Operation method for stable and smooth operation of hydrogen-rich carbon circulating oxygen blast furnace

Through the all-oxygen nitrogen distribution method and real-time gas concentration adjustment, the operation problem of hydrogen-rich carbon circulating oxygen blast furnace in stable anterograde operation is solved, and the stable operation and carbon emission reduction goals of the blast furnace are achieved.

CN118932127APending Publication Date: 2024-11-12XINJIANG BAYI IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410989831.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The hydrogen-rich carbon circulating oxygen blast furnace has insufficient control capabilities in stable forward operation, which leads to difficult operation problems, affecting its advantages in carbon reduction process technology.

Method used

Use all-oxygen nitrogen to blow the blast furnace, control the concentration of oxygen, nitrogen and decarbonized gas, observe the differential pressure and material line movement of the blast furnace in real time, adjust the gas ratio to ensure the direct movement of the blast furnace, and gradually adjust the reduction during stable operation. Nitrogen, increase the amount of decarbonized gas spray to increase the effective reduction gas content.

Benefits of technology

The stable forward operation of the blast furnace is achieved, the efficiency of furnace charge reduction is improved, carbon emissions is reduced, and the safety and efficiency of blast furnace operation is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932127A_ABST
    Figure CN118932127A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of blast furnace smelting, and particularly discloses an operation method for stable and smooth operation of a hydrogen-carbon-rich circulating oxygen blast furnace, the main structure of a furnace charge is high-alkalinity sintered ore and acid pellets, and the method comprises the following steps: blowing air into the blast furnace in a mode of total oxygen and nitrogen in the initial stage of blowing, intermittently adding decarburized coal gas, the oxygen concentration is controlled between 21% and 28%; the blast furnace differential pressure and stockline action are observed in real time in the blowing period, whether the blast furnace runs smoothly or not is judged according to the blast furnace differential pressure and stockline action, and if yes, blast continues to be conducted on the blast furnace; if not, stopping air supply immediately; if the furnace is difficult to run and the furnace condition is continuously deteriorated, reducing oxygen, reducing decarburized coal gas and adding nitrogen until the furnace runs smoothly; during the stable operation period, nitrogen is gradually reduced, the injection amount of the decarburized coal gas is gradually increased, and the oxygen concentration in the comprehensive injection gas is controlled within the range of 23-30%. The invention solves the problem of difficult smooth operation of the hydrogen-rich carbon cycle oxygen blast furnace, and realizes the effects of carbon reduction and emission reduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of blast furnace smelting, and in particular to a method for operating a hydrogen-rich carbon cycle oxygen blast furnace in a stable and forward manner. Background Art

[0002] At present, 90% of pig iron in China is produced by traditional blast furnace ironmaking process. The carbon emissions of blast furnace ironmaking process account for more than 70% of the carbon emissions of the steel metallurgical industry. The traditional blast furnace has developed into an extremely efficient reactor today. The theory and technology of high production, low consumption, long life, efficiency, high quality and environmental protection have developed to its peak. Its efficiency and status cannot be completely replaced by other processes. If we can make technological breakthroughs in the existing traditional blast furnaces and make the blast furnaces green and low-carbon, it will surely become an innovation point for the development of low-carbon technology in traditional blast furnaces. However, traditional blast furnaces need to consume a lot of coke to supplement the heat required for iron oxide reduction and soft melting, and the traditional blast furnace ironmaking fuel has reached its limit.

[0003] The emergence of the hydrogen-rich carbon cycle oxygen blast furnace has achieved major technological breakthroughs in traditional blast furnace full oxygen smelting, top gas decarbonization and heating and recycling, and hydrogen-rich metallurgical technology, enabling traditional blast furnaces to reduce carbon emissions by more than 30%. Due to the special process properties of the hydrogen-rich carbon cycle oxygen blast furnace, the operating technology to ensure the stable and smooth operation of the blast furnace is not mature, and the lack of control ability makes it difficult to control the smooth operation of the hydrogen-rich carbon cycle oxygen blast furnace, resulting in the inability to properly exert its technological advantages in carbon reduction. Summary of the invention

[0004] The object of the present invention is to provide a method for operating a hydrogen-rich carbon cycle oxygen blast furnace in a stable and smooth operation, so as to solve the problem that the hydrogen-rich carbon cycle oxygen blast furnace is difficult to operate due to inadequate control of the smooth operation of the hydrogen-rich carbon cycle oxygen blast furnace.

