Method for regulating and controlling inclusions in steel and preparation method and application of IF steel

By adding aluminum-magnesium alloy during the preparation of IF steel to generate fine MgO-Al2O3 inclusions, the problems of continuous casting nodules and rolling defects caused by Al2O3 inclusions in IF steel are solved, thereby improving production efficiency and product quality.

CN118932137APending Publication Date: 2024-11-12HUNAN VALIN LIANYUAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411015569.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively control Al2O3 inclusions in IF steel, leading to nodule formation in continuous casting nozzles, accumulation of inclusions in the crystallizer, and sand hole defects in the final product. Furthermore, existing magnesium treatment technologies require additional equipment and extend smelting time.

Method used

In the preparation of IF steel, aluminum-magnesium alloy is added for deoxidation and alloying, generating fine MgO-Al2O3 inclusions. The inclusions are removed by vacuum control and RH cycle optimization, reducing smelting time.

Benefits of technology

This resulted in a reduction of 1/3 to 1/2 in the number of inclusions in IF steel, a reduction in size to 8μm, the removal of stopper rods and SEN nozzle nodules, and an improvement in production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965583960000071
    Figure BDA0004965583960000071
  • Figure BDA0004965583960000081
    Figure BDA0004965583960000081
Patent Text Reader

Abstract

The invention relates to the technical field of metal casting, in particular to a method for regulating and controlling inclusions in steel and a preparation method and application of IF steel. The method comprises the following steps: adding an aluminum-magnesium alloy into molten steel to carry out deoxidation alloying treatment; wherein in the aluminum-magnesium alloy, the mass fraction of magnesium is 2%-4%. According to the method, an aluminum-magnesium alloy containing 2%-4% of magnesium is added, so that oxide inclusions in the steel are fine and dispersed, and MgO-Al2O3 inclusions are mainly used. According to the method, the effect of removing the inclusions through soft blowing of the IF steel is fully utilized, and the inclusion removal effect is better; meanwhile, according to the method, the smelting time prolonged due to the fact that a wire feeding device is adopted for adding magnesium traditionally is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal casting, and in particular to a method for regulating inclusions in steel, a preparation method of IF steel and its application. Background Art

[0002] IF steel is mainly used as high-end stamping plates, such as automobile panels and home appliance plates, and has strict requirements on the surface quality of the products. The current typical IF steelmaking process is molten iron pre-desulfurization → converter → RH refining → conventional slab continuous casting. One of the important factors affecting the surface quality of the plate is the cleanliness of the molten steel and the inclusions in the steel. The aluminum deoxidation process of IF steel will generate a large number of Al2O3 inclusions, which are easy to cause nodules in the continuous casting nozzle. Some nodules of Al2O3 inclusions enter the crystallizer under the action of molten steel scouring, becoming large-sized inclusions in the continuous casting billet. After rolling, they become linear defects on hot-rolled coils or cold-rolled coils, resulting in the scrapping or downgrading of the product. In addition, Al2O3 inclusions themselves are also very easy to aggregate with each other to form relatively large clusters of inclusions, which are distributed in the steel billet matrix. These inclusions may cause sand hole defects in the final stamping process of the finished plate, thereby seriously affecting the product quality. In order to control the Al2O3 inclusions in IF steel, the main methods currently used are: ① reducing the oxygen content in molten steel to reduce the amount of Al2O3 inclusions generated; ② magnesium treatment technology.

[0003] In order to reduce the oxygen content in molten steel to reduce the amount of Al2O3 inclusions generated, the prior art discloses a method for producing IF steel for automobile outer panels without inclusion defects, which requires that the oxygen content at the converter end point is between 250ppm and 550ppm, the oxygen content at the RH decarburization end point is ≤350ppm, and the content of oxidizing components in the ladle slag is ≤4.0%. In addition, the tundish uses a flow stabilizer, a high retaining wall and a filter to control the flow to remove the Al2O3 inclusions that have been produced in the steel as much as possible. However, no matter how the method of controlling the oxygen content in IF steel is controlled, more Al2O3 deoxidation products are still inevitably produced in the steel, which eventually become relatively large Al2O3 inclusions.

