Regeneration and recovery method for transformer oil
Through the use of porous inorganic particles composite chitosan adsorption materials and bacterial cellulose modified chitosan, the problem of insufficient adsorption capacity of traditional adsorbents is solved, efficient regeneration and purification of transformer oil is achieved, and the quality of regenerated oil is improved. Recovery rate.
Patent Information
- Application Number
- CN202410852587.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-12
AI Technical Summary
During the regeneration process of existing transformer oil, traditional adsorption and regeneration capabilities of traditional adsorbents are poor, and they cannot effectively deal with severely aging waste oil, resulting in poor regeneration effect.
Porous inorganic particle composite chitosan adsorbent is used as a regenerated adsorbent. Through filtration and adsorption treatment, the acid resistance of bacterial cellulose modified chitosan is combined with the acid resistance of bacterial cellulose modified chitosan, and the ratio of adsorbent addition and material types are optimized to improve the adsorption effect.
Effective adsorption of acidic impurities, particulate carbon and metal ions in the transformer oil is achieved, the purification quality of recycled oil is improved, the recovery rate is reduced due to excessive adsorption, and the physical and chemical properties of recycled oil are significantly improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of regenerating transformer oil, and in particular to a transformer oil regeneration and recovery method. Background Art
[0002] Transformers are important power equipment, and transformer oil plays a cooling and insulating role in them. Its stability and safety are one of the key links to ensure the reliable operation of electricity, and are highly valued by the industry. Most transformer oils in my country use mineral insulating oil, which comes from petroleum and is a non-renewable resource. Generally speaking, transformer oil has excellent insulation properties, few impurities, and clear color. However, after a long period of operation, the transformer oil will gradually age due to the influence of temperature, electric field and air, and will produce oxides or decomposition products. At the same time, transformer oil will also corrode the materials inside the transformer, forming small molecules or colloidal impurities. The presence of these substances will reduce the physical and chemical properties of the oil, and thus pose a serious threat to the electrical strength of the insulating oil.
[0003] Since the main body of transformer waste oil is still qualified lubricant base oil, after scientific and reasonable refining process, transformer waste oil can be regenerated and its quality is equivalent to that of new transformer oil. Therefore, the recycling of transformer waste oil is of great significance to improving resource utilization, improving enterprise economic benefits and protecting the ecological environment.
[0004] With respect to the above-mentioned related technologies, the inventors found that in the existing transformer oil regeneration process, the technical solution of adsorption regeneration is relatively convenient and quick, but the adsorption regeneration ability of traditional adsorbents is poor, and they can only simply improve the color of waste transformer oil. The adsorption effect on transformer waste oil that is not seriously aged is not good. Summary of the invention
[0005] In order to improve the defect of poor regeneration and recovery effect of existing transformer oil, the present application provides a transformer oil regeneration and recovery method.
[0006] A transformer oil regeneration and recovery method, characterized in that it comprises the following steps: Take the waste transformer oil and filter it to remove the added particles and impurities in the waste transformer oil, and collect the filtrate; The filtrate is placed in a reaction device, and the temperature in the reaction device is increased and stirred for 25-30 minutes; After the heat preservation and stirring are completed, a regeneration adsorbent is added to the reaction device, and the stirring and adsorption process is continued. After the adsorption is completed, the oil is filtered again and allowed to stand and cool to room temperature, thereby completing the regeneration and recovery step of the transformer oil; The regeneration adsorbent is a porous inorganic particle composite chitosan adsorption material.
[0007] Through the above technical scheme, the present application first effectively filters the impurities and added particles in the transformer oil to preliminarily remove the impurities. On this basis, the porous inorganic particle composite chitosan adsorption material is used as the main adsorption material for treatment. Since chitosan linear polysaccharide has multiple amino groups and hydroxyl groups in its molecules, it can effectively combine with metal ions or acidic substances, thereby better adsorbing acidic impurities, particulate carbon, metal ions and other substances in the transformer oil, thereby realizing the effective regeneration of waste transformer oil.