[0005] To achieve the above object, the present invention provides a method for operating a hydrogen-rich carbon cycle oxygen blast furnace in a stable and forward manner, characterized in that the main structure of the charge is a high-basicity sintered ore with acidic pellets, the basicity of the sintered ore is between 2.2 and 2.6 times, and the magnesium oxide in the sintering is not less than 2%, and the method comprises:

[0006] S1: At the beginning of the blast, the blast furnace is blown with full oxygen and nitrogen, and then decarbonized coal gas is added intermittently. The total amount of each gas addition is controlled within 5%, and the interval time is not less than 3 minutes. The oxygen concentration is controlled between 21-28%, and the concentration of carbon monoxide in the decarbonized coal gas is controlled to be not less than 60%, and the concentration of carbon dioxide is controlled to be less than 3%;

[0007] S2: During the blowing period, the blast furnace differential pressure and the action of the material line are observed in real time, and according to the blast furnace differential pressure and the action of the material line, it is judged whether the blast furnace is running smoothly. If the blast furnace is running smoothly, the blast furnace is blown in accordance with the blowing method at the initial stage of the blast opening; if the blast furnace is difficult to run, the air addition is stopped immediately; if the blast furnace is difficult to run and the furnace condition continues to deteriorate, oxygen and decarbonized coal gas are reduced, and nitrogen is added until the blast furnace runs smoothly;

[0008] S3: During stable operation, gradually reduce nitrogen and gradually increase the injection amount of decarbonized coal gas to keep the oxygen concentration in the comprehensive injection gas within the range of 23-30% to increase the content of effective reducing gas in the injection gas; the stable operation period is when the blast furnace has achieved full oxygen and full air volume operation, and the number of hourly material running batches reaches 5 batches or more; the effective reducing gas mainly contains carbon monoxide and hydrogen.

[0009] The present invention aims at the special process properties of the hydrogen-rich carbon cycle oxygen blast furnace. The operation technology to ensure the stable and smooth operation of the blast furnace is not mature, the control ability is insufficient, and the smooth operation of the hydrogen-rich carbon cycle oxygen blast furnace is difficult to control. The blast furnace is blasted by using a method of all-oxygen and nitrogen. If the blast furnace is difficult to operate or further deteriorates, the concentrations of oxygen, nitrogen, and decarbonized coal gas in the blast process are controlled and adjusted to make the blast furnace run smoothly; nitrogen is reduced under the stable and smooth operation of the blast furnace, and the injection amount of decarbonized coal gas is gradually increased to increase the content of effective reducing gas in the injection gas, which can quickly complete the reduction reaction of the charge and improve the reduction efficiency of the charge. The method provided by the present invention not only solves the problem of the smooth operation of the hydrogen-rich carbon cycle oxygen blast furnace during operation, but also realizes the carbon reduction and emission reduction of the blast furnace ironmaking process.

[0010] Preferably, if the blast furnace is difficult to operate and the furnace condition continues to deteriorate, reduce oxygen, reduce decarbonization gas, and add nitrogen until the blast furnace operates smoothly, specifically including: gradually reducing the decarbonization gas by 5-10% each time, increasing the nitrogen by 5-10% each time, and reducing the oxygen by 5-10% each time according to the total oxygen concentration range of 21-25% until the blast furnace operates smoothly.

[0011] The present invention proposes that when the blast furnace is difficult to operate and the furnace condition continues to deteriorate, in order to ensure the safe operation of the blast furnace, the gas concentration of the blast furnace is gradually and slowly adjusted, the decarbonized coal gas is reduced by 5-10% each time, the nitrogen is increased by 5-10% each time, and the oxygen is reduced by 5-10% each time according to the requirement of the total oxygen concentration range of 21-25%, thereby preventing the furnace condition from further deteriorating and ensuring the safe operation of the blast furnace.

[0012] Preferably, during stable operation, nitrogen is gradually reduced and the decarbonized coal gas injection amount is gradually increased, specifically including: gradually reducing nitrogen by 10-20% each time, and gradually increasing the decarbonized coal gas injection amount by 10-20% each time, blowing in oxygen, and keeping the oxygen concentration in the comprehensive injection gas within the range of 23-30%.

