Modified fly ash foam stabilizer as well as preparation method and application thereof
Through the grinding of modified fly ash foam stabilizer and sonication of acetic acid, the stability and cost problems of traditional foam stabilizer are solved, the stability of foam materials is improved and the efficient utilization of industrial waste is achieved, the production process is simplified and the production process is reduced. The cost.
Patent Information
- Application Number
- CN202410991825.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing foam stabilizer has shortcomings in terms of stability and production costs, and the treatment process of traditional fly ash is complicated, making it difficult to achieve efficient recycling of industrial waste.
By grinding and sieving fly ash, combined with acetic acid ultrasonic treatment, an ultrafine fly ash foam stabilizer is prepared for improving the stability of foam materials and used in the fields of building materials, petroleum industry, etc.
It has achieved the improvement of the stability of foam materials, simplified production processes, reduced costs, promoted the high-value utilization of industrial waste, and has environmental protection and economic benefits.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource utilization of industrial solid wastes, in particular to a modified fly ash foam stabilizer and a preparation method and application thereof. Background Art
[0002] With the widespread application of foam technology in many fields, such as building materials, cosmetics, food industry, pharmaceutical manufacturing and mineral processing, the requirements for the stability and performance of foam are increasing. Foam materials, including but not limited to foam concrete, foam plastics, foam metals, food foaming agents and foam formulas in cosmetics, need to maintain a stable foam structure from preparation to final application or consumption to ensure their excellent physical properties, processing performance and use effects. In this context, the importance of foam stabilizers (foam stabilizers) as key additives has become increasingly prominent.
[0003] Traditional foam stabilizers are mainly divided into three categories: synergistic, thickening and nano solid particles. Each type has its own unique advantages and limitations. Although synergistic foam stabilizers can improve foam stability through multiple mechanisms, their effects are often limited when used alone, and they often need to be combined with other types of foam stabilizers to enhance the effect; thickening foam stabilizers stabilize foam by increasing liquid viscosity, but they have the disadvantages of easy agglomeration of raw materials, complex processing and possible impact on product transparency; nano solid particles show good foam stabilization effects with their unique surface properties and nano effects, but the high production cost and usage restrictions limit their wide application.
[0004] In view of the above challenges, exploring low-cost, efficient and environmentally friendly new foam stabilizers has become a research hotspot. Fly ash, as an industrial byproduct produced in large quantities in thermal power plants, not only has a huge stock, but also has good physical and chemical properties. Its low price and potential environmentally friendly properties make it an ideal building material modifier.
[0005] Therefore, developing a method for modifying fly ash to enhance its foam stability in various application scenarios can not only improve the overall performance of foam products, but also achieve high-value utilization of industrial waste, which has important environmental and economic significance. Summary of the invention
[0006] In order to address the deficiencies in the prior art, the present invention provides a modified fly ash foam stabilizer and a preparation method and application thereof, aiming to develop a new type of foam stabilizer with low cost, significant effect and environmental friendliness through modified fly ash technology, which not only solves the problems of poor foam stabilizing performance, complex treatment process and high production cost of traditional foam stabilizers, but also promotes the recycling of industrial waste, and has important economic and environmental value.
[0007] Specifically, the present invention provides a modified fly ash foam stabilizer, which is composed of the following components by mass percentage:
[0008] Ultrafine fly ash 0.5%~1.0%, acetic acid 0.25‰~0.75‰, the balance is water;
[0009] The particle size of the ultrafine fly ash is less than 45 μm.
[0010] In some specific embodiments of the present invention, the modified fly ash foam stabilizer preparation method comprises the following preparation steps: grinding and sieving fly ash to obtain ultrafine fly ash, then mixing the ultrafine fly ash with acetic acid and water, ultrasonicating the acetic acid, and then filtering and drying to obtain the modified fly ash foam stabilizer;
[0011] The mass percentages of the ultrafine fly ash, acetic acid and water are as follows: 0.5% to 1.0% ultrafine fly ash, 0.25‰ to 0.75‰ acetic acid, and the balance water;
[0012] The particle size of the ultrafine fly ash is less than 45 μm.
