Impurity-containing crude oil demulsifier and preparation method thereof
Through the reaction of polyols and epoxychlorohydrin and other materials, a heterocrude oil-containing deemulsion agent is prepared, which solves the problem of difficult treatment of polymer crude oil deemulsion in the prior art, and achieves efficient flocculation and demulsification The results have improved the oil field recovery rate and resource recovery efficiency.
Patent Information
- Application Number
- CN202411353124.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-26
AI Technical Summary
The prior art is difficult to effectively treat crude oil deemulsion containing polymers, resulting in difficulty in separation of oil and water and challenges in resource recycling, and conventional deemulsion agents have limited effects.
Polyols and epoxychlorohydrin reacted under Lewis acid catalyzed to obtain terminal hydroxychloropolymer polyether, and amination and etherification reaction with alcohol amine and sodium alkoxide to obtain amine alkoxy polyether, and after crosslinking, it is used to obtain phenolic aldehydes. The amine resin polyether is compounded to form a heterocrude-containing deemulsifier with rich polar amine structures to achieve flocculation-coalization effect.
This method not only has good demulsification effect, but also allows water droplets to flocculate, simplifies the process of demulsification of crude oil, improves the efficiency of oil purification and water purification, saves energy, and improves economic benefits and equipment processing rate.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oilfield demulsifiers, and in particular to a demulsifier for impure crude oil and a preparation method thereof. Background Art
[0002] With the continuous development of oil fields, major oil fields are gradually aging. In order to improve the recovery rate of crude oil, relevant personnel have given different methods. Among them, chemical flooding technology, as one of the most promising ways to improve the recovery rate, is widely used in oil field recovery. Chemical flooding includes polymer flooding, alkaline water flooding, surfactant flooding, etc., which improves the recovery rate by changing the fluid properties or increasing the contact area between the fluid and the rock and crude oil. However, due to the large-scale use of new polymers and surfactants, polymers inevitably appear in some crude oil production fluids. The presence of residual polymers in crude oil leads to enhanced stability of oil-water emulsions, difficulty in oil-water separation, and many other problems such as increased emulsified oil and high impurity content in purified oil, which brings great damage and burden to the formation and gathering and transportation system, and then makes the subsequent crude oil demulsification and resource recovery face new challenges. Conventional demulsifiers are difficult to handle such production fluids.
[0003] The patent with the publication number CN114736337B, entitled a demulsifier, its preparation method and its application, discloses a demulsifier, which is a copolymer of vinyl-containing aromatic hydrocarbons, long-chain α-olefins and allyl alcohol polyethers. The copolymer is used as the main agent of the heavy oil pretreatment agent, and has good compatibility with the colloid asphaltene of the heavy oil, and has a good demulsification effect on the stubborn emulsion formed by the colloid asphaltene and sludge in the heavy oil. Anionic surfactants such as dodecylbenzene sulfonic acid can play a role in dispersing the sludge emulsion, which is beneficial for the copolymer demulsifier to play a better role, but the above technical solution has a limited effect on the demulsification of crude oil containing polymers.
[0004] Therefore, it is necessary to provide a crude oil demulsifier containing impurities and a preparation method thereof to solve the problems existing in the above-mentioned prior art. Summary of the invention
[0005] In view of this, the present invention provides a crude oil demulsifier containing impurities and a preparation method thereof, so as to achieve the purpose of achieving good demulsification effect on crude oil containing impurities.
[0006] To achieve the above object, the present invention provides a method for preparing a crude oil demulsifier containing impurities, comprising the following steps: S1, polyol and epichlorohydrin react under Lewis acid catalysis to obtain hydroxyl-terminated chloropolyether, and the hydroxyl-terminated chloropolyether is partially aminized with alcoholamine in an organic solvent to obtain aminochloropolyether; S2, subjecting the aminochloropolyether to an etherification reaction with sodium alcoholate to obtain an aminoalkoxypolyether, and further reacting the aminoalkoxypolyether with an aliphatic or alicyclic diisocyanate to obtain a cross-linked polyether; S3, compounding the cross-linked polyether with the phenolic amine resin polyether to obtain a crude oil demulsifier containing impurities.