[0013] The present invention achieves a steady increase in the effective reducing gas in the injected gas by gradually reducing nitrogen by 10-20% each time and gradually increasing the injection amount of decarbonized coal gas by 10-20% each time during stable operation, injecting oxygen, and maintaining the oxygen concentration in the comprehensive injected gas within the range of 23-30%.

[0014] Preferably, the method further comprises: before the blast furnace is shut down for maintenance, 20-30% of nitrogen is introduced into the injected coal gas to replace the 20-30% of decarbonized coal gas injection in equal amount.

[0015] In order to ensure the normal operation of the hydrogen-rich carbon cycle oxygen blast furnace, the operating personnel will regularly inspect and maintain the hydrogen-rich carbon cycle oxygen blast furnace. In order to ensure smooth furnace start-up, the present invention proposes to cut into 20-30% nitrogen in the injected coal gas before the blast furnace is overhauled and shut down, and replace 20-30% of the decarbonized coal gas injection in equal amounts to reduce the effective components of the reducing gas in the injected coal gas, thereby achieving the purpose of reducing the reducing potential of the coal gas injected into the blast furnace.

[0016] Preferably, while introducing 20-30% nitrogen into the injected coal gas to replace 20-30% of the decarbonized coal gas injection in equal amount, the following step is also included: reducing the proportion of high basicity sintered ore in the main structure of the furnace charge by 10-20%.

[0017] In order to ensure that the furnace can be opened smoothly after the wind is stopped, the present invention not only adjusts the injected coal gas, but also reduces the proportion of high-basicity sintered ore in the main structure of the charge by 10-20%, effectively avoiding excessive reduction of the charge, reducing the reduction and pulverization of the sintered ore, and creating conditions for the subsequent smooth furnace opening.

[0018] Preferably, while gradually reducing nitrogen and gradually increasing the injection amount of decarbonized coal gas, the following steps are also included: gradually adjusting the proportion of high-basicity sintered ore in the main structure of the furnace charge to a range of 50-70%.

[0019] In order to avoid the rapid pulverization of high-basicity sintered ore during the stable forward operation of the blast furnace, which would affect the forward operation of the blast furnace, the present invention controls the effective reducing gas injected into the blast furnace and adjusts the proportion of high-basicity sintered ore in the main structure of the charge, so that the high-basicity sintered ore can quickly pass through its reduction and pulverization zone, thereby reducing the pulverization effect in the fast zone of the blast furnace and the deterioration of the forward operation of the blast furnace caused by sintering pulverization. On this basis, it is easy to increase the amount of decarbonization coal gas injected, thereby achieving the carbon emission reduction target.

[0020] Preferably, when the blast furnace top temperature is lower than 90°C, the gas injection rate per ton of iron is increased to 50-100m 3 / t, lower the material line by 2-4 meters and adjust the fabric angle by 1-2 degrees.

[0021] With the increase of smelting strength, the top temperature drops greatly. When the top temperature of the blast furnace is lower than 90℃, the present invention proposes to increase the gas injection volume to 50-100m3 / ton of iron. 3 / t, lower the material line by 2-4 meters, adjust the material distribution angle by 1-2 degrees to increase the gas output temperature at the furnace top, reduce the resistance loss of the material column, and increase the injection volume of decarbonized gas to ensure the stable operation of the blast furnace and achieve the goal of reducing fossil energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the operation flow of a method for stably running a hydrogen-rich carbon cycle oxygen blast furnace provided by the present invention;

[0023] Figure 2 It is a process flow diagram of a method for stably and smoothly operating a hydrogen-rich carbon circulating oxygen blast furnace provided by the present invention. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below through specific embodiments:

[0025] The reference numerals in the drawings of the specification include:

[0026] 1. Loading port; 2. Blast furnace gas; 3. Gas purification device; 4. Pipe network; 5. Decarbonization device; 6. Decarbonized gas; 7. Gas heating furnace; 8. Decarbonized gas after heating; 9. Nitrogen; 10. Oxygen; 11. Furnace body gas pressurization heating device; 12. Furnace body nozzle; 13. Iron mouth.