[0004] As for magnesium treatment technology, the prior art discloses a method for improving the magnesium modification effect of IF steel. At the end of RH refining, magnesium-containing cored wire is fed into the molten steel by a segmented precision wire feeding method, and Al2O3 inclusions in IF steel are modified into fine and dispersed MgO-Al2O3 inclusions, and the mass percentage of MgO in MgO-Al2O3 is 22% to 100%. However, the magnesium wire feeding process of this method is divided into 2-3 times, and a soft blowing time of 5min to 15min is required after wire feeding. A certain amount of MgO-Al2O3 inclusions in the steel are removed by soft blowing, so as to ensure that the stopper rod does not rise during the continuous casting of the molten steel. Not only does it need to add additional wire feeding equipment in the RH process and prolong the smelting time, but it also wastes the effective removal effect of the RH vacuum treatment pure circulation process on inclusions in the molten steel. Summary of the invention

[0005] In order to solve the above problems, the present application proposes a method for regulating inclusions in steel, a method for preparing IF steel and its application. The method adds aluminum-magnesium alloy in the alloying step, which not only reduces the smelting time, but also reduces the number and size of MgO-Al2O3 composite inclusions.

[0006] This application is implemented through the following technical solutions:

[0007] In the first aspect, the present application proposes a method for regulating inclusions in steel, comprising the following steps:

[0008] Adding aluminum-magnesium alloy to molten steel for deoxidation and alloying treatment;

[0009] Wherein, the mass fraction of magnesium in the aluminum-magnesium alloy is 2% to 4%.

[0010] The first aspect of the present application proposes a method for regulating inclusions in steel, adding an aluminum-magnesium alloy containing 2% to 4% magnesium to make the oxide inclusions in the steel fine and dispersed, mainly MgO-Al2O3 inclusions. This method makes full use of the role of soft blowing in removing inclusions in IF steel, and the inclusion removal effect is better; at the same time, this method shortens the smelting time that is prolonged by adding magnesium using traditional wire feeding equipment. After the aluminum-magnesium alloy is added to the molten steel, a reaction of 2[Al]+[Mg]+4(O)=MgO-Al2O3 will occur, and the generated MgO-Al2O3 spinel is a high-melting-point compound of 2000°C, which is a solid particle in the molten steel and has a sharp octahedral structure, and is not easy to collide and grow in the molten steel. Therefore, the inclusions have the characteristics of being fine and dispersed.

[0011] In some possible implementations, the amount of aluminum-magnesium alloy added is 0.6kg / t to 1.2kg / t. The amount of aluminum-magnesium alloy added is mainly determined by the oxygen content in the molten steel before deoxidation and the Al content required by the produced IF steel itself. The added aluminum-magnesium alloy first reacts with the oxygen in the steel, and the unreacted aluminum can ensure that the Al element content in the molten steel reaches the requirement of 200 to 1000ppm for IF steel under normal conditions. The requirement of 2% to 4% magnesium in the aluminum-magnesium alloy ensures that there is enough Mg element in the molten steel to make the product of the deoxidation reaction MgO-Al2O3 instead of Al2O3. When 0.6kg / t to 1.2kg / t of the aluminum-magnesium alloy is added, the inclusions in the obtained steel are mainly MgO-Al2O3 composite inclusions.

[0012] In some possible implementations, the mass fraction of aluminum in the aluminum-magnesium alloy is more than 95%. Within this component range, it is ensured that Al is still the main element for deoxidation of the molten steel, because the deoxidation effect of the Al element is stable and thorough. At the same time, because the boiling point of Mg is 1090°C, the solubility of Mg in molten steel is limited, especially under extreme vacuum (≤100Pa), the solubility of Mg in molten steel is almost 0, so excess Mg is very easy to volatilize and dissipate in the molten steel. Therefore, the proportion of magnesium in the aluminum-magnesium alloy cannot be too high, otherwise it will cause a waste of Mg element. After adding the aluminum-magnesium alloy, it is sufficient to ensure that the Mg element in the steel is sufficient to generate MgO-Al2O3 composite inclusions.

