Automobile steel smelting method capable of reducing carbon emission
By using a mixed semi-steel of electric furnace water and blast furnace water molten steel in steel smelting for converter blowing, combined with molten iron pretreatment, converter smelting and LF furnace refining processes, the carbon emissions of the smelting process have been successfully reduced and the high carbon emissions of the steel industry have been solved. The problem has achieved the production of low-carbon automotive steel.
Patent Information
- Application Number
- CN202411369061.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-03
AI Technical Summary
The high carbon emissions problem in the steel industry leads to large energy consumption and carbon emissions, especially in the automotive industry, and it is difficult to achieve low-carbon transformation, and the existing technology is difficult to effectively reduce carbon emissions in the smelting process.
The mixed semi-steel of electric furnace water and blast furnace water molten steel is used for converter blowing. Through the process flow of molten iron pretreatment, converter smelting, LF furnace refining and continuous casting, process parameters such as temperature, time and addition of auxiliary materials are controlled to reduce carbon emissions.
The thermal balance of the smelting process and the effective reduction of carbon emissions of the entire production line are achieved, the chemical composition and cleanliness requirements of low-carbon automotive steel are met, non-metallic inclusions are reduced, and the performance is in line with the ultra-low-carbon automotive steel product standards.
Smart Images

Figure CN119061315A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgical manufacturing, and in particular relates to a smelting method for automobile steel with reduced carbon emissions. Background Art
[0002] As a typical resource and energy intensive industry, the steel industry's total energy consumption accounts for about 11% of the country's total energy consumption, and its carbon emissions account for about 15% of the country's total carbon emissions. It is the "main battlefield" for energy conservation and emission reduction.
[0003] The automotive industry and the steel industry are working together to reduce carbon emissions. European automobile companies are moving upstream to build low-carbon supply chains and are particularly eager to find suppliers in China. Low-carbon emission smelting has become an external requirement for the transformation of the steel industry.
[0004] Although the domestic green steel market is just getting started, the demand for this type of steel will expand across the entire society and the entire industrial chain. The demand is on the eve of an explosion, and now is an important window to seize the advantageous position in the development of green steel.
[0005] Against this backdrop, Bengang Group has broken through the carbon emission bottleneck encountered by traditional production methods, developed new ways to increase benefits, and used low-carbon emission automotive steel as an embedding point to find a "solution" to transform towards green and low-carbon development. Summary of the invention
[0006] The present invention provides a method for smelting automobile steel with reduced carbon emissions. The method uses semi-steel mixed with electric furnace molten steel (total amount 30% to 70%) + blast furnace molten iron (total amount 70% to 30%) to perform converter blowing, which not only ensures the thermal balance of the smelting process, but also effectively reduces the carbon emissions of the entire production line production process.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for smelting automobile steel with reduced carbon emission, the method comprising: using semi-steel mixed with molten electric furnace steel accounting for 30wt% to 70wt% of the total amount and molten blast furnace iron accounting for 70wt% to 30wt% of the total amount to perform converter blowing, the converter blowing comprising molten iron pretreatment, converter smelting, LF furnace refining and continuous casting, wherein the LF furnace refining comprises: an operation time of 55 to 65 minutes, a pre-treatment temperature of 1550 to 1560°C, an argon stop temperature of 1595 to 1605°C, a station leaving temperature of 1590 to 1600°C, an end point oxygen of 500 to 540ppm, and a ladle temperature of 1550 to 1570°C.
[0009] In the LF furnace refining process: the amount of auxiliary materials and alloys added: active lime 4.5-5.5kg / t, high carbon ferromanganese 1.5-1.6kg / t, medium carbon ferromanganese 1.4-1.5kg / t, aluminum particles 0.45-0.55kg / t, aluminum wire 0.5-0.6m / t, to ensure online baking before steelmaking, adopt submerged arc operation, and prevent nitrogen increase.