[0008] Furthermore, the addition ratio of the regenerated adsorbent is 2.2-3.5%.
[0009] Through the above technical scheme, the present application optimizes the addition ratio of the regenerated adsorbent. On the one hand, the regenerated adsorbent after the optimized ratio has a good and sufficient adsorption effect, thereby improving the adsorption and purification quality of the regenerated adsorbent. On the other hand, effective control of the addition amount of the regenerated adsorbent can prevent the defect that its adsorption effect is too good, resulting in a decrease in the regeneration recovery rate of the transformer oil after the transformer oil is adsorbed.
[0010] Furthermore, the porous inorganic particles include at least one of attapulgite, diatomaceous earth or bentonite.
[0011] Through the above technical scheme, the present application optimizes the types of porous inorganic particles, and the selected attapulgite, diatomaceous earth or bentonite can maintain good crystal shape, crystallinity and adsorption effect when used as a composite material.
[0012] Furthermore, the chitosan in the porous inorganic particle composite chitosan adsorption material is an acid-resistant modified chitosan, and the acid-resistant modified chitosan is prepared by cross-linking and modifying bacterial cellulose.
[0013] Furthermore, the porous inorganic particle composite chitosan adsorption material is prepared by the following scheme: Place bacterial cellulose in a homogenizing stirring device, stir and mix, and collect the mixed liquid; Chitosan and glacial acetic acid are mixed and placed in deionized water, and after the mixed solution is added, stirring and mixing are continued, ultrasonic dispersion is performed, and the dispersion is collected; The porous inorganic particles are placed in an acidic modifier, acidified, washed and dried, and then placed in a calcining device, calcined, ground and pulverized to obtain mixed inorganic particles; The mixed inorganic particles are mixed with the dispersion, stirred and cross-linked, heated and kept warm, the sol is collected and aged, vacuum-freeze-dried, ground and dispersed, and the porous inorganic particle composite chitosan adsorption material can be prepared.
[0014] Through the above technical scheme, the present application further modifies chitosan. Since chitosan will dissolve when the pH is lower than 5.5 and has poor mechanical properties, when it is directly prepared into an adsorbent, the adsorbent will disintegrate due to the acidic environment. The present application optimizes it and modifies it through bacterial cellulose. Bacterial cellulose has a unique network structure. It is connected by molecular factors and intermolecular hydrogen bonds to form a supramolecular porous fiber network structure. At the same time, bacterial cellulose has negative electrical properties, which is beneficial to reduce the electrostatic repulsion of impurity ions in transformer oil, thereby improving the acid resistance of chitosan while improving its adsorption and purification effects.
[0015] Furthermore, the acidic modifier is H2SO4 with a concentration of 0.5-0.8 mol / L.
[0016] In summary, this application has the following beneficial effects: First, the present application first effectively filters the impurities and added particles in the transformer oil to preliminarily remove the impurities. On this basis, the porous inorganic particle composite chitosan adsorption material is used as the main adsorption material for treatment. Since chitosan linear polysaccharide has multiple amino groups and hydroxyl groups in its molecules, it can effectively combine with metal ions or acidic substances, thereby better adsorbing acidic impurities, particulate carbon, metal ions and other substances in the transformer oil, thereby achieving effective regeneration of waste transformer oil.
[0017] Second, the present application optimizes the addition ratio of the regenerated adsorbent. On the one hand, the regenerated adsorbent after the optimized ratio has a good and sufficient adsorption effect, thereby improving the adsorption and purification quality of the regenerated adsorbent. On the other hand, effective control of the addition amount of the regenerated adsorbent can prevent the defect that the adsorption effect is too good, resulting in a decrease in the regeneration recovery rate of the transformer oil after the transformer oil is adsorbed.