[0007] In the technical scheme provided by the present invention, a product obtained by ring-opening of polyol and epichlorohydrin is gradually subjected to amination and etherification reactions with alcoholamine and sodium alcoholate to obtain aminoalkoxy polyether, which is compounded with phenolic amine resin polyether after cross-linking. The obtained demulsifier has rich polar amino structure, and can achieve flocculation-agglomeration effect by combining various raw materials, and flocculate impurities in crude oil, which not only has good demulsification effect and flocculates water droplets, but also facilitates the subsequent removal of impurities from crude oil.
[0008] Optionally, the conditions for synthesizing the terminal hydroxyl chlorinated polyether are a temperature of 50-60° C. and a time of 2-8 h; and the conditions for synthesizing the amino chlorinated polyether are a temperature of 50-100° C. and a time of 2-8 h.
[0009] Optionally, the molar ratio of the polyol to epichlorohydrin is 1:9-30; the mass of the Lewis acid is 0.1-0.8% of the mass of the epichlorohydrin; and the mass ratio of the alcohol amine: the terminal hydroxyl chlorinated polyether: the organic solvent is 0.1-0.6:1:1-3.
[0010] Optionally, the polyol is glycerol or trimethylolpropane; the Lewis acid is one of triisobutylaluminum, aluminum trichloride, boron trifluoride ether and phosphoric acid; the ethanolamine is monoethanolamine or isopropanolamine; and the organic solvent is xylene or S-1500 solvent oil.
[0011] Optionally, the synthesis conditions of the aminoalkoxy polyether are a temperature of 50-100°C and a time of 2-8 hours; the synthesis conditions of the cross-linked polyether are 40-60°C and a time of 2-8 hours, and the compounding conditions are a temperature of 40-50°C and a time of 3-4 hours.
[0012] Optionally, the mass of the aliphatic or alicyclic diisocyanate is 0.5-5% of the mass of the terminal hydroxyl chloropolyether, and the mass of the sodium alkoxide is 10-60% of the mass of the terminal hydroxyl chloropolyether.
[0013] Optionally, the aliphatic or alicyclic diisocyanate includes one or a combination of two or more of isophorone diisocyanate, methylcyclohexane diisocyanate and trimethylhexamethylene diisocyanate, and the sodium alkoxide is sodium methoxide or sodium ethoxide.
[0014] Optionally, the mass ratio of the cross-linked polyether to the phenolic amine resin polyether in S3 is 1:1-3.
[0015] Optionally, the epichlorohydrin, the olamine, the sodium alkoxide and the aliphatic or alicyclic diisocyanate are added dropwise; the aliphatic or alicyclic diisocyanate is dissolved in xylene and added dropwise to the aminoalkoxy polyether.
[0016] In order to achieve the above object, the present invention also provides a crude oil demulsifier containing impurities obtained by the above preparation method.