[0013] In some specific embodiments of the present invention, the specific method for grinding and screening the fly ash is: using a ball mill to grind the fly ash for 15 minutes to 25 minutes; then screening the ground fly ash using a 325-mesh standard sieve to obtain ultrafine fly ash.
[0014] In some specific embodiments of the present invention, the ultrasonic frequency of the acetic acid ultrasound is 60 to 120 KHz, and the acetic acid ultrasound time is 10 min to 30 min.
[0015] In some specific embodiments of the present invention, the specific method of filtration and drying is: the fly ash after ultrasonic treatment with acetic acid is filtered through a vacuum filter for 15 minutes to 30 minutes, and placed in a 120° C. oven for drying for 1 hour to 2 hours.
[0016] The present invention also provides a method for preparing a modified fly ash foam stabilizer, comprising the following preparation steps: grinding and sieving fly ash to obtain ultrafine fly ash, then mixing the ultrafine fly ash with acetic acid and water, subjecting the ultrafine fly ash to ultrasonic treatment of acetic acid, and then filtering and drying to finally obtain the modified fly ash foam stabilizer.
[0017] In some specific embodiments of the present invention, the specific method for grinding and screening the fly ash is: using a ball mill to grind the fly ash for 15 minutes to 25 minutes; then screening the ground fly ash using a 325-mesh standard sieve to obtain ultrafine fly ash.
[0018] In some specific embodiments of the present invention, the ultrasonic frequency of the acetic acid ultrasound is 60 to 120 KHz, and the acetic acid ultrasound time is 10 min to 30 min.
[0019] In some specific embodiments of the present invention, the specific method of filtration and drying is: the fly ash after ultrasonic treatment with acetic acid is filtered through a vacuum filter for 15 minutes to 30 minutes, and placed in a 120° C. oven for drying for 1 hour to 2 hours.
[0020] The present invention also provides the use of any of the modified fly ash foam stabilizers described above or the modified fly ash foam stabilizers prepared by any of the preparation methods described above in building materials, petroleum industry, mineral processing, chemical foaming and environmental engineering.
[0021] In some specific embodiments of the present invention, the modified fly ash foam stabilizer described in any one of the above or the modified fly ash foam stabilizer prepared by any one of the above preparation methods can be used as a building material for preparing foamed concrete; it can also be used in drilling fluids in the petroleum industry to improve the stability and lubrication properties of mud; it can also be used as a flotation agent in mineral processing to improve the recovery rate and purity of minerals; it can also be used to control the size and uniformity of foam in chemical foaming. In addition, it can also be used in environmental engineering fields such as sewage treatment and waste gas treatment as an adsorbent and stabilizer.
[0022] Compared with the prior art, the present invention has the following significant advantages and effects:
[0023] First, the prepared foam stabilizer can be directly added to the foaming liquid, which is simple and quick to operate, without the need for complicated pretreatment steps, greatly improving production efficiency. Secondly, after sufficient mixing and physical foaming, the obtained foam exhibits extremely excellent foam stabilization performance, significantly improving the quality and stability of the product. Furthermore, the entire preparation process is simple and easy, which not only reduces labor and time costs, but also reduces energy consumption, meeting the requirements of energy conservation and environmental protection.
[0024] In addition, by using fly ash as the main raw material for modification, high-value utilization of industrial waste is achieved, the pressure on the environment is reduced, and a positive contribution is made to sustainable development. DETAILED DESCRIPTION
[0025] In conjunction with specific embodiments, the present invention will be further described. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the application.
[0026] Example 1
[0027] Weigh the following raw materials by weight: ordinary fly ash: water = 120:20000, mix thoroughly, add 50 parts of foaming agent to prepare bubbles; then test the water secretion and sedimentation distance of the bubbles. In this example, the water secretion of the bubbles prepared in 1 hour is 78-93 mL, and the sedimentation distance is 9-14 mm.
[0028] Example 2
[0029] Weigh the following raw materials: ordinary fly ash: water = 120: 20000, grind the fly ash for 20 minutes, mix it with water, and then add 50 parts of foaming agent to prepare bubbles; then test the water secretion and sedimentation distance of the bubbles. In this example, the water secretion of the bubbles prepared in 1 hour is 76-86 mL, and the sedimentation distance is 8.5-12 mm.