[0018] Third, the present application further modifies chitosan. Since chitosan will dissolve when the pH is lower than 5.5 and has poor mechanical properties, when it is directly prepared into an adsorbent, the adsorbent will disintegrate due to the acidic environment. The present application optimizes it and modifies it through bacterial cellulose. Bacterial cellulose has a unique network structure. It is connected by molecular factors and intermolecular hydrogen bonds to form a supramolecular porous fiber network structure. At the same time, bacterial cellulose has negative electrical properties, which is beneficial to weaken the electrostatic repulsion of impurity ions in transformer oil, thereby improving the acid resistance of chitosan while improving its adsorption and purification effects. DETAILED DESCRIPTION
[0019] The present application is further described in detail below in conjunction with embodiments.
[0020] Preparation Example 1 Porous inorganic particle composite chitosan adsorption material 1 20 g of chitosan and 8 g of glacial acetic acid were mixed in 1200 mL of deionized water, and stirred to prepare a mixed solution; 200 g of attapulgite was first placed in 2 L of H2SO4 with a concentration of 0.5 mol / L, acidified, rinsed with deionized water 3 times, dried at 55°C for 3 h, placed in a calcination device, calcined at 500°C for 2 h, ground and pulverized, and mixed inorganic particles were collected; After mixing 200-300g of mixed inorganic particles with 1200g of mixed liquid, stirring and cross-linking for 30 minutes, heating to 50°C and keeping warm, collecting the sol liquid and aging it for 3h, vacuum freeze-drying, grinding and dispersing, the porous inorganic particle composite chitosan adsorption material 1 can be prepared.
[0021] Preparation Example 2 Porous inorganic particle composite chitosan adsorption material 2 200 g of 2.0% bacterial cellulose solution was placed in a homogenizing stirring device, stirred and mixed at 1000 r / min and the mixed solution was collected; Take 20g chitosan and 8g glacial acetic acid and mix them in 1200mL deionized water. After adding the mixture, continue to stir and mix at 2000r / min, ultrasonically disperse at 200W and collect the dispersion; 200 g of attapulgite was first placed in 2 L of H2SO4 with a concentration of 0.5 mol / L, acidified, rinsed with deionized water 3 times, dried at 55°C for 3 h, placed in a calcination device, calcined at 500°C for 2 h, ground and pulverized, and mixed inorganic particles were collected; After mixing 200-300g of mixed inorganic particles with 1200g of dispersion liquid, stir and cross-link for 30 minutes, heat to 50°C and keep warm, collect the sol liquid and age it for 3h, vacuum freeze-dry, grind and disperse it, and the porous inorganic particle composite chitosan adsorption material 2 can be prepared.
[0022] Preparation Example 3 Porous inorganic particle composite chitosan adsorption material 3 350 g of 2.0% bacterial cellulose solution was placed in a homogenizing stirring device, stirred and mixed at 1250 r / min and the mixed solution was collected; Take 22g chitosan and 9g glacial acetic acid and mix them in 1350mL deionized water. After adding the mixture, continue to stir and mix at 2500r / min, ultrasonically disperse at 200W and collect the dispersion; 250 g of attapulgite was first placed in 2 L of H2SO4 with a concentration of 0.65 mol / L, acidified, rinsed with deionized water 5 times, dried at 55°C for 3 h, placed in a calcination device, calcined at 500°C for 2 h, ground and pulverized, and mixed inorganic particles were collected; After mixing 250g of mixed inorganic particles with 1350g of dispersion liquid, stir and cross-link for 30 minutes, heat to 50°C and keep warm, collect the sol liquid and age it for 3h, vacuum freeze-dry, grind and disperse it, and the porous inorganic particle composite chitosan adsorption material 3 can be prepared.