[0013] In some possible implementations, the deoxidation alloying treatment step includes: adding the aluminum-magnesium alloy at a vacuum degree of 5kPa to 7kPa, and then performing RH circulation. Vacuum degree is the basic condition to ensure the circulation of molten steel in the RH furnace. Through practical exploration, under a vacuum degree of 5kPa to 7kPa, on the one hand, the molten steel can circulate normally in the RH furnace, and the relative movement speed between the molten steel and the slag surface is smaller than that under the ultimate vacuum degree, which is conducive to the floating of inclusions in the molten steel into the slag; on the other hand, under this vacuum degree, the Mg element has a greater solubility in the molten steel and is not easy to volatilize, which ensures the smooth progress of the magnesium-aluminum deoxidation reaction.

[0014] Furthermore, the RH cycle time is 4 to 6 minutes. Within this cycle time range, full use is made of the soft blowing of steel to remove inclusions, so that most of the inclusions generated by deoxidation in the steel float to the slag, and the inclusion removal effect is better.

[0015] In the second aspect, the present application proposes a method for preparing IF steel, comprising the steps of converter steelmaking, RH refining, continuous casting and rolling; wherein the RH refining step comprises: after decarburizing the molten steel, using the method for regulating inclusions in steel provided in the present application to regulate the oxide inclusions in the steel, and then adding ferrotitanium alloy for ferrotitanium alloying treatment.

[0016] The preparation method of IF steel of the present application adopts the method for regulating inclusions in steel provided by the present application to optimize oxide inclusions in molten steel. There is no accumulation of inclusions in the stopper rod and SEN nozzle (immersion nozzle) during the continuous casting process, the liquid level of the crystallizer is stable, and the oxide inclusions in the molten steel of the tundish and the hot-rolled coil are mainly MgO-Al2O3 composite inclusions. Compared with the conventional aluminum deoxidation process of IF steel, the number of inclusions is reduced by 1 / 3 to 1 / 2, the size of the inclusions is smaller, and the average size of the oxide inclusions is reduced from 12μm to 8μm. Compared with the method of adding magnesium wire to the wire feeder, the refining treatment time is shortened by 15min, the wire feeding operation is omitted, and the production efficiency is improved.

[0017] In some possible implementations, the amount of the titanium-iron alloy added is 0.3 kg / t to 0.6 kg / t.

[0018] In some possible implementations, the titanium-iron alloying treatment step includes: adding the titanium-iron alloy under a vacuum degree of 5 kPa to 7 kPa, and then performing RH cycle and then breaking the vacuum to exit the station.

[0019] Furthermore, the RH cycle time in the titanium-iron alloying step is 3 minutes to 5 minutes.

[0020] In some possible implementations, the final oxygen content of the converter steelmaking is 500ppm to 800ppm. Within this final oxygen content range, it can be ensured as much as possible that no additional oxygen blowing is required during the RH treatment process, and the oxygen after decarburization is 300ppm to 400ppm.

[0021] In some possible implementations, the slag is modified after the converter steelmaking process, so that the iron oxide content in the RH incoming slag is not higher than 6.0%. In this case, no obvious secondary oxidation caused by the ladle slag or the generation of additional Al2O3 inclusions will occur.

[0022] In some possible implementations, in the decarburization step of the RH refining, the oxygen content at the RH decarburization endpoint is 300ppm-400ppm, and the vacuum degree is 10Pa-100Pa. At this time, the ultimate vacuum degree of RH ensures the effect and production efficiency of RH deep decarburization.

[0023] Furthermore, the IF steel is IF steel for automobile plates, household appliance plates or building plates.

[0024] In a third aspect, the present application proposes an application of the method for regulating inclusions in steel provided by the present application in steel smelting. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0026] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.

[0027] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.

[0028] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0029] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0030] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0031] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0032] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0033] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0034] Example 1

[0035] This embodiment provides a method for controlling inclusions in steel, comprising the following steps:

[0036] Under a vacuum degree of 6.2 kPa, 164 kg of aluminum-magnesium alloy was added to 205 t of molten steel for deoxidation and alloying treatment; wherein the mass fraction of Mg in the aluminum-magnesium alloy was 3.0%.

[0037] This embodiment also provides a method for preparing IF steel, comprising the following steps:

[0038] (1) Converter steelmaking: A 210t converter is used to smelt IF steel molten steel, with a molten steel output of 205t. The final oxygen content of the converter is controlled at 657ppm.

