Preparation method of environment-friendly transparent conductive leather
By expanding, oil tanning, bleaching and water retention treatment of the naked skin after desalting and softening, and adding transparent conductive materials, transparent conductive leather with high light transmittance and good conductivity was prepared through the drum tanning step, which solved the traditional leather The problems of opacity and poor durability have broadened their application in smart devices and medical materials, while meeting environmental protection requirements.
Patent Information
- Application Number
- CN202411300903.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-18
AI Technical Summary
Traditional leather is opaque and poorly durable, and existing transparent leather lacks exploration in conductivity, limiting its application in smart flexible electronic devices and medical materials.
The bare leather after desalting and softening is used for expansion, oil tanning, bleaching, and water retention treatment, and transparent conductive materials are added to prepare transparent conductive leather with high light transmittance and good conductivity through drum tanning and drying steps.
It realizes transparent conductive leather with colorless, high light transmittance, friction-resistant and tensile resistance, has good electrical properties, and can be decomposed in natural environments, complying with environmental protection standards.
Smart Images

Figure CN118932121A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing an environmentally friendly transparent conductive leather, and in particular to a transparent conductive leather, a transparent optical element, a transparent medical material, a flexible electronic display device and a preparation method thereof. Background Art
[0002] Leather is a natural bio-based material composed of peptide chains, collagen, collagen fibrils and collagen fibers in sequence. It is naturally flexible, durable and biodegradable, so it is widely used in clothing, luggage and car interiors. However, traditional leather is opaque, which limits its application in flexible displays, transparent medical materials, and wearable flexible electronic devices. There are two reasons why traditional leather is opaque. First, in the internal structure of the leather, the refractive index of the leather collagen fiber structure and the refractive index of the air in the leather pores are quite different. Second, in the leather processing process, tanning is mostly done by vegetable tanning, chrome tanning or aluminum tanning, which makes the color of the tanning agent appear.
[0003] Among the existing transparent leather production methods, there is a method for preparing transparent leather by soaking chrome-tanned leather in ionic liquid. The final product will inevitably have a blue color after chrome tanning, and the light transmittance is relatively low. Transparent leather can also be prepared by using deashed and softened bare leather as raw material and treating it with multifunctional active substances or polyols. Although the product produced by this method has high light transmittance and is colorless, its durability is poor because it has not been tanned. Transparent leather can also be prepared by using the refractive index matching principle, but by replacing its original skeleton with a polymer in situ inside the bare leather, the bare leather itself loses its biodegradable characteristics.
[0004] In addition, the existing transparent leather lacks exploration in conductivity, which limits its application in the fields of smart flexible electronic devices, touch screens in smart wearable technologies, flexible circuit boards, etc. In addition, transparent conductive leather can also be used to create more innovative and unique designs. By adding conductive functions, more diverse lighting effects, display functions, etc. can be achieved on transparent leather, adding more value and appeal to the product.
[0005] Therefore, developing a method for producing colorless, highly transmittance-efficient and environmentally friendly transparent conductive leather is very important to improve its quality and application range. Summary of the invention
[0006] The object of the present invention is to provide an environmentally friendly method for preparing transparent conductive leather to solve one or more of the above-mentioned problems in the prior art.
[0007] In one aspect, the present invention provides a method for preparing an environmentally friendly transparent conductive leather, comprising the following steps: Step 1. Swelling: Soak the delimed and softened bare skin in an acid or alkali aqueous solution at 15-35°C for 1-14 days; Step 2. Oil tanning: weigh the hides obtained in step 1, place them in a drum, add 100%-500% of its weight of oil tanning agent, start the drum, and tan at 15-35°C for 2-48 hours to allow the oil tanning agent to fully fill the pores of the hides; Step 3. Bleaching and decolorization: placing the leather obtained in step 2 in a bleaching solution and allowing it to stand and soak for 10-30 minutes; Step 4. Water retention treatment and drying: Take out the skin obtained in step 3, put it in a rotating drum, add 150%-500% of its weight of water retention agent, rotate for 1-72 hours, and then dry it on a stretch board at 40-60 ℃ for 6-72 hours, and control the moisture content at 20%-30%; Step 5. Preparation of transparent conductive solution: Mix the transparent conductive material with a solvent or an adhesive to prepare a conductive solution with a mass fraction of 2%-20%, ensuring uniform mixing to obtain stable conductive performance; Step 6. Conductive treatment: Add the conductive solution prepared in step 5 to the transparent leather obtained in step 4, and dry on a stretcher at 40-60° C. for 3-6 h.