[0010] The tapping temperature of the blast furnace molten iron is ≥1490°C; the chemical composition of the molten iron is calculated by weight percentage: C: 3.9% to 4.5%, Si: 0.30% to 0.60%, P≤0.09%, S≤0.04%, and the rest is Fe and unavoidable impurities. The tapping amount is 30% to 70% of the effective volume of the torpedo tank.
[0011] The electric furnace steelmaking includes electric furnace smelting and LF operation: the electric furnace smelting adopts all scrap steel smelting, and the scrap steel is well classified and managed, and the scrap steel containing special elements (Cu, Ni, Mo, Cr) is not allowed to be used; the smelting cycle is 40-60min; the amount of ingredients added: oxygen consumption 21-23Nm 3 / t, foaming agent 17-20kg / t, lime 40-42kg / t, magnesite 25-26kg / t, aluminum wire segment 1.0-1.1kg / t, ladle ash 2.0-2.1kg / t, ferrosilicon 1.0-1.1kg / t. The tapping conditions are: [O]≤600ppm, [C]0.05%-0.3%, [P]≤0.050%, residual [Ni+Cu]≤0.10%, [Cr]≤0.08%, [N]≤0.008%; the tapping temperature is 1600-1630℃.
[0012] During the whole process of LF operation, argon is blown and stirred at the bottom of the ladle. Large argon stirring and heating are not allowed. The slag color must turn white after the total power supply time is ≥20min; the amount of alloy and auxiliary materials added per ton of steel: lime 60-62kg / t, aluminum wire segment 0.8-1.0kg / t, ferrosilicon 0.8-1.0kg / t, silicon carbide 1.0-1.1kg / t. The chemical composition of the molten steel after the LF furnace is calculated by weight percentage: C: 0.9%-1.0%, Si: 0.15%-0.25%, P≤0.013%, S≤0.025%, Cr≤0.15%, Ni≤0.05%, Cu≤0.08%, and the rest are Fe and unavoidable impurities; the molten steel temperature is controlled at ≥1640℃.
[0013] After LF operation, it is folded into a torpedo tank filled with molten iron from a blast furnace. In order to reduce the temperature drop of the steel in the torpedo tank, the folding cycle of a single package is controlled to be ≤10min. After the folding is completed, carbonized rice husks are added to the torpedo tank to ensure the covering effect. The temperature of the mixed semi-steel is ≥1390℃.
[0014] The molten iron pretreatment comprises: adding 1.4-1.5 kg / t of lime and 0.23-0.24 kg / t of magnesium powder; the slag removal amount is 11-12 kg / t; the treatment time is 40-50 min, and the pretreatment blowing time is 7-9 min.
[0015] The converter smelting cycle is 20-30 minutes, the blowing duration is 8-10 minutes, the final carbon is 0.05wt%-0.06wt%, the final oxygen is 400-500ppm, the final temperature is 1625-1650℃, and the oxygen consumption per ton of steel is 32-33m 3 / t, add: active lime 23-24kg / t, dolomite 11-12kg / t, limestone 23-24kg / t, sinter 3.5-4.5kg / t. Converter re-blowing: Bottom blowing system blows argon throughout the whole process.
[0016] The continuous casting: the casting cycle is 60-70 minutes, the casting temperature is 1560-1570℃, and the pulling speed is 1.1-1.2m / min. The sealing of the long water nozzle and the argon flow control must be carried out in accordance with the current regulations. The cover of the middle ladle and the ladle body are required to be sealed, and the holes on the cover except the pouring hole are required to be covered.
[0017] The chemical composition of the automobile steel is calculated by weight percentage as follows: C 0.05%-0.30%, Si≤0.05%, Mn0.88%-1.00%, P≤0.020%, S≤0.020%, Alt 0.02%-0.06%, Ti≤0.02%, Cr+Nb+Cu≤0.20%, N≤0.0055%, and the rest is Fe and unavoidable impurities.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1) This method uses a mixture of electric furnace molten steel and blast furnace molten iron for converter blowing, which not only ensures the heat source required for converter smelting, but also effectively reduces carbon emissions generated during the blowing process.