[0039] (2) Modification: After steel is tapped, 400 kg of Al40 modifier is added to the slag for modification.

[0040] (3) RH refining:

[0041] ① Decarburization: The iron oxide content in the RH incoming slag is 5.5%. Using 100Pa ultimate vacuum decarburization, the oxygen end point of RH decarburization is 372ppm.

[0042] ② Control inclusions: After decarburization, the RH vacuum degree was adjusted from 85Pa to 6.2kPa, and 164Kg (0.8kg / t) of aluminum-magnesium alloy was added at one time for deoxidation and alloying. Then the RH cycle was continued for 5 minutes, and most of the inclusions generated by deoxidation in the steel floated to the slag; the mass fraction of Mg in the aluminum-magnesium alloy was 3.0%.

[0043] ③Titanium-iron alloying: Add 80Kg of titanium-iron alloying, then RH cycle for 4 minutes before breaking through the air and leaving the station.

[0044] (4) The molten steel after leaving the station is continuously cast and rolled to obtain hot-rolled coils of IF steel.

[0045] Example 2

[0046] Example 2 proposes a method for regulating inclusions in steel and a method for preparing IF steel. The steps are basically the same as those in the example, except that the mass of the added aluminum-magnesium alloy is 123 kg (0.6 kg / t).

[0047] Example 3

[0048] Example 3 proposes a method for regulating inclusions in steel and a method for preparing IF steel. The steps are basically the same as those in the example, except that the mass of the added aluminum-magnesium alloy is 246 kg (1.2 kg / t).

[0049] Example 4

[0050] Example 4 proposes a method for regulating inclusions in steel and a method for preparing IF steel. The steps are basically the same as those in the example, except that the mass fraction of magnesium in the added aluminum-magnesium alloy is 2%.

[0051] Example 5

[0052] Example 5 proposes a method for regulating inclusions in steel and a method for preparing IF steel. The steps are basically the same as those in the example, except that the mass fraction of magnesium in the added aluminum-magnesium alloy is 4%.

[0053] Comparative Example 1

[0054] Comparative Example 1 proposes a method for preparing IF steel, comprising the following steps:

[0055] (1) Converter steelmaking: A 210t converter is used to smelt IF steel molten steel, with a molten steel output of 205t. The final oxygen content of the converter is controlled at 657ppm.

[0056] (2) Modification: After steel is tapped, 400 kg of Al40 modifier is added to the slag for modification.

[0057] (3) RH refining:

[0058] ① Decarburization: The iron oxide content in the RH incoming slag is 5.5%. The oxygen content at the RH decarburization endpoint is 372ppm.

[0059] ②Control inclusions: After decarburization, the RH vacuum is adjusted from 85Pa to 6.2kPa, and 164Kg of pure aluminum blocks are added at one time for deoxidation and alloying, followed by RH circulation for 5 minutes.

[0060] ③Titanium-iron alloying: add 80kg of titanium-iron alloying, then RH cycle for 4 minutes before breaking through the air and leaving the station.

[0061] (4) The steel after leaving the station is continuously cast and rolled to obtain hot-rolled coils of IF steel.

[0062] Comparative Example 2

[0063] Comparative Example 2 proposes a method for preparing IF steel, and the steps are basically the same as those of Example 1, except that the amount of aluminum-magnesium alloy added is 307.5 kg (1.5 kg / t).

[0064] Comparative Example 3

[0065] Comparative Example 3 proposes a method for preparing IF steel, and the steps are basically the same as those of Example 1, except that the amount of aluminum-magnesium alloy added is 102.5 kg (0.5 kg / t).

[0066] Comparative Example 4

[0067] Comparative Example 4 proposes a method for preparing IF steel, and the steps are basically the same as those of Example 1, except that the mass fraction of Mg in the aluminum-magnesium alloy is 5.0%.

[0068] Comparative Example 5

[0069] Comparative Example 5 proposes a method for preparing IF steel, and the steps are basically the same as those of Example 1, except that the mass fraction of Mg in the aluminum-magnesium alloy is 1.0%.