[0023] Preparation Example 4 Porous inorganic particle composite chitosan adsorption material 4 500 g of 2.0% bacterial cellulose solution was placed in a homogenizing stirring device, stirred and mixed at 1500 r / min and the mixed solution was collected; Take 25g chitosan and 8-10g glacial acetic acid and mix them in 1500mL deionized water. After adding the mixture, continue to stir and mix at 3000r / min, ultrasonically disperse at 200W and collect the dispersion; 300 g of porous inorganic particles were first placed in 2 L of H2SO4 with a concentration of 0.8 mol / L, acidified, rinsed with deionized water 5 times, dried at 55°C for 3 h, placed in a calcination device, calcined at 500°C for 2 h, ground and pulverized, and mixed inorganic particles were collected; After mixing 300 g of mixed inorganic particles with 1500 g of dispersion, stir and cross-link for 30 minutes, heat to 50°C and keep warm, collect the sol liquid and age it for 3 hours, freeze-dry in vacuum, grind and disperse, and the porous inorganic particle composite chitosan adsorption material 4 can be prepared.
[0024] Preparation Example 5 Porous inorganic particle composite chitosan adsorption material 5 350 g of 2.0% bacterial cellulose solution was placed in a homogenizing stirring device, stirred and mixed at 1250 r / min and the mixed solution was collected; Take 22g chitosan and 9g glacial acetic acid and mix them in 1350mL deionized water. After adding the mixture, continue to stir and mix at 2500r / min, ultrasonically disperse at 200W and collect the dispersion; 250 g of diatomaceous earth was placed in 2 L of H2SO4 with a concentration of 0.65 mol / L, acidified, rinsed with deionized water 5 times, dried at 55°C for 3 h, placed in a calcination device, calcined at 500°C for 2 h, ground and pulverized, and mixed inorganic particles were collected; After mixing 250g of mixed inorganic particles with 1350g of dispersion liquid, stir and cross-link for 30min, heat to 50°C and keep warm, collect the sol liquid and age it for 3h, freeze-dry in vacuum, grind and disperse, and the porous inorganic particle composite chitosan adsorption material 5 can be prepared.
[0025] Preparation Example 6 Porous inorganic particle composite chitosan adsorption material 6 350 g of 2.0% bacterial cellulose solution was placed in a homogenizing stirring device, stirred and mixed at 1250 r / min and the mixed solution was collected; Take 22g chitosan and 9g glacial acetic acid and mix them in 1350mL deionized water. After adding the mixture, continue to stir and mix at 2500r / min, ultrasonically disperse at 200W and collect the dispersion; 250 g of bentonite was first placed in 2 L of H2SO4 with a concentration of 0.65 mol / L, acidified, rinsed with deionized water 5 times, dried at 55°C for 3 h, placed in a calcination device, calcined at 500°C for 2 h, ground and pulverized, and mixed inorganic particles were collected; After mixing 250g of mixed inorganic particles with 1350g of dispersion liquid, stir and cross-link for 30 minutes, heat to 50°C and keep warm, collect the sol liquid and age it for 3h, vacuum freeze-dry, grind and disperse it, and the porous inorganic particle composite chitosan adsorption material 6 can be prepared.
[0026] Example 1 A transformer oil regeneration and recovery method comprises the following steps: Waste transformer oil with an acid value of 0.38 mgKOH / g and a dielectric loss factor of 0.0355 is first filtered to remove the added particles and impurities in the waste transformer oil, and the filtrate is collected; Place the filtrate in a reaction device, heat the reaction device to 60°C, and stir for 25-30 minutes; After the heat preservation and stirring are completed, the regeneration adsorbent 1 is added in an amount of 2.2% and placed in the reaction device, and the stirring and adsorption treatment is continued. After the adsorption treatment for 2 hours, it is filtered again and allowed to stand and cool to room temperature, and the regeneration and recovery step of the transformer oil is completed.
[0027] Example 2 A transformer oil regeneration and recovery method comprises the following steps: Waste transformer oil with an acid value of 0.38 mgKOH / g and a dielectric loss factor of 0.0355 is first filtered to remove the added particles and impurities in the waste transformer oil, and the filtrate is collected; Place the filtrate in a reaction device, heat the reaction device to 60°C, and stir for 25-30 minutes; After the heat preservation and stirring are completed, the regeneration adsorbent 1 is added in an amount of 3% and placed in the reaction device, and the stirring and adsorption treatment is continued. After the adsorption treatment for 2 hours, it is filtered again and allowed to stand and cool to room temperature, and the regeneration and recovery step of the transformer oil is completed.