[0027] An embodiment of the present invention provides a method for operating a hydrogen-rich carbon cycle oxygen blast furnace in a stable and forward manner. The method comprises:

[0028] It is understandable that the effective reducing gas (mainly carbon monoxide and hydrogen) in the coal gas exceeds 70%. This part of the reducing gas can quickly complete the reduction reaction of the charge, and will also quickly reduce and pulverize the sintered ore. The pulverized sintered ore has poor air permeability, which will affect the smooth operation of the blast furnace. Therefore, high-basicity sintered ore and acidic pellets are used as the main structure of the charge. The basicity of the sintered ore is between 2.2-2.6 times, and the magnesium oxide in the sintering is not less than 2%.

[0029] S1: At the beginning of the blast, the blast furnace is blown with full oxygen and nitrogen, and then decarbonized coal gas 6 is added intermittently. The total amount of gas added each time is controlled within 5%, and the interval time is not less than 3 minutes. The concentration of oxygen 10 is controlled between 21-28%, and the concentration of carbon monoxide in the decarbonized coal gas 6 is controlled to be not less than 60%, and the concentration of carbon dioxide is controlled to be less than 3%.

[0030] It is understandable that in S1, oxygen 10 and nitrogen 9 are added after the furnace top charging line starts to move, and decarbonized coal gas 6 is further added to reduce the effective components of reducing gas in the coal gas, prevent the sintered ore in the charge from being reduced and pulverized too early at low temperature, and thus realize the smooth operation of the blast furnace in the initial stage of opening the blast furnace, creating conditions for adding decarbonized coal gas 6 in the next stage.

[0031] S2: During the blowing period, observe the blast furnace differential pressure and the material line movement in real time, and judge whether the blast furnace is running smoothly based on the blast furnace differential pressure and the material line movement. If the blast furnace is running smoothly, continue to blow air into the blast furnace according to the blowing method at the beginning of the blast; if the blast furnace is difficult to run, stop adding air immediately; if the blast furnace is difficult to run and the furnace condition continues to deteriorate, reduce oxygen by 10, reduce decarbonized coal gas by 6, and add nitrogen by 9 until the blast furnace runs smoothly.

[0032] It can be understood that during the blowing period, if the blast furnace differential pressure does not rise significantly and the material line movement continues, it means that the blast furnace is running smoothly, that is, it continues to follow the blast mode at the initial stage of opening the wind, adopts the method of full oxygen and nitrogen 9 to blow air into the blast furnace, and then intermittently adds decarbonized coal gas 6; if the blast furnace differential pressure rises to a preset differential pressure threshold (which can be set according to the actual operating state of the blast furnace, and is not limited in the present embodiment), and the material line movement is sluggish, it means that the furnace condition is difficult to operate, that is, immediately stop adding air to the blast furnace; if the blast furnace differential pressure rises to the upper limit value of the preset differential pressure threshold, and the material line movement is seriously sluggish, it means that the blast furnace is difficult to operate and the furnace condition continues to deteriorate, that is, reduce oxygen 10, reduce decarbonized coal gas 6, and add nitrogen 9 until the blast furnace runs smoothly, that is, gradually reduce the decarbonized coal gas 6 by 5-10% each time, increase the nitrogen 9 by 5-10% each time, and reduce the oxygen 10 by 5-10% each time according to the range of the total oxygen concentration of 21-25%, until the blast furnace runs smoothly.

[0033] S3: During stable operation, gradually reduce nitrogen 9, and gradually increase the injection amount of decarbonized coal gas, keep the oxygen concentration in the comprehensive injection gas within the range of 23-30%, so as to increase the content of effective reducing gas in the injection gas; wherein, the stable operation period is the period when the blast furnace has achieved full oxygen and full air volume operation, and the number of hourly material running batches reaches 5 batches or more; the effective reducing gas mainly contains carbon monoxide and hydrogen.

[0034] This step S3 specifically includes: gradually reducing the nitrogen 9 by 10-20% each time, and gradually increasing the decarbonized coal gas injection amount by 10-20% each time, blowing in oxygen 10, and maintaining the oxygen concentration in the comprehensive injection gas within the range of 23-30%. Under the condition of slow material speed in the early stage, a steady increase in the effective reducing gas in the injection gas is achieved.