[0008] In some embodiments, the delimed and softened bare hide in step 1 is selected from one of cow top hide, cow split hide, sheep hide, goat hide or pig hide.
[0009] In some embodiments, the acid in step 1 is selected from one of sulfuric acid, nitric acid or hydrochloric acid, and the base is selected from one of sodium hydroxide, potassium hydroxide or calcium hydroxide.
[0010] In some embodiments, the oil tanning agent in step 2 is selected from one or more of fish oil, lanolin, castor oil, olive oil, rapeseed oil or linseed oil.
[0011] In some embodiments, the bleaching solution in step 3 is selected from one of sodium peroxide, hydrogen peroxide, sodium hypochlorite, sodium chlorite or oxalic acid.
[0012] In some embodiments, the water-retaining agent in step 4 is selected from one or more of propylene glycol, sorbitol, polyethylene glycol, glycerol, sodium hyaluronate, urea or trehalose.
[0013] In some embodiments, the rotation speed of the drum in steps 2 and 4 is 80-150 r / min.
[0014] In some embodiments, in step 5, the transparent conductive material is selected from any one of indium tin oxide (ITO), poly(3,4-ethylenedioxythiophene) (PEDOT), poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS), silver nanowires (AgNWs), copper oxide (Cu2O), or a mixture thereof, and the solvent or adhesive is one or more of water, ethanol, isopropanol, tetrahydrofuran, 1,2-dimethoxyethane (DME), epoxy resin, acrylate resin, or polyvinyl chloride.
[0015] In some embodiments, the conductive solution in step 6 is added by one or more methods selected from spraying, printing, filtration or dipping.
[0016] In another aspect, the present invention provides a transparent conductive leather prepared by the above method.
[0017] Beneficial effects of the present invention: The present invention selects deashed and softened bare skin as raw material, studies and develops a preparation process of environmentally friendly transparent conductive leather, and can obtain transparent leather with excellent light transmittance through the steps of expansion, bleaching, drum tanning and the like. The use of drum tanning can make the oil tanning agent and the water retaining agent fully fill between the swollen bare skin fibers, significantly enhance the binding force between the reaction raw materials and the bare skin, form a tougher skeleton, and make the transparent leather have strong friction resistance and tensile resistance. At the same time, transparent conductive materials are added to make it have good electrical properties. The raw materials used have relatively little impact on the environment during production and processing, and the final product can be decomposed by microorganisms in the natural environment, which can reduce the damage to the environment and the ecosystem, and meet the current environmental protection standards and sustainable development requirements.
[0018] The present invention improves the process, selects different oil tanning agents, bleaching agents, water retaining agents, and transparent conductive materials, and adopts a drum tanning method to prepare transparent leather with high light transmittance, friction resistance, stretch resistance, excellent conductivity and environmental friendliness that can be used for flexible display screens. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The photo and UV-visible-near-infrared spectra of the transparent conductive leather prepared in Example 1 of the present invention are shown; Figure 2 The scanning electron microscope images of the surface and cross section of the transparent conductive leather prepared in Example 1 of the present invention; Figure 3 This is a scanning electron microscope image of the surface of the transparent conductive leather prepared in Example 1 of the present invention after being bent 500 times and rubbed 500 times; Figure 4is a stress-strain curve of the transparent conductive leather prepared in Example 1 of the present invention after stretching; Figure 5 This is a resistance change diagram of the transparent conductive leather prepared in Example 1 of the present invention at room temperature. DETAILED DESCRIPTION
[0020] The present invention is further described below in conjunction with the examples. The following examples are only used to more clearly illustrate the performance of the present invention, and are not limited to the following examples.