[0028] Example 3 A transformer oil regeneration and recovery method comprises the following steps: Waste transformer oil with an acid value of 0.38 mgKOH / g and a dielectric loss factor of 0.0355 is first filtered to remove the added particles and impurities in the waste transformer oil, and the filtrate is collected; Place the filtrate in a reaction device, heat the reaction device to 60°C, and stir for 25-30 minutes; After the heat preservation and stirring are completed, the regeneration adsorbent 1 is added in an amount of 3.5% and placed in the reaction device, and the stirring and adsorption treatment is continued. After the adsorption treatment for 2 hours, it is filtered again and allowed to stand and cool to room temperature, and the regeneration and recovery step of the transformer oil is completed.
[0029] Example 4 A transformer oil regeneration and recovery method comprises the following steps: Waste transformer oil with an acid value of 0.38 mgKOH / g and a dielectric loss factor of 0.0355 is first filtered to remove the added particles and impurities in the waste transformer oil, and the filtrate is collected; Place the filtrate in a reaction device, heat the reaction device to 60°C, and stir for 25-30 minutes; After the heat preservation and stirring are completed, the regeneration adsorbent 2 is added in an amount of 3% and placed in the reaction device, and the stirring and adsorption treatment is continued. After the adsorption treatment for 2 hours, it is filtered again and allowed to stand and cool to room temperature, and the regeneration and recovery step of the transformer oil is completed.
[0030] Example 5 A transformer oil regeneration and recovery method comprises the following steps: Waste transformer oil with an acid value of 0.38 mgKOH / g and a dielectric loss factor of 0.0355 is first filtered to remove the added particles and impurities in the waste transformer oil, and the filtrate is collected; Place the filtrate in a reaction device, heat the reaction device to 60°C, and stir for 25-30 minutes; After the heat preservation and stirring are completed, the regeneration adsorbent 3 is added in an amount of 3% and placed in the reaction device, and the stirring and adsorption treatment is continued. After the adsorption treatment for 2 hours, it is filtered again and left to cool to room temperature, and the regeneration and recovery step of the transformer oil is completed.
[0031] Example 6 A transformer oil regeneration and recovery method comprises the following steps: Waste transformer oil with an acid value of 0.38 mgKOH / g and a dielectric loss factor of 0.0355 is first filtered to remove the added particles and impurities in the waste transformer oil, and the filtrate is collected; Place the filtrate in a reaction device, heat the reaction device to 60°C, and stir for 25-30 minutes; After the heat preservation and stirring are completed, the regeneration adsorbent 4 is added in an amount of 3% and placed in the reaction device, and the stirring and adsorption treatment is continued. After the adsorption treatment for 2 hours, it is filtered again and allowed to stand and cool to room temperature, and the regeneration and recovery step of the transformer oil is completed.
[0032] Example 7 A transformer oil regeneration and recovery method comprises the following steps: Waste transformer oil with an acid value of 0.38 mgKOH / g and a dielectric loss factor of 0.0355 is first filtered to remove the added particles and impurities in the waste transformer oil, and the filtrate is collected; Place the filtrate in a reaction device, heat the reaction device to 60°C, and stir for 25-30 minutes; After the heat preservation and stirring are completed, the regeneration adsorbent 5 is added in an amount of 3% and placed in the reaction device, and the stirring and adsorption treatment is continued. After the adsorption treatment for 2 hours, it is filtered again and allowed to stand and cool to room temperature, and the regeneration and recovery step of the transformer oil is completed.