[0070] In order to verify the progress of the above embodiments, the number, size and oxide composition of oxide inclusions in the tundish molten steel and hot-rolled coils in the IF steel preparation process of Examples 1 to 5 and Comparative Examples 1 to 5 were tested. At the same time, the accumulation and nodulation of inclusions in the stopper rod and SEN nozzle during the continuous casting process were observed. The results are shown in Table 1 below.

[0071] Table 1

[0072]

[0073]

[0074] It can be seen from Table 1 above:

[0075] (1) It can be seen from Example 1 and Comparative Example 1 that there is no accumulation of inclusions in the stopper rod and SEN nozzle during the continuous casting process of Example 1, and the liquid level of the crystallizer is stable. The oxide inclusions in the molten steel in the tundish and the hot-rolled coil are mainly MgO-Al2O3 composite inclusions, with fewer inclusions and smaller sizes.

[0076] (2) It can be seen from Examples 1 to 3 and Comparative Examples 2 to 3 that too much or too little addition of aluminum-magnesium alloy will deteriorate the cleanliness of IF steel. When too much is added, the Al content in the steel is high, and secondary oxidation is more likely to occur, generating additional Al2O3 inclusions. When too little is added, the degree of deoxidation of the molten steel is not thorough enough, and the inclusions generated in the steel are not easy to float up and remove.

[0077] (4) It can be seen from Examples 1, 4 and 5 and Comparative Examples 4 to 5 that the addition of an aluminum-magnesium alloy containing 2% to 4% magnesium makes the oxide inclusions in the steel fine and dispersed, so that there is no accumulation of inclusions in the stopper rod and SEN nozzle during the continuous casting process, and the oxide inclusions in the molten steel in the tundish and the hot-rolled coil are mainly MgO-Al2O3 composite inclusions, and the number of inclusions is smaller and the size is smaller. The addition of an aluminum-magnesium alloy containing more than 4% magnesium can also make the inclusions fine and dispersed, but it causes a certain degree of waste of Mg in the alloy. The addition of an aluminum-magnesium alloy containing less than 2% magnesium, due to the lack of Mg element participating in the reaction in the steel, Al2O3 and MgO-Al2O3 inclusions exist in the steel at the same time, and the number and size of inclusions are increased.

[0078] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A method for regulating inclusions in steel, characterized in that: The steps include: Adding aluminum-magnesium alloy to molten steel for deoxidation and alloying treatment; Wherein, the mass fraction of magnesium in the aluminum-magnesium alloy is 2% to 4%.

2. The method for controlling inclusions in steel according to claim 1, characterized in that: The addition amount of the aluminum-magnesium alloy is 0.6kg / t to 1.2kg / t.

3. The method for controlling inclusions in steel according to claim 1, characterized in that: In the aluminum-magnesium alloy, the mass fraction of aluminum is greater than 95%.

4. The method for controlling inclusions in steel according to any one of claims 1 to 3, characterized in that: The deoxidation alloying treatment step includes: adding the aluminum-magnesium alloy under a vacuum degree of 5 kPa to 7 kPa, and then performing RH cycle.

5. The method for controlling inclusions in steel according to claim 4, characterized in that: The RH cycle time is 4 to 6 minutes.

6. A method for preparing IF steel, comprising the steps of converter steelmaking, RH refining, continuous casting and rolling; characterized in that: The RH refining step comprises: after decarburizing the molten steel, adjusting the oxide inclusions in the steel by using the method for adjusting the inclusions in the steel as claimed in any one of claims 1 to 6, and then adding ferrotitanium to carry out ferrotitanium alloying treatment.

7. The method for preparing IF steel according to claim 6, characterized in that: The addition amount of the titanium-iron alloy is 0.3kg / t to 0.6kg / t.

8. The method for preparing IF steel according to claim 6, characterized in that: The titanium-iron alloying treatment step comprises: adding the titanium-iron alloy under a vacuum degree of 5 kPa to 7 kPa, and then performing RH circulation and then breaking the vacuum and exiting the station.

9. The method for preparing IF steel according to claim 8, characterized in that: The RH cycle time in the titanium-iron alloying step is 3 minutes to 5 minutes.

10. Use of the method for controlling inclusions in steel as claimed in any one of claims 1 to 6 in steelmaking.