[0017] The above technical solution of the present invention includes at least the following beneficial effects: In the technical scheme provided by the present invention, a product obtained by ring-opening of polyol and epichlorohydrin is gradually subjected to amination and etherification reactions with alcoholamine and sodium alcoholate to obtain aminoalkoxy polyether, which is compounded with phenolic amine resin polyether after cross-linking. The obtained demulsifier has rich polar amino structure, and can achieve flocculation-agglomeration effect by combining various raw materials, and flocculate impurities in crude oil, which not only has good demulsification effect and flocculates water droplets, but also facilitates the subsequent removal of impurities from crude oil, realizes rapid demulsification, clean oil and clear water, saves energy, and improves economic benefits and equipment treatment rate. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0019] The phenalkamine resin polyether used in the embodiment of the present invention is a conventional phenalkamine resin polyether, which can be purchased or synthesized. One of the synthesis methods is provided below: Synthesis of Phenolic Amine Resin Polyether (DPA): 292.5Kg of polyethylene polyamine (n=2) and 114.2Kg of bisphenol A were put into the reactor, heated to 40~50℃, and 164.6Kg of formaldehyde (36.5%) solution was added dropwise. The addition was completed in 2 hours, and the temperature was kept for 3 hours. The phenol-formaldehyde amine resin (DP) of 535KG was obtained at a vacuum degree of 0.085~0.095Mpa and 100-110℃ for about 3 hours, and the temperature was lowered to 80℃ for standby use. 430.7Kg of phenol-formaldehyde amine resin (DP) was put into the autoclave, 1.5Kg of potassium hydroxide was added, and the phenol-formaldehyde amine resin (DP) was dehydrated for half an hour at 100-110℃, and the temperature was raised to 130~150℃, and 580Kg of propylene oxide was introduced. The reaction was complete, and 330Kg of ethylene oxide was introduced. The reaction was complete, and the phenol-formaldehyde amine resin polyether (DPA) was obtained. The temperature was lowered to below 80℃, and the material was discharged for standby use.
[0020] Example 1 92 kg of propylene glycol and 5 kg of boron trifluoride ether were added into a reactor, heated to 50 ° C, 925 kg of epichlorohydrin was added dropwise, the addition was completed within 3 hours, and the reaction was continued for 4 hours to obtain terminal hydroxyl chloropolyether, namely intermediate A, which was cooled to below 80 ° C, discharged and set aside; 500 kg of intermediate A and 500 kg of xylene were added into a reactor, heated to 100 ° C, 100 kg of monoethanolamine was added dropwise, the addition was completed within 2 hours, and the reaction was continued for 3 hours to obtain amino chloropolyether, namely intermediate B, which was cooled to below 80 ° C, and discharged; 1100 kg of intermediate B was added into a reactor, heated to 100 ° C, 80 kg sodium methoxide, add it dropwise in 2 hours, continue to react for 5 hours, obtain amino alkoxy polyether, namely intermediate C, cool it to below 80°C, and discharge it; put 1100Kg intermediate C into the reactor, heat it to 40°C, add 5Kg trimethylhexamethylene diisocyanate (dissolved in 20Kg xylene) dropwise in 2 hours, continue to react for 3 hours, obtain cross-linked polyether, namely intermediate D, cool it to below 50°C, and discharge it; put 1100Kg intermediate D into the reactor, heat it to 40°C, pump in 2000Kg phenolic amine resin polyether (DPA) in 2 hours, continue to stir for 2 hours, obtain a demulsifier containing impure crude oil, and discharge it.
[0021] Example 2 92 kg of trimethylolpropane and 2.8 kg of triisobutylaluminum were added into a reactor, heated to 60°C, 2775 kg of epichlorohydrin was added dropwise, the addition was completed within 3 hours, and the reaction was continued for 5 hours to obtain terminal hydroxyl chloropolyether, namely intermediate A, which was cooled to below 80°C, discharged and set aside; 600 kg of intermediate A and 1800 kg of S-1500 solvent oil were added into a reactor, heated to 50°C, 60 kg of isopropanolamine was added dropwise, the addition was completed within 2 hours, and the reaction was continued for 5 hours to obtain amino chloropolyether, namely intermediate B, which was cooled to below 80°C and discharged; 1200 kg of intermediate B was added into a reactor, heated to 50°C , add 360kg of sodium ethoxide dropwise, add it dropwise within 2 hours, continue to react for 3 hours, obtain amino alkoxy polyether, namely intermediate C, cool it to below 80°C, and discharge it; put 1200kg of intermediate C into the reactor, heat it to 60°C, add 30kg of isophorone diisocyanate (dissolved in 20kg of xylene) dropwise within 2 hours, continue to react for 5 hours, obtain cross-linked polyether, namely intermediate D, cool it to below 50°C, and discharge it; put 1200kg of intermediate D into the reactor, heat it to 50°C, pump in 1200kg of phenolic amine resin polyether (DPA) within 2 hours, continue to stir for 1 hour, obtain a demulsifier containing impure crude oil, and discharge it.