[0021] Embodiment 1: In this embodiment, we selected de-ashed and softened sheepskin as raw material, and selected fish oil as oil tanning agent to prepare transparent leather.
[0022] First, cut the delimed and softened sheepskin into specific sizes, wash it with pure water and set aside.
[0023] Dissolve hydrochloric acid in water to prepare a 6% hydrochloric acid aqueous solution, mix it with the bare skin so that it covers the bare skin, and let it stand for 5 days. After the reaction is completed, pour out the excess reaction solution, pick up the skin with tweezers, wash off the excess hydrochloric acid on the surface with pure water, wipe dry, and weigh.
[0024] Place the swollen leather in a drum, add 200% of its weight of fish oil, set the speed to 120 r / min, and tan for 3 h at 30°C. After the reaction, pour out the excess reaction solution, pick up the leather with tweezers, rinse off the excess fish oil on the surface with pure water, and wipe dry.
[0025] Prepare a 15% sodium hypochlorite aqueous solution, add it to the leather treated above, and let it sit for 20 minutes. After the reaction, pour out the excess reaction solution, pick up the leather with tweezers, rinse off the excess bleaching liquid on the surface with pure water, and wipe it dry.
[0026] Dissolve sorbitol in water to prepare a 10% water retainer solution, mix it with the leather treated above and place it in a drum. The dosage is 180% of the weight of the leather. Set the speed to 100 r / min and tan for 1 h at 30°C. After the reaction is completed, pour off the excess reaction solution, pick up the leather with tweezers, rinse off the excess water retainer on the surface with pure water, and wipe dry.
[0027] The transparent leather obtained after the above steps was dried on a stretch board at 45°C for 12 h, and the moisture content was controlled at 20%-30%.
[0028] The silver nanowire powder was added to a mixed solution of ethanol and water and stirred with a magnetic stirrer until a uniform dispersion was achieved. The silver nanowires were diluted to a 5% aqueous solution by adding an appropriate amount of purified water. The silver nanowires were dispersed by ultrasonic treatment.
[0029] The silver nanowire aqueous solution with a mass fraction of 5% prepared in the above step was evenly added to ensure that the entire transparent leather was covered and formed into a uniform film, and then filtered. The solution was dried on a stretch board at 40°C for 4 h to accelerate the curing process.
[0030] Example 1 was tested: from Figure 1 It can be seen that the transparent conductive leather prepared in Example 1 has high transmittance. The analysis of the ultraviolet-visible-near-infrared spectrum shows that the transmittance in part of the visible light region can reach 75% or more.
[0031] from Figure 2 It can be seen that after drum tanning, the oil tanning agent and the leather are well combined, and the oil tanning agent is tightly combined with the leather collagen fiber bundles. Subsequently, a water-retaining agent is used to fill the interior to make its surface smooth and have excellent stability.
[0032] The transparent conductive leather was placed on a friction tester, the friction tester pressure was set to 50 kPa, the sandpaper mesh was 1000 mesh, and the friction times were 500 times. By comparing the scanning electron microscope images before and after the friction, it can be seen that the transparent conductive leather was only slightly damaged on the surface, such as Figure 3 As shown. This proves that the transparent conductive leather prepared by this method has strong wear resistance.
[0033] The transparent conductive leather is placed on a mechanical testing machine for stretching, and its stress-strain curve can be obtained, such as Figure 4 As shown, analysis shows that the maximum stress it can withstand is up to 8 MPa, which proves that the transparent conductive leather prepared by this method has better stretchability.