[0033] Example 8 A transformer oil regeneration and recovery method comprises the following steps: Waste transformer oil with an acid value of 0.38 mgKOH / g and a dielectric loss factor of 0.0355 is first filtered to remove the added particles and impurities in the waste transformer oil, and the filtrate is collected; Place the filtrate in a reaction device, heat the reaction device to 60°C, and stir for 25-30 minutes; After the heat preservation and stirring are completed, the regeneration adsorbent 6 is added in an amount of 3% and placed in the reaction device, and the stirring and adsorption treatment is continued. After the adsorption treatment for 2 hours, it is filtered again and allowed to stand and cool to room temperature, and the regeneration and recovery step of the transformer oil is completed.
[0034] Performance Testing The transformer oils regenerated and recovered in Examples 1-8 were subjected to performance tests, specifically testing their acid value, pH and breakdown voltage, and the results were recorded as shown in Table 1 below: Table 1 Performance test table
[0035] In combination with Examples 1-3, it can be found that the present application first effectively filters the impurities and added particles in the transformer oil to preliminarily remove the impurities. On this basis, the porous inorganic particle composite chitosan adsorption material is used as the main adsorption material for treatment. Since chitosan linear polysaccharides have multiple amino groups and hydroxyl groups in their molecules, they can effectively combine with metal ions or acidic substances, thereby better adsorbing acidic impurities, particulate carbon, metal ions and other substances in the transformer oil, thereby achieving effective regeneration of waste transformer oil.
[0036] Secondly, from the comparison of the test results of the above-mentioned Examples 1-3 and Examples 4-8 and Table 1, it can be found that: the present application modifies chitosan by bacterial cellulose. Since bacterial cellulose has a unique network structure, it is connected by molecular factors and intermolecular hydrogen bonds to form a supramolecular porous fiber network structure. At the same time, bacterial cellulose has negative electrical properties, which is beneficial to weaken the electrostatic repulsion of impurity ions in transformer oil, thereby improving the acid resistance of chitosan while improving its adsorption and purification effects.
[0037] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
[0038] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.
[0039] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.
[0040] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.
Claims
1. A transformer oil regeneration and recovery method, characterized in that: The following steps are involved: Take the waste transformer oil and filter it to remove the added particles and impurities in the waste transformer oil, and collect the filtrate; The filtrate is placed in a reaction device, and the temperature in the reaction device is increased and stirred for 25-30 minutes; After the heat preservation and stirring are completed, a regeneration adsorbent is added to the reaction device, and the stirring and adsorption treatment is continued. After the adsorption is completed, the oil is filtered again and allowed to stand and cool to room temperature, thereby completing the regeneration and recovery step of the transformer oil; The regeneration adsorbent is a porous inorganic particle composite chitosan adsorption material.
2. A transformer oil regeneration and recovery method according to claim 1, characterized in that: The addition ratio of the regenerated adsorbent is 2.2-3.5%.
3. A transformer oil regeneration and recovery method according to claim 1, characterized in that: The porous inorganic particles include at least one of attapulgite, diatomaceous earth or bentonite.
4. A transformer oil regeneration and recovery method according to claim 1, characterized in that: The chitosan in the porous inorganic particle composite chitosan adsorption material is acid-resistant modified chitosan, and the acid-resistant modified chitosan is prepared by cross-linking and modifying bacterial cellulose.
5. A transformer oil regeneration and recovery method according to claim 4, characterized in that: The porous inorganic particle composite chitosan adsorption material is prepared by the following scheme: Place bacterial cellulose in a homogenizing stirring device, stir and mix, and collect the mixed liquid; Chitosan and glacial acetic acid are mixed and placed in deionized water, and after the mixed solution is added, stirring and mixing are continued, ultrasonic dispersion is performed, and the dispersion is collected; The porous inorganic particles are placed in an acidic modifier, acidified, washed and dried, and then placed in a calcining device, calcined, ground and pulverized to obtain mixed inorganic particles; The mixed inorganic particles are mixed with the dispersion, stirred and cross-linked, heated and kept warm, the sol is collected and aged, vacuum-freeze-dried, ground and dispersed, and the porous inorganic particle composite chitosan adsorption material can be prepared.