[0022] Example 3 92 kg of glycerol and 14.8 kg of aluminum chloride were added to a reactor, heated to 55 ° C, 1850 kg of epichlorohydrin was added dropwise, the addition was completed within 3 hours, and the reaction was continued for 3 hours to obtain terminal hydroxyl chloropolyether, namely intermediate A, which was cooled to below 80 ° C, discharged and set aside; 400 kg of intermediate A and 1200 kg of xylene were added to a reactor, heated to 80 ° C, 240 kg of isopropanolamine was added dropwise, the addition was completed within 2 hours, and the reaction was continued for 4 hours to obtain amino chloropolyether, namely intermediate B, which was cooled to below 80 ° C, and discharged; 1000 kg of intermediate B was added to a reactor, heated to 90 ° C, 400 kg of intermediate B was added dropwise, and the addition was completed within 2 hours. kg sodium ethoxide, add it dropwise in 2 hours, continue to react for 4 hours to obtain amino alkoxy polyether, namely intermediate C, cool it to below 80°C, and discharge it; put 1000Kg of intermediate C into the reactor, heat it to 50°C, add 2Kg of methyl cyclohexane diisocyanate (dissolved in 20Kg of xylene) dropwise in 2 hours, continue to react for 4 hours to obtain cross-linked polyether, namely intermediate D, cool it to below 50°C, and discharge it; put 1000Kg of intermediate D into the reactor, heat it to 45°C, pump in 3000Kg of phenolic amine resin polyether (DPA) in 2 hours, continue stirring for 1.5 hours to obtain a demulsifier containing impure crude oil, and discharge it.
[0023] Example 4 Compared with Example 1, the only difference is that the aliphatic or alicyclic diisocyanate in Example 4 is 2.5 kg of isophorone diisocyanate and 2.5 kg of methylcyclohexane diisocyanate. The rest of the raw materials and steps are the same as in Example 1.
[0024] Comparative Example 1 It is a modified phenolic amine polyoxypropylene polyoxyethylene resin demulsifier commonly used in the industry in the prior art.
[0025] The demulsifiers of Examples 1 to 4 and Comparative Example 1 were tested for relevant properties. The demulsifier of the present invention was subjected to a demulsification experiment on crude oil containing impurities in a certain oil field in Northwest China at a temperature of 45-55° C. The determination method and reagents of the bottle test method refer to the petroleum and natural gas industry standard SY / T 5281-2000 of the People's Republic of China "Crude Oil Demulsifier Performance Detection Method (Bottle Test Method)"; Test conditions: 50° C., 50 ml oil content, 100 mg / l demulsifier addition, and manual mixing for 100 times.
[0026] The physical properties of the impure oil are as follows: oil sample density (density bottle method): 0.9254 g / ml (20°C); oil sample water content (distillation method): 54%; organic impurity content: 7.4%; the results are shown in Table 1.
[0027] Table 1 Performance test table of Examples 1 to 4 and Comparative Example 1
[0028] It can be seen from Table 1 that the demulsifiers prepared in Examples 1 to 4 of the present invention perform better than those in Comparative Example 1 in terms of demulsification effect and dehydration rate.
[0029] After using the demulsifier of comparative example 1, there is a slight emulsified layer on the oil-water interface, while after using the demulsifiers prepared by embodiments 1 to 4 of the present invention, there is no emulsified layer. It can be seen that the demulsifier provided by the present invention is better than comparative example 1 in terms of demulsification effect.
[0030] Combined with the fact that the inorganic content in the sediment after using the demulsifier of Comparative Example 1 is much lower than the inorganic content in the sediment after using the demulsifier prepared by Examples 1 to 4, it can be seen that the demulsifier prepared by the present invention performs better in demulsifying and removing impurities for inorganic polymers.