[0034] Ten batches of transparent conductive leather were prepared using the same method, and their resistance values were tested respectively. Figure 5 As shown, analysis shows that the resistance is below 500 ohms, which proves that the transparent conductive leather prepared by this method has good electrical properties.
[0035] Embodiment 2: In this embodiment, we selected delimed and softened pigskin as raw material, and castor oil and rapeseed oil as oil tanning agents to prepare transparent leather.
[0036] First, cut the delimed and softened pigskin into specific sizes, wash it with pure water and set aside.
[0037] Dissolve sulfuric acid in water to prepare a 3% sulfuric acid aqueous solution, mix it with the bare skin so that it covers the bare skin, and let it stand for 7 days. After the reaction is completed, pour out the excess reaction solution, pick up the skin with tweezers, wash off the excess sulfuric acid on the surface with pure water, wipe dry, and weigh.
[0038] Place the swollen bare hide in a drum, add 230% of its mass of castor oil and rapeseed oil mixed tanning agent at a ratio of 1:2, set the speed to 80 r / min, and tan for 5 hours at 25°C. After the reaction, pour off the excess reaction solution, pick up the leather with tweezers, rinse off the excess tanning agent on the surface with pure water, and wipe dry.
[0039] Prepare a 20% oxalic acid aqueous solution, add it to the leather treated above, and let it stand for 15 minutes. After the reaction, pour out the excess reaction solution, pick up the leather with tweezers, rinse off the excess bleaching liquid on the surface with pure water, and wipe it dry.
[0040] Dissolve polyethylene glycol in water to prepare a 10% water retainer solution, mix it with the leather treated above and place it in a drum, the dosage is 200% of the weight of the leather, set the speed to 120 r / min, and tan at 30°C for 2 hours. After the reaction is completed, pour off the excess reaction solution, pick up the leather with tweezers, rinse off the excess water retainer on the surface with pure water, and wipe dry.
[0041] The transparent leather obtained after the above steps was dried on a stretch board at 50°C for 8 h, and the moisture content was controlled at 20%-30%.
[0042] Indium oxide and tin oxide powders were mixed evenly in a ratio of 1:2, and the mixed powders were added into isopropanol to prepare an indium tin oxide coating with a mass fraction of 5%. The powders in the solvent were fully mixed and dispersed using an oscillating ball mill until a uniform coating solution was obtained.
[0043] Drop 5% indium tin oxide coating on the center of the transparent leather, start the spin coater at 1000 RPM to evenly distribute the coating solution on the transparent leather surface. Dry on a stretcher at 45°C for 3 h to accelerate the curing process.
[0044] Embodiment 3: In this embodiment, we selected delimed and softened cow top leather as raw material, and rapeseed oil as oil tanning agent to prepare transparent leather.
[0045] First, cut the de-limed and softened cow top hide into specific sizes, wash it with pure water and set aside.
[0046] Dissolve potassium hydroxide in water to prepare a 5% potassium hydroxide aqueous solution, mix it with the bare skin so that it covers the bare skin, and let it stand for 12 days. After the reaction is completed, pour out the excess reaction solution, pick up the skin with tweezers, wash off the excess alkaline solution on the surface with pure water, wipe dry, and weigh.
[0047] Place the bare leather after alkali swelling in a drum, add 200% rapeseed oil by weight, set the speed to 150 r / min, and tan for 8 hours at 30°C. After the reaction, pour off the excess reaction solution, pick up the leather with tweezers, rinse off the excess oil tanning agent on the surface with pure water, and wipe dry.
[0048] Prepare a 10% hydrogen peroxide aqueous solution, add it to the leather treated above, and let it stand for 10 minutes. After the reaction, pour out the excess reaction solution, pick up the leather with tweezers, rinse off the excess bleaching liquid on the surface with pure water, and wipe it dry.