[0030] Example 3
[0031] The fly ash was ground for 20 minutes, and then sieved with a 325-mesh standard sieve to obtain ultrafine fly ash. The following raw materials were weighed, ultrafine fly ash: water = 120: 20000, and then the ultrafine fly ash was mixed with water, and 50 parts of a foaming agent were added after sufficient mixing to prepare bubbles; and then the water secretion and sedimentation distance of the bubbles were tested. In this embodiment, the water secretion of the bubbles prepared in 1 hour was 72-83 mL, and the sedimentation distance was 8-11 mm.
[0032] Example 4
[0033] The fly ash was ground for 20 minutes, and then sieved with a 325-mesh standard sieve to obtain ultrafine fly ash. The following raw materials were weighed, ultrafine fly ash: acetic acid: water = 120:10:20000, and 50 parts of foaming agent were added after being fully mixed, filtered and dried to prepare bubbles; and then the water secretion and sedimentation distance of the bubbles were tested. In this embodiment, the water secretion of the bubbles prepared in 1 hour was 50-62 mL, and the sedimentation distance was 6-7.5 mm.
[0034] Example 5
[0035] Grind the fly ash for 20 minutes, then use a 325 mesh standard sieve to sieve and process to obtain ultrafine fly ash, then weigh the following raw materials, ultrafine fly ash: acetic acid: water = 120:10:20000, after fully mixing, ultrasonic treatment with acetic acid (frequency 60KHz) for 20 minutes, filtering and drying, add 50 parts of foaming agent to prepare bubbles; then test the water secretion and sedimentation distance of the bubbles. The water secretion of the bubbles prepared in this embodiment is 42-56mL for 1h, and the sedimentation distance is 4.5-6.5mm. The 7d strength of the foamed concrete prepared in this embodiment using a foam stabilizer is 20%-40% higher than that of Comparative Example 1.
[0036] Example 6
[0037] Grind the fly ash for 20 minutes, then use a 325 mesh standard sieve to sieve to obtain ultrafine fly ash, then weigh the following raw materials, ultrafine fly ash: acetic acid: water = 120:10:20000, after fully mixing, ultrasonic treatment with acetic acid (frequency 120KHz) for 20 minutes, filtering and drying, add 50 parts of foaming agent to prepare bubbles; then test the bubble exudation and sedimentation distance. The bubble exudation in this embodiment is 30-36mL for 1h, and the sedimentation distance is 2.5-4mm. The 7d strength of the foamed concrete prepared by the foam stabilizer in this embodiment is 60%-70% higher than that of Comparative Example 1. The raw material cost is 15%-20% of that of Comparative Example 4.
[0038] Comparative Examples 1 to 4
[0039] Comparative Example 1:
[0040] 50 parts of foaming agent and 2000 parts of water are directly mixed fully, and the bubbles of comparative example 1 can be prepared by physical foaming method. The bubbles of comparative example 1 are prepared with a water secretion of 68-95 mL in 1 hour and a sedimentation distance of 8.5-11.5 mm.
[0041] Comparative Example 2:
[0042] 10-50 parts of calcium stearate (synergistic type) foam stabilizer was added to Comparative Example 1 to obtain bubbles prepared in Comparative Example 2. The bubbles prepared in Comparative Example 2 had a water secretion of 64-82 mL in 1 hour and a sedimentation distance of 7.5-9.5 mm.
[0043] Comparative Example 3:
[0044] 10-50 parts of xanthan gum (viscosity-enhancing) foam stabilizer are added to Comparative Example 1 to obtain bubbles prepared in Comparative Example 3. The bubbles prepared in Comparative Example 3 have a water secretion of 52-64 mL in 1 hour and a sedimentation distance of 5-8 mm.
[0045] Comparative Example 4:
[0046] 10-50 parts of nano-silicon dioxide were added to Comparative Example 1, and the bubbles were prepared by magnetic stirring, acetic acid ultrasonic treatment and other steps to obtain the bubbles prepared by Comparative Example 4. The water secretion of the bubbles prepared by Comparative Example 4 was 57-64 mL for 1 hour, and the sedimentation distance was 5-7.5 mm.