[0020] In order to achieve the above-mentioned purpose of the invention, the present invention provides a smelting method for automotive steel with reduced carbon emissions, the specific steps of which are: (30wt%~70wt% of molten steel in electric furnace + 70wt%~30wt% of molten iron in blast furnace) → converter steelmaking → LF → continuous casting billet meets the requirements of automotive steel composition, cleanliness and other indicators.
[0021] 2) The “semi-steel” process reduces the carbon content of the charge entering the converter, effectively reducing carbon oxide emissions.
[0022] 3) The non-metallic inclusions and performance of the finished product meet the requirements of ultra-low carbon automotive steel products. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0024] The specific implementation modes of the present invention are further described below in conjunction with the embodiments.
[0025] Embodiment 1:
[0026] 1. Process route: A smelting method for automotive steel with reduced carbon emissions. The method uses a mixture of electric furnace molten steel (50% in total) and blast furnace molten iron (50% in total) for converter blowing, which not only ensures the thermal balance of the smelting process, but also effectively reduces the carbon emissions of the entire production line.
[0027] 2. Chemical composition: The chemical composition of automobile steel is calculated by weight as follows: C: 0.07%, Si: 0.04%, Mn: 0.92%, P: 0.014%, S: 0.010%, Alt: 0.03%, Ti: 0.009%, Cr+Nb+Cu: 0.165%, N: 0.0050%, and the rest is Fe and unavoidable impurities.
[0028] 3. Blast furnace molten iron + electric furnace process:
[0029] 1) Blast furnace molten iron: The chemical composition of molten iron is calculated by weight percentage: C: 4.1%, Si: 0.40%, P: 0.07%, S: 0.028%, and the rest is Fe and unavoidable impurities. The molten iron tapping temperature is 1521℃, and the tapping amount is 50% of the effective volume of the torpedo tank.
[0030] 2) Electric furnace smelting: Ingredients: Use all scrap steel for smelting, and do a good job of classification and management of scrap steel. Scrap steel containing special elements (Cu, Ni, Mo, Cr) is not allowed to be used; smelting cycle 55min; amount of oxygen added per ton of steel: 23Nm 3 / t, foaming agent 19kg / t, lime 41kg / t, magnesite 25kg / t, aluminum wire segment 1.0kg / t, ladle ash 2.0kg / t, ferrosilicon 1.0kg / t.
[0031] Steel tapping conditions: oxygen content 550ppm, [C] 0.14%, [P] 0.035%, residual [Ni+Cu] 0.078%, [Cr] 0.06%, [N] 0.005%, and steel tapping temperature is 1610℃.
[0032] 3) LF operation: The ladle bottom is blown with argon for stirring during the whole process. Large argon stirring is not allowed to heat up. The slag color must turn white after a total power supply time of 25 minutes. The amount of alloy and auxiliary materials added per ton of steel: lime 61kg / t, aluminum wire segment 0.9kg / t, ferrosilicon 0.9kg / t, silicon carbide 1.0kg / t. The chemical composition of the molten steel after the LF furnace is calculated by weight percentage: C: 0.95%, Si: 0.21%, P: 0.010%, S: 0.015%, Cr: 0.12%, Ni: 0.04%, Cu: 0.05%, and the rest is Fe and unavoidable impurities; the molten steel temperature is controlled at 1651℃.
[0033] 4) Operation of folding into torpedo tank: In order to reduce the temperature drop of steel in torpedo tank, the folding cycle of single package is controlled at 7 minutes; after the folding is completed, carbonized rice husk is added into the torpedo tank to ensure the covering effect, and the temperature of the semi-steel after mixing is 1410℃.
[0034] 4. Converter process:
[0035] 1) Hot metal pretreatment: Hot metal requires pretreatment, lime 1.4kg / t, magnesium powder 0.24kg / t, slag removal amount 11kg / t, treatment time 46min, pretreatment blowing time 8min.