[0049] Dissolve trehalose in water to prepare a 15% water retainer solution, mix it with the leather treated above and place it in a drum, the dosage is 180% of the weight of the leather, set the speed to 100 r / min, and tan for 3 hours at 35°C. After the reaction is completed, pour off the excess reaction solution, pick up the leather with tweezers, rinse off the excess water retainer on the surface with pure water, and wipe dry.
[0050] The transparent leather obtained after the above steps was dried on a stretch board at 45°C for 10 h, and the moisture content was controlled at 20%-30%.
[0051] The aqueous solution of polystyrene sulfonate and 3,4-ethylenedioxythiophene monomer were mixed, the pH value was adjusted to 3, and the mixed solution and potassium permanganate were mixed and ultrasonically treated for 10 minutes under a nitrogen atmosphere. The ultrasonically treated reaction solution was reacted at 25°C for 10 hours to obtain a PEDOT:PSS polymer. It was dispersed in isopropanol to prepare a PEDOT:PSS coating with a mass fraction of 2%.
[0052] Spray the transparent leather at a distance of 10 cm, and evenly spray 2% PEDOT:PSS coating on the surface of the transparent leather. The nozzle is 10 cm away from the transparent leather, and the spraying speed and angle are kept consistent. Dry the board at 40°C for 5 hours to accelerate the curing process.
[0053] Embodiment 4: In this embodiment, we selected de-ashed and softened cow split hide as raw material, and selected olive oil and lanolin as oil tanning agents to prepare transparent leather.
[0054] First, cut the delimed and softened cow split hide into specific sizes, wash it with pure water and set aside.
[0055] Dissolve calcium hydroxide in water to prepare a 6% calcium hydroxide aqueous solution, mix it with the bare skin so that it covers the bare skin, and let it stand for 10 days. After the reaction is completed, pour out the excess reaction solution, pick up the skin with tweezers, wash off the excess alkaline solution on the surface with pure water, wipe dry, and weigh.
[0056] Place the bare hide after alkali swelling in a drum, add 250% of its weight of olive oil and lanolin mixed tanning agent, the mass ratio is 3:2, set the speed to 100 r / min, and tan for 12 hours at 25℃. After the reaction, pour off the excess reaction solution, pick up the leather with tweezers, rinse off the excess oil tanning agent on the surface with pure water, and wipe dry.
[0057] Prepare an 8% sodium chlorite aqueous solution, add it to the leather treated above, and let it stand for 10 minutes. After the reaction, pour out the excess reaction solution, pick up the leather with tweezers, rinse off the excess bleaching liquid on the surface with pure water, and wipe it dry.
[0058] Dissolve polyethylene glycol and glycerol in water to prepare a 20% water retainer solution with a mass ratio of 1:1. Mix it with the leather treated as above and place it in a drum. The amount is 300% of the weight of the leather. Set the speed to 120 r / min and tan for 5 hours at 30°C. After the reaction is completed, pour off the excess reaction solution, pick up the leather with tweezers, rinse off the excess water retainer on the surface with pure water, and wipe dry.
[0059] The transparent leather obtained after the above steps was dried on a stretch board at 55°C for 10 h, and the moisture content was controlled at 20%-30%.
[0060] Copper sulfate pentahydrate was dissolved in deionized water, and a mixed solution of glucose, sodium hydroxide, and PVP was added to adjust the pH to 1, and then a sodium hypophosphite solution was added. After the reaction, the product was separated by high-speed centrifugation, washed with deionized water and anhydrous ethanol, and dried in a vacuum drying oven for 12 h to obtain copper nanoparticles, which were oxidized to form copper oxides. The copper oxide coating with a mass fraction of 3% was prepared by dispersing it in tetrahydrofuran.
[0061] Place the transparent leather on the printing table, pour the above copper oxide coating with a mass fraction of 3%, and use a scraper to evenly scrape the coating across the screen and transfer it to the transparent leather surface through the image opening on the screen. Dry it on a stretcher at 50°C for 3 hours to accelerate the curing process.