[0035] In order to avoid the rapid pulverization of high-basicity sintered ore in the forward operation of the blast furnace, which affects the forward operation of the blast furnace, the embodiment of the present invention proposes to adjust the proportion of high-basicity sintered ore in the main structure of the charge to reduce the pulverization of high-basicity sintered ore. Specifically: during the stable operation period, while adjusting the decarbonization coal gas injection amount and nitrogen 9, the proportion of high-basicity sintered ore in the main structure of the charge is gradually adjusted to the range of 50-70%. During the stable operation period of the embodiment of the present invention, after the material speed reaches more than 5 batches, by controlling the effective reducing gas injected into the blast furnace and adjusting the proportion of high-basicity sintered ore in the main structure of the charge, the high-basicity sintered ore can quickly pass through its reduction and pulverization interval, reducing its pulverization effect in the fast zone of the blast furnace, reducing the deterioration of the forward operation of the blast furnace caused by sintering pulverization, and on this basis, it is easy to increase the decarbonization coal gas injection amount, thereby achieving the carbon emission reduction target.

[0036] It should be understood that in order to ensure the normal operation of the hydrogen-rich carbon cycle oxygen blast furnace, the operating personnel will regularly inspect and maintain the hydrogen-rich carbon cycle oxygen blast furnace. In order to ensure smooth furnace opening, the embodiment of the present invention proposes to cut in 20-30% nitrogen 9 in the injected coal gas before the furnace is opened and the wind is shut down, and replace the 20-30% decarbonized coal gas 6 with an equal amount to reduce the content of the effective reducing gas in the injected coal gas, reduce the reduction potential of the blast furnace gas 2, and at the same time reduce the proportion of high-basicity sintered ore in the main structure of the charge by 10-20%, effectively avoiding excessive reduction of the charge, reducing the reduction pulverization of the sintered ore, and creating conditions for the subsequent smooth furnace opening. (The furnace opening steps after the inspection are completed follow steps S1, S2 and S3).

[0037] With the increase of smelting strength, the top temperature drops greatly. When the top temperature of the blast furnace is lower than 90°C, the embodiment of the present invention proposes to increase the gas injection volume by 50-100m3 per ton of iron. 3 / t, lower the material line by 2-4 meters and adjust the material distribution angle by 1-2 degrees to increase the gas output temperature at the furnace top, reduce the resistance loss of the material column, and increase the injection volume of decarbonized gas to ensure the stable operation of the blast furnace and achieve the goal of reducing fossil energy consumption.

[0038] It can be understood that the process flow of the embodiment of the present invention is specifically as follows: the charge is added to the hydrogen-rich carbon circulating oxygen blast furnace through the charging port 1, the blast furnace gas 2 in the hydrogen-rich carbon circulating oxygen blast furnace enters the pipeline 4 and the decarbonization device 5 respectively through the gas purification device 3, the decarbonization device 5 decarbonizes the purified blast furnace gas 2 to obtain decarbonized gas 6, and then the decarbonized gas 6 is input into the gas heating furnace 7 for heating to obtain heated decarbonized gas 8, and further the oxygen 10, the heated decarbonized gas 8 and the nitrogen 9 are adjusted to ensure the smooth running of the blast furnace, and the molten iron and slag are discharged through the iron mouth 13; the furnace body gas in the hydrogen-rich carbon circulating oxygen blast furnace is adjusted by the furnace body gas pressurized heating device 11 through the furnace body nozzle 12.

[0039] The embodiment of the present invention aims at the special process properties of the hydrogen-rich carbon cycle oxygen blast furnace. The operation technology to ensure the stable and smooth operation of the blast furnace is still immature, the control ability is insufficient, and the smooth operation of the hydrogen-rich carbon cycle oxygen blast furnace is difficult to control. The blast furnace is blasted by using a method of all-oxygen and nitrogen. If the blast furnace is difficult to operate or further deteriorates, the concentrations of oxygen 10, nitrogen 9, and decarbonized coal gas 6 in the blasting process are controlled and adjusted to make the blast furnace run smoothly; when the blast furnace is running stably and smoothly, the nitrogen 9 is reduced, and the injection amount of decarbonized coal gas is gradually increased to increase the content of effective reducing gas in the injected gas. The effective reducing gas can quickly complete the reduction reaction of the charge and improve the reduction efficiency of the charge. The method provided by the embodiment of the present invention not only solves the problem of the smooth operation of the furnace condition of the hydrogen-rich carbon cycle oxygen blast furnace during operation and start-up and shutdown for maintenance, but also achieves carbon reduction and emission reduction in the blast furnace ironmaking process.