[0036] 2) Converter smelting: smelting cycle 24min, blowing duration 9min, end point carbon 0.05wt%, end point oxygen 440ppm, end point temperature 1640℃, oxygen consumption per ton of steel 32m 3 / t, active lime 23Kg / t, dolomite 11Kg / t, limestone 23Kg / t, sintered ore 3.9Kg / t. Converter re-blowing: Bottom blowing system is argon-blown throughout the whole process.
[0037] 3) LF refining: operation time 58min, pre-treatment temperature 1556℃, argon stop temperature 1599℃, leaving station temperature 1595℃, final oxygen 520ppm, ladle temperature 1560℃. Amount of auxiliary materials and alloys added per ton of steel: active lime 4.9Kg / t, high carbon ferromanganese 1.5Kg / t, medium carbon ferromanganese 1.4Kg / t, aluminum particles 0.48Kg / t, aluminum wire 0.5m / t, ensure online baking before steelmaking, adopt submerged arc operation to prevent nitrogen increase.
[0038] 4) Continuous casting: Casting cycle 64min, casting temperature 1565℃, pulling speed 1.1m / min, the sealing of the long water nozzle and the control of argon gas flow must be carried out in accordance with the current regulations; the cover and the body of the tundish are required to be sealed, and all holes on the cover except the pouring holes are required to be covered.
[0039] Embodiment 2:
[0040] 1. Process route: A smelting method for automotive steel with reduced carbon emissions. This method uses a mixture of electric furnace molten steel (45% in total) and blast furnace molten iron (55% in total) to perform converter blowing, which not only ensures the thermal balance of the smelting process, but also effectively reduces the carbon emissions of the entire production line.
[0041] 2. Chemical composition: The chemical composition of automobile steel is calculated by weight as follows: C: 0.18%, Si: 0.04%, Mn: 0.92%, P: 0.015%, S: 0.012%, Alt: 0.04%, Ti: 0.015%, Cr+Nb+Cu: 0.182%, N: 0.0051%, and the rest is Fe and unavoidable impurities.
[0042] 3. Blast furnace molten iron + electric furnace process:
[0043] 1) Blast furnace molten iron: The chemical composition of molten iron is as follows by weight: C: 4.2%, Si: 0.40%, P: 0.07%, S: 0.03%, and the rest is Fe and unavoidable impurities. The temperature is 1510℃, and the amount of iron produced is 55% of the effective volume of the torpedo tank.
[0044] 2) Electric furnace smelting: Ingredients: Use all scrap steel for smelting, and do a good job of classification and management of scrap steel. Scrap steel containing special elements (Cu, Ni, Mo, Cr) is not allowed to be used; smelting cycle 56min; amount of oxygen added per ton of steel: 21Nm 3 / t, foaming agent 17kg / t, lime 42kg / t, magnesite 25kg / t, aluminum wire segment 1.0kg / t, ladle ash 2.0kg / t, ferrosilicon 1.0kg / t.
[0045] Steel tapping conditions: oxygen content 560ppm, [C] 0.15%, [P] 0.030%, residual [Ni+Cu] 0.077%, [Cr] 0.06%, [N] 0.005%, temperature: 1615°C.
[0046] 3) LF operation: The ladle bottom is blown with argon for stirring during the whole process. Large argon stirring is not allowed to heat up. The slag color must turn white after a total power supply time of 24 minutes. The amount of alloy and auxiliary materials added per ton of steel: lime 60kg / t, aluminum wire segment 0.9kg / t, ferrosilicon 0.9kg / t, silicon carbide 1.0kg / t. The chemical composition of the molten steel after the LF furnace is calculated by weight percentage: C: 0.9%, Si: 0.19%, P: 0.012%, S: 0.015%, Cr: 0.10%, Ni: 0.03%, Cu: 0.05%, and the rest is Fe and unavoidable impurities; the molten steel temperature is controlled at 1650℃.