[0062] Therefore, the transparent leather prepared by the present invention uses deashed and softened bare skin as raw material, and the oil tanning agent is fully combined with the bare skin fiber bundle through drum tanning. The oil tanning agent can significantly improve the transparency of the leather. The tanning method also retains the mechanical strength of the leather and enhances the durability. The water-retaining agent is combined with the transparent leather so that the leather has excellent friction resistance and tensile resistance while having excellent water retention. At the same time, the added transparent conductive material enables it to have good electrical properties, which can broaden its application in the fields of flexible display screens, transparent optical elements, etc. The raw materials and processed materials have little impact on the environment during the processing process, and the produced transparent leather can be decomposed by microorganisms in the natural environment, and has environmentally friendly characteristics.
[0063] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing an environmentally friendly transparent conductive leather, characterized in that: The following steps are involved: Step 1. Swelling: Soak the delimed and softened bare skin in an acid or alkali aqueous solution at 15-35°C for 1-14 days; Step 2. Oil tanning: weigh the hides obtained in step 1, place them in a drum, add 100% to 500% of the weight of the hides and start the drum, and tan at 15 to 35°C for 2 to 48 hours; Step 3. Bleaching and decolorization: placing the leather obtained in step 2 in the bleaching solution and soaking for 10-30 minutes; Step 4. Water retention treatment and drying: Take out the skin obtained in step 3, put it in a rotating drum, add 150%-500% of its weight of water retention agent, rotate for 1-72 hours, and then dry it on a stretch board at 40-60 ℃ for 6-72 hours, and control the moisture content at 20%-30%; Step 5. Preparation of transparent conductive solution: mixing the transparent conductive material with a solvent or an adhesive to prepare a conductive solution with a mass fraction of 2% to 20%; Step 6. Conductive treatment: Add the conductive solution prepared in step 5 to the transparent leather obtained in step 4, and dry on a stretch board at 40-60°C for 3-6 hours.
2. The preparation method according to claim 1, characterized in that: The delimed and softened bare hide in step 1 is selected from one of cattle top hide, cattle split hide, sheep hide, goat hide or pig hide.
3. The preparation method according to claim 1, characterized in that: The acid in step 1 is selected from one of sulfuric acid, nitric acid or hydrochloric acid, and the base is selected from one of sodium hydroxide, potassium hydroxide or calcium hydroxide.
4. The preparation method according to claim 1, characterized in that: The oil tanning agent in step 2 is selected from one or more of fish oil, lanolin, castor oil, olive oil, rapeseed oil or linseed oil.
5. The preparation method according to claim 1, characterized in that: The bleaching liquid in step 3 is selected from one of sodium peroxide, hydrogen peroxide, sodium hypochlorite, sodium chlorite or oxalic acid.
6. The preparation method according to claim 1, characterized in that: The water-retaining agent in step 4 is selected from one or more of propylene glycol, sorbitol, polyethylene glycol, glycerol, sodium hyaluronate, urea or trehalose.
7. The preparation method according to claim 1, characterized in that: The rotating speed of the drum in steps 2 and 4 is 80-150 r / min.
8. The preparation method according to claim 1, characterized in that: In step 5, the transparent conductive material is selected from any one of indium tin oxide (ITO), poly(3,4-ethylenedioxythiophene) (PEDOT), poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS), silver nanowires (AgNWs), copper oxide (Cu2O), or a mixture thereof, and the solvent or adhesive is one or more of water, ethanol, isopropanol, tetrahydrofuran, 1,2-dimethoxyethane (DME), epoxy resin, acrylate resin, or polyvinyl chloride.
9. The preparation method according to claim 1, characterized in that: The conductive solution in step 6 is added in a manner selected from one or more of spraying, printing, filtration or dipping.
10. An environmentally friendly transparent conductive leather obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Production method of transparent leather
CN111455118A
Method for producing transparent leather based on organic tanning agent
CN112322806A
Method for manufacturing technical art pig rawhide
JP2003055700A