[0047] The test results show that, compared with the comparative example, the embodiment has the effect of improving the stability of bubbles and thus improving the strength of foamed concrete, avoiding the collapse of foam in concrete before initial setting, and has a cost advantage.
[0048] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A modified fly ash foam stabilizer, characterized in that: The modified fly ash foam stabilizer is composed of the following components by mass percentage: Ultrafine fly ash 0.5%~1.0%, acetic acid 0.25‰~0.75‰, the balance is water; The particle size of the ultrafine fly ash is less than 45 μm.
2. The modified fly ash foam stabilizer according to claim 1, characterized in that: The modified fly ash foam stabilizer preparation method comprises the following preparation steps: grinding and sieving fly ash to obtain ultrafine fly ash, then mixing the ultrafine fly ash with acetic acid and water, performing acetic acid ultrasonic treatment, and then performing suction filtration and drying treatment to finally obtain the modified fly ash foam stabilizer.
3. The modified fly ash foam stabilizer according to claim 2, characterized in that: The specific method of grinding and screening the fly ash is: using a ball mill to grind the fly ash for 15 minutes to 25 minutes; then screening the ground fly ash using a 325-mesh standard sieve to obtain ultrafine fly ash.
4. The modified fly ash foam stabilizer according to claim 2, characterized in that: The ultrasonic frequency of the acetic acid ultrasound is 60 to 120 KHz, and the acetic acid ultrasound time is 10 min to 30 min.
5. The modified fly ash foam stabilizer according to any one of claims 2 to 4, characterized in that: The specific method of the filtration and drying is as follows: the fly ash after ultrasonic treatment with acetic acid is filtered through a vacuum filter for 15 minutes to 30 minutes, and then placed in a 120° C. oven for drying for 1 hour to 2 hours.
6. A method for preparing a modified fly ash foam stabilizer, characterized in that: The method comprises the following preparation steps: grinding and sieving fly ash to obtain ultrafine fly ash, then mixing the ultrafine fly ash with acetic acid and water, subjecting the ultrafine fly ash to ultrasonic treatment with acetic acid, and then filtering and drying the mixture to obtain a modified fly ash foam stabilizer. The mass percentages of the ultrafine fly ash, acetic acid and water are as follows: 0.5% to 1.0% ultrafine fly ash, 0.25‰ to 0.75‰ acetic acid, and the balance water; The particle size of the ultrafine fly ash is less than 45 μm.
7. The method for preparing the modified fly ash foam stabilizer according to claim 6, characterized in that: The specific method of grinding and screening the fly ash is: using a ball mill to grind the fly ash for 15 minutes to 25 minutes; then screening the ground fly ash using a 325-mesh standard sieve to obtain ultrafine fly ash.
8. The method for preparing the modified fly ash foam stabilizer according to claim 6, characterized in that: The ultrasonic frequency of the acetic acid ultrasound is 60 to 120 KHz, and the acetic acid ultrasound time is 10 min to 30 min.
9. The method for preparing the modified fly ash foam stabilizer according to any one of claims 6 to 8, characterized in that: The specific method of the filtration and drying is as follows: the fly ash after ultrasonic treatment with acetic acid is filtered through a vacuum filter for 15 minutes to 30 minutes, and then placed in a 120° C. oven for drying for 1 hour to 2 hours.
10. Use of the modified fly ash foam stabilizer according to any one of claims 1 to 5 or the modified fly ash foam stabilizer prepared by the preparation method according to any one of claims 6 to 9 in building materials, petroleum industry, mineral processing, chemical foaming and environmental engineering.
Citation Information
Patent Citations
Technology for coal ash fibre surface treatment and use of asphalt reinforcing modification thereof
CN101250032A
Powdery acid leaching modified white soot compound lead salt stabilizer and preparation method thereof
CN108004413A
Novel foam stabilizer and preparation method thereof
CN112175600A
Preparation and application of fly ash@loofah sponge three-dimensional reticular porous composite material
CN112871143A
Porous fly ash modified foam concrete as well as preparation method and application thereof
CN116477967A
Cited By
A foam stabilizer based on graded modification of enteromorpha and a preparation method and application thereof
CN121343578B