[0047] 4) Operation of folding into torpedo tank: In order to reduce the temperature drop of steel in torpedo tank, the folding cycle of single package is controlled at 8 minutes; after the folding is completed, carbonized rice husk is added into the torpedo tank to ensure the covering effect, and the temperature of the mixed semi-steel is 1400℃.
[0048] 4. Converter process design:
[0049] 1) Hot metal pretreatment: Hot metal requires pretreatment, lime 1.4 kg / t, magnesium powder 0.23 kg / t, slag removal amount 11 kg / t, total treatment time 47 min, pretreatment blowing time 8 min.
[0050] 2) Converter smelting: smelting cycle 26min, blowing duration 9min, end point carbon 0.05wt%, end point oxygen 450ppm, end point temperature 1635℃, oxygen consumption per ton of steel 32m 3 / t, active lime 23kg / t, dolomite 11kg / t, limestone 23kg / t, sinter 3.9kg / t. Converter re-blowing: Bottom blowing system is argon-blown throughout the whole process.
[0051] 3) LF refining: operation time 62min, pre-treatment temperature 1557℃, argon stop temperature 1602℃, leaving station temperature 1597℃, final oxygen 525ppm, ladle temperature 1560℃. Amount of auxiliary materials and alloys added per ton of steel: active lime 5.2kg / t, high carbon ferromanganese 1.5kg / t, medium carbon ferromanganese 1.4kg / t, aluminum particles 0.48kg / t, aluminum wire 0.5m / t, ensure online baking before steelmaking, adopt submerged arc operation to prevent nitrogen increase.
[0052] 4) Continuous casting: Casting cycle 65min, casting temperature 1568℃, pulling speed 1.1m / min, the long water nozzle sealing and argon flow control must be carried out in accordance with the current regulations; the ladle cover and the ladle body are required to be sealed, and all holes on the ladle cover except the pouring holes are required to be covered.
[0053] Embodiment 3:
[0054] 1. Process route: A smelting method for automotive steel with reduced carbon emissions. This method uses semi-steel mixed with electric furnace molten steel (total 52%) + blast furnace molten iron (total 48%) for converter blowing, which not only ensures the thermal balance of the smelting process, but also effectively reduces the carbon emissions of the entire production line production process.
[0055] 2. Chemical composition: The chemical composition of automobile steel is calculated by weight as follows: C: 0.13%, Si: 0.04%, Mn: 0.93%, P: 0.013%, S: 0.016%, Alt: 0.04%, Ti: 0.011%, Cr+Nb+Cu: 0.175%, N: 0.0047%, and the rest is Fe and unavoidable impurities.
[0056] 3. Blast furnace molten iron + electric furnace process:
[0057] 1) Blast furnace molten iron: The chemical composition of molten iron is as follows by weight: C: 4.2%, Si: 0.48%, P: 0.07%, S: 0.03%, and the rest is Fe and unavoidable impurities. The temperature is 1496℃, and the amount of iron produced is 48% of the effective volume of the torpedo tank.
[0058] 2) Electric furnace smelting: Ingredients: Use all scrap steel for smelting, and do a good job of classification and management of scrap steel. Scrap steel containing special elements (Cu, Ni, Mo, Cr) is not allowed to be used; smelting cycle 48min; amount of oxygen added per ton of steel: 22Nm 3 / t, foaming agent 17kg / t, lime 40kg / t, magnesite 25kg / t, aluminum wire segment 1.0kg / t, ladle ash 2.0kg / t, ferrosilicon 1.0kg / t.
[0059] Steel tapping conditions: oxygen content 540 ppm, [C] 0.15%, [P] 0.035%, residual [Ni+Cu] 0.06%, [Cr] 0.06%, [N] 0.006%, temperature: 1614°C.