[0040] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for operating a hydrogen-rich carbon cycle oxygen blast furnace in a stable and forward manner. It is characterized in that The main structure of the charge is high-basicity sintered ore with acidic pellets, the basicity of the sintered ore is between 2.2 and 2.6 times, and the magnesium oxide in the sintering is not less than 2%. The method comprises: S1: At the beginning of the blast furnace, the blast furnace is blown with full oxygen and nitrogen, and then decarbonized coal gas (6) is added intermittently, the total amount of each gas addition is controlled within 5%, and the interval time is not less than 3 minutes, the oxygen concentration is controlled between 21-28%, and the concentration of carbon monoxide in the decarbonized coal gas (6) is controlled to be not less than 60%, and the concentration of carbon dioxide is controlled to be less than 3%; S2: During the blowing period, the blast furnace differential pressure and the material line movement are observed in real time, and according to the blast furnace differential pressure and the material line movement, it is determined whether the blast furnace is running smoothly. If the blast furnace is running smoothly, the blast furnace is continued to be blown according to the blowing method at the initial stage of opening the blast furnace; if the blast furnace is difficult to run, the air addition is stopped immediately; if the blast furnace is difficult to run and the furnace condition continues to deteriorate, oxygen (10) is reduced, decarbonized coal gas (6) is reduced, and nitrogen (9) is added until the blast furnace runs smoothly; S3: During stable operation, gradually reduce nitrogen (9) and gradually increase the injection amount of decarbonized coal gas to maintain the oxygen concentration in the comprehensive injection gas within the range of 23-30% to increase the content of effective reducing gas in the injection gas; wherein, the stable operation period is a period when the blast furnace has achieved full oxygen and full air volume operation and the number of hourly material running batches reaches 5 batches or more; the effective reducing gas mainly contains carbon monoxide and hydrogen.

2. The stable and forward operation method of the hydrogen-rich carbon cycle oxygen blast furnace according to claim 1, It is characterized in that If the blast furnace is difficult to operate and the furnace condition continues to deteriorate, then reduce oxygen (10), reduce decarbonized coal gas (6), and add nitrogen (9) until the blast furnace operates smoothly, specifically including: gradually reducing the decarbonized coal gas (6) by 5-10% each time, increasing the nitrogen (9) by 5-10% each time, and reducing the oxygen (10) by 5-10% each time according to the total oxygen concentration range of 21-25% until the blast furnace operates smoothly.

3. The stable and forward operation method of the hydrogen-rich carbon cycle oxygen blast furnace according to claim 1, It is characterized in that During the stable operation, the nitrogen (9) is gradually reduced, and the decarbonized coal gas injection amount is gradually increased, specifically including: gradually reducing the nitrogen (9) by 10-20% each time, and gradually increasing the decarbonized coal gas injection amount by 10-20% each time, blowing in oxygen (10), and maintaining the oxygen concentration in the comprehensive injection gas within the range of 23-30%.

4. The method for operating a hydrogen-rich carbon cycle oxygen blast furnace in a stable and forward manner according to claim 1, It is characterized in that The method further comprises: before the blast furnace is shut down for maintenance, 20-30% of nitrogen (9) is introduced into the injected coal gas, and an equal amount of 20-30% of decarbonized coal gas (6) is injected to replace the injected gas.

5. The method for operating a hydrogen-rich carbon cycle oxygen blast furnace in a stable and forward manner according to claim 4, It is characterized in that While cutting in 20-30% nitrogen (9) into the injected coal gas to replace 20-30% of the decarbonized coal gas (6) for injection, the following steps are also included: reducing the proportion of high-basicity sintered ore in the main structure of the furnace charge by 10-20%.

6. The method for operating a hydrogen-rich carbon cycle oxygen blast furnace in a stable and forward manner according to claim 1, It is characterized in that While gradually reducing the nitrogen (9) and gradually increasing the injection amount of the decarbonized coal gas, the method further includes the following steps: gradually adjusting the proportion of high-basicity sintered ore in the main structure of the furnace charge to a range of 50-70%.

7. The method for operating a hydrogen-rich carbon cycle oxygen blast furnace in a stable and forward manner according to claim 1, It is characterized in that When the top temperature of the blast furnace is lower than 90℃, the gas injection volume per ton of iron is increased to 50-100m 3 / t, lower the material line by 2-4 meters and adjust the fabric angle by 1-2 degrees.