[0031] The above are preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for preparing a crude oil demulsifier containing impurities, characterized in that: The following steps are involved: S1, polyol and epichlorohydrin react under Lewis acid catalysis to obtain hydroxyl-terminated chloropolyether, and the hydroxyl-terminated chloropolyether is partially aminized with alcoholamine in an organic solvent to obtain aminochloropolyether; S2, subjecting the aminochloropolyether to an etherification reaction with sodium alcoholate to obtain an aminoalkoxypolyether, and further reacting the aminoalkoxypolyether with an aliphatic or alicyclic diisocyanate to obtain a cross-linked polyether; S3, compounding the cross-linked polyether with the phenolic amine resin polyether to obtain a crude oil demulsifier containing impurities.
2. The method for preparing a crude oil demulsifier according to claim 1, characterized in that: The conditions for synthesizing the terminal hydroxyl chlorinated polyether are a temperature of 50-60° C. and a time of 2-8 hours; the conditions for synthesizing the amino chlorinated polyether are a temperature of 50-100° C. and a time of 2-8 hours.
3. The method for preparing a crude oil demulsifier according to claim 1, characterized in that: The molar ratio of the polyol to epichlorohydrin is 1:9-30; the mass of the Lewis acid is 0.1-0.8% of the mass of the epichlorohydrin; and the mass ratio of the alcohol amine: the terminal hydroxyl chlorinated polyether: the organic solvent is 0.1-0.6:1:1-3.
4. The method for preparing a demulsifier containing impure crude oil according to claim 3, characterized in that: The polyol is glycerol or trimethylolpropane; the Lewis acid is one of triisobutylaluminum, aluminum trichloride, boron trifluoride ether and phosphoric acid; the alcohol amine is monoethanolamine or isopropanolamine; and the organic solvent is xylene or S-1500 solvent oil.
5. The method for preparing a demulsifier containing impure crude oil according to claim 1, characterized in that: The synthesis conditions of the aminoalkoxy polyether are 50-100°C and 2-8h; the synthesis conditions of the cross-linked polyether are 40-60°C and 2-8h, and the compounding conditions are 40-50°C and 3-4h.
6. The method for preparing a demulsifier containing impure crude oil according to claim 1, characterized in that: The mass of the aliphatic or alicyclic diisocyanate is 0.5-5% of the mass of the terminal hydroxyl chloropolyether, and the mass of the sodium alkoxide is 10-60% of the mass of the terminal hydroxyl chloropolyether.
7. The method for preparing a demulsifier containing impure crude oil according to claim 6, characterized in that: The aliphatic or alicyclic diisocyanate includes one or a combination of two or more of isophorone diisocyanate, methylcyclohexane diisocyanate and trimethylhexamethylene diisocyanate, and the sodium alkoxide is sodium methoxide or sodium ethoxide.
8. The method for preparing a demulsifier containing impure crude oil according to claim 1, characterized in that: The mass ratio of the cross-linked polyether to the phenolic amine resin polyether in S3 is 1:1-3.
9. The method for preparing a demulsifier containing impure crude oil according to claim 1, characterized in that: The epichlorohydrin, the olamine, the sodium alkoxide and the aliphatic or alicyclic diisocyanate are added dropwise; the aliphatic or alicyclic diisocyanate is dissolved in xylene and added dropwise to the aminoalkoxy polyether.
10. A demulsifier for crude oil containing impurities obtained by the method for preparing a demulsifier for crude oil containing impurities according to any one of claims 1 to 9.
Citation Information
Patent Citations
A demulsifier, its preparation method and its application
CN114736337B
High-temperature sewage treatment reverse demulsifier of ultra-heavy oil
CN103086472A
Polyurethane type crude oil demulsifier and preparation method thereof
CN105601866A
Macromolecular crude oil demulsifier
CN111718745A
Demulsifier for polymer-containing crude oil and preparation method thereof
CN116375953A