[0060] 3) LF operation: The ladle bottom is blown with argon for stirring during the whole process. Large argon stirring is not allowed to heat up. The slag color must turn white after a total power supply time of 26 minutes. The amount of alloy and auxiliary materials added per ton of steel: lime 60kg / t, aluminum wire segment 0.9kg / t, ferrosilicon 0.9kg / t, silicon carbide 1.0kg / t. The chemical composition of the molten steel after the LF furnace is calculated by weight percentage: C: 0.95%, Si: 0.18%, P: 0.012%, S: 0.022%, Cr: 0.12%, Ni: 0.04%, Cu: 0.06%; the rest is Fe and unavoidable impurities. The molten steel temperature is controlled at 1650℃.
[0061] 4) Operation of folding into torpedo tank: In order to reduce the temperature drop of steel in torpedo tank, the folding cycle of single package is controlled at 9 minutes; after the folding is completed, carbonized rice husk is added into the torpedo tank to ensure the covering effect, and the temperature of the semi-steel after mixing is 1410℃.
[0062] 4. Converter process:
[0063] 1) Pretreatment of molten iron: molten iron requires pretreatment, lime 1.4kg / t, magnesium powder 0.23kg / t, slag removal amount 11.5kg / t, total treatment time 42min, pretreatment blowing time 8min.
[0064] 2) Converter smelting: smelting cycle 27min, blowing duration 9min, end point carbon 0.05wt%, end point oxygen 460ppm, end point temperature 1640℃, oxygen consumption per ton of steel 32m 3 / t, active lime 23kg / t, dolomite 11kg / t, limestone 23kg / t, sintered ore 4.0kg / t. Converter re-blowing: Bottom blowing system is argon-blown throughout the whole process.
[0065] 3) LF refining: operation time 60min, pre-treatment temperature 1556℃, argon stop temperature 1600℃, leaving station temperature 1595℃, final oxygen 520ppm, ladle temperature 1560℃. Amount of auxiliary materials and alloys added per ton of steel: active lime 4.9kg / t, high carbon ferromanganese 1.5kg / t, medium carbon ferromanganese 1.4kg / t, aluminum particles 0.49kg / t, aluminum wire 0.5m / t, ensure online baking before steelmaking, adopt submerged arc operation to prevent nitrogen increase.
[0066] 4) Continuous casting: Casting cycle 65min, casting temperature 1565℃, pulling speed 1.1m / min, the sealing of the long water nozzle and the control of argon gas flow must be carried out in accordance with the current regulations; the cover and the body of the tundish are required to be sealed, and all holes on the cover except the pouring holes are required to be covered.
[0067] Mechanical properties standard requirements are shown in Table 1.
[0068] Table 1:
[0069]
[0070] The head, middle and tail of the steel plates of Examples 1-3 were sampled and tested respectively. The test results are shown in Table 2.
[0071] Table 2:
[0072] Example Rolling specification (mm) Yield strength (MPa) Tensile strength(MPa) Elongation after fracture Example 1 0.8 187 324 40.0 Example 1 0.8 201 367 35.0 Example 1 0.8 199 312 40.0 Example 2 0.8 191 327 41.0 Example 2 0.8 211 348 35.0 Example 2 0.8 203 328 35.0 Example 3 0.8 222 314 40.0 Example 3 0.8 183 294 40.0 Example 3 0.8 179 335 35.0
[0073] As can be seen from Table 2, Examples 1-3 meet the performance standard requirements, so this method is feasible.
Claims
1. A method for smelting automobile steel with reduced carbon emissions, characterized in that: The method comprises the following steps: using semi-steel mixed with electric furnace molten steel accounting for 30wt% to 70wt% of the total volume and blast furnace molten iron accounting for 70wt% to 30wt% of the total volume to be blown in a converter, wherein the converter blowing comprises molten iron pretreatment, converter smelting, LF furnace refining and continuous casting, wherein the LF furnace refining comprises: an operation time of 55 to 65 minutes, a pre-treatment temperature of 1550 to 1560°C, an argon stop temperature of 1595 to 1605°C, a station leaving temperature of 1590 to 1600°C, an end point oxygen of 500 to 540ppm and a ladle temperature of 1550 to 1570°C.
