bacillus bacterial solution for 20-30 minutes under a vacuum environment, loading the Bacillus bacteria into the NaX zeolite structure to obtain a microorganism-loaded coal gangue-based zeolite; S3: drying the microorganism-loaded coal gangue-based zeolite obtained in step S2 for 0.25-0.5h, grinding it, and passing it through a 7-16 mesh sieve to obtain microorganism-loaded coal gangue-based zeolite particles; S4: using composite organic calcium salt and adaptive gel coating material as powder coating material, wherein the adaptive gel coating material is composed of nano-lignin, chitosan lactate and sodium alginate in a mass ratio of 1:(3-8):(5-11); coating and granulating the microorganism-loaded gangue-based zeolite particles obtained in step S3 by spraying and wetting, and the powder coating material forms a gel hard shell on the surface of the microorganism-loaded gangue-based zeolite particles, and drying after balling to obtain the microorganism-loaded porous additive.

2. The method for preparing a microorganism-loaded porous additive according to claim 1, characterized in that: In step S1, the mass ratio of the NaOH to the coal gangue powder is 1:(1-1.25); the coal gangue powder is prepared by calcining at a high temperature above 800°C, grinding, and passing through a 120-200 mesh sieve.

3. The method for preparing a microorganism-loaded porous additive according to claim 1 or 2, characterized in that: In step S2, the mass ratio of the microorganism to the gangue-based zeolite is 1:(3-7).

4. A microorganism-loaded porous additive according to claim 1 or 2, characterized in that: In step S2, the Bacillus bacterial liquid is a mixed bacterial liquid, including at least two of Bacillus pasteurianus, Bacillus subtilis, Bacillus cohnii, Bacillus alkali, Bacillus halophilus, Bacillus thuringiensis and the like.

5. The method for preparing a microorganism-loaded porous additive according to claim 1 or 2, characterized in that: In step S4, the mass ratio between the adaptive gel coating material and the composite organic calcium salt is 1:(1.5-3); the mass ratio between the powder coating material and the microorganism-loaded coal gangue-based zeolite particles is 1:(3-6).

6. The microbial-loaded porous additive for self-repair of cracks in coal mine plugging materials according to claim 1 or 2, characterized in that: The composite organic calcium salt includes at least two of calcium acetate, calcium lactate, sugar alcohol calcium or EDTA chelated calcium.

7. The method for preparing a microorganism-loaded porous additive according to claim 1, characterized in that: In step S4, the thickness of the water-soluble hard shell is 0.05-0.1 mm.

8. A microorganism-loaded porous additive prepared by the preparation method according to any one of claims 1 to 7.

9. The use of the microbial-loaded porous additive as claimed in claim 8 in the preparation of coal mine plugging materials for crack self-repair, wherein the specific application process is: during the stirring process of preparing the coal mine inorganic plugging material, the microbial-loaded porous additive is added in a proportion of 1-2% by external doping.

10. Use of the microorganism-loaded porous additive according to claim 9 in preparing a coal mine plugging material for crack self-repairing, characterized in that: The adaptive gel coating material in the microbial loaded porous additive can maintain the hydration state for a time within the range of 24-72 hours by adjusting the ratio of nano-lignin, chitosan lactate and sodium alginate, which is consistent with the crack appearance time of the mixed coal mine inorganic plugging material.