2. A method for smelting automobile steel with reduced carbon emissions according to claim 1, characterized in that: In the LF furnace refining process: the amount of auxiliary materials and alloys added: active lime 4.5-5.5kg / t, high carbon ferromanganese 1.5-1.6kg / t, medium carbon ferromanganese 1.4-1.5kg / t, aluminum particles 0.45-0.55kg / t, aluminum wire 0.5-0.6m / .
3. The method for smelting automobile steel with reduced carbon emissions according to claim 1, characterized in that: The tapping temperature of the blast furnace molten iron is ≥1490°C; the chemical composition of the molten iron is as follows by weight percentage: C: 3.9%-4.5%, Si: 0.30%-0.60%, P≤0.09%, S≤0.04%, and the rest is Fe and unavoidable impurities.
4. The method for smelting automobile steel with reduced carbon emissions according to claim 1, characterized in that: The electric furnace molten steel smelting includes electric furnace smelting and LF operation: the electric furnace smelting adopts all scrap steel smelting, and the scrap steel does not contain Cu, Ni, Mo, and Cr; the smelting cycle is 40 to 60 minutes; the steel tapping conditions are: [O] ≤ 600ppm, [C] 0.05% to 0.3%, [P] ≤ 0.050%, residual [Ni+Cu] ≤ 0.10%, [Cr] ≤ 0.08%, [N] ≤ 0.008%; the steel tapping temperature is 1600 to 1630°C; During the whole process of LF operation, argon is blown and stirred at the bottom of the ladle, and the total power supply time is ≥20min. The chemical composition of the molten steel after LF furnace is as follows by weight: C: 0.9%~1.0%, Si: 0.15%~0.25%, P≤0.013%, S≤0.025%, Cr≤0.15%, Ni≤0.05%, Cu≤0.08%, and the rest is Fe and unavoidable impurities; the molten steel temperature is controlled at ≥1640℃.
5. The method for smelting automobile steel with reduced carbon emissions according to claim 4, characterized in that: After LF operation, the folded package is put into the torpedo tank filled with molten iron from the blast furnace, and the folding cycle of a single package is controlled to be ≤10min; after the folding is completed, carbonized rice husk is added to the torpedo tank, and the temperature of the mixed semi-steel is ≥1390℃.
6. The method for smelting automobile steel with reduced carbon emissions according to claim 1, characterized in that: The molten iron pretreatment comprises: adding 1.4-1.5 kg / t of lime and 0.23-0.24 kg / t of magnesium powder; the slag removal amount is 11-12 kg / t; the treatment time is 40-50 min, and the pretreatment blowing time is 7-9 min.
7. The method for smelting automobile steel with reduced carbon emissions according to claim 1, characterized in that: The converter smelting cycle is 20-30 minutes, the blowing duration is 8-10 minutes, the end point carbon is 0.05wt%-0.06wt%, the end point oxygen is 400-500ppm, and the end point temperature is 1625-1650℃.
8. The method for smelting automobile steel with reduced carbon emissions according to claim 1, characterized in that: The continuous casting has a casting cycle of 60 to 70 minutes, a casting temperature of 1560 to 1570° C., and a pulling speed of 1.1 to 1.2 m / min.
9. The method for smelting automobile steel with reduced carbon emissions according to claim 1, characterized in that: The chemical composition of the automobile steel is calculated by weight percentage as follows: C 0.05%-0.30%, Si≤0.05%, Mn 0.88%-1.00%, P≤0.020%, S≤0.020%, Alt 0.02%-0.06%, Ti≤0.02%, Cr+Nb+Cu≤0.20%, N≤0.0055%, and the rest is Fe and unavoidable impurities.
Citation Information
Cited By
Nitrogen-controlled smelting method of steel for automobile panel
CN120967099A
Method for smelting low-carbon emission-reducing hot stamping steel with large scrap ratio
CN122428081A
A method for smelting a low-carbon, emission-reducing hot stamping steel with a large scrap ratio
CN122428081B