High-speed wheel suitable for high strength and toughness matching in low-temperature environment and heat treatment method and preparation method of high-speed wheel
By adopting specific heat treatment methods on high-speed wheels, including heating and hierarchical cooling, the wheel strength and toughness problems in low-temperature environments are solved, and the matching of high-strength and high-low-temperature impact performance is achieved, ensuring the safety of train use and reducing the safety of the train. smelting costs and energy consumption.
Patent Information
- Application Number
- CN202410998195.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing high-speed wheels have decreased strength, are prone to deformation and brittle fracture in low temperature environments, which affects the stability and service life of the train. The existing heat treatment methods have increased energy consumption and smelting costs, and have failed to effectively ensure impact performance below -40℃.
A heat treatment method is adopted, including heating to 850-870℃ and cooling to 810-830℃, heating to 810-830℃ again, and then rapid cooling is achieved by spraying hot water and cold water, and finally tempering treatment is carried out to control the grain structure. To improve ferrite content and pearlite sheet spacing, ensure high strength and high toughness of the wheels in low temperature environments.
The high strength and high-temperature impact toughness of the wheels in low-temperature environments are achieved, ensuring safe use performance, and reducing smelting costs and energy consumption, while maintaining the ferrite-pearl structure state and reducing cutting processing volume.
Smart Images

Figure CN118932162A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wheel steel, and in particular relates to a high-speed wheel with high strength and toughness matching suitable for low-temperature environments, and a heat treatment method and a preparation method thereof. Background Art
[0002] At present, the high-speed wheels in service in my country are mainly ER8 wheels in the European standard. This grade of wheels can maintain good service performance in the face of short-distance, single-line, and stable climate. However, my country has a vast territory and a large geographical span, with both high-temperature and humid areas and low-temperature and severe cold areas. The application and service environment and conditions of high-speed rail are varied. In recent years, the operation of high-speed EMUs in cold areas has gradually become popular. For example, the Harbin-Dalian passenger dedicated line opened on December 1, 2012 has a maximum operating speed of 300km / h and withstands the ambient temperature difference of -40℃ to +40℃. In the future, if high-speed trains are operated in Xinjiang, Inner Mongolia, Tibet and other regions or other countries in high-cold areas, the minimum ambient temperature may be lower than -40℃, so the reliability of low-temperature service of wheels must be faced squarely.
[0003] The impact of low temperature environment on high-speed railway is mainly manifested in the following aspects:
[0004] 1. Under low temperature, the strength of the material will drop significantly, making it more prone to deformation and brittle fracture, which will seriously affect the stability of train travel.
[0005] 2. At low temperatures, the toughness of the material will also decrease, making it more prone to cracking, which will seriously affect the service life of the wheel and driving safety.
[0006] Therefore, it is extremely necessary to design and manufacture high-speed wheels with high strength and toughness suitable for low-temperature service environments.
[0007] The Chinese patent with publication number CN 116623098 A and publication date August 22, 2023 discloses steel and production method for passenger locomotive wheels in high-cold areas, wheels and production method, with composition C: 0.44-0.54%, Si: 0.40-0.65%, Mn: 0.80-1.2%, Cr: 0.15-0.30%, V: 0.08-0.15%, Al: 0.008-0.015%, P: 0.005-0.010%, S: 0.006-0.015%; TO: ≤10ppm, [H]: ≤1.5ppm, [N]: 50-80ppm, and the rest are Fe and unavoidable impurity elements. The heat treatment method used is: first heating and heat preservation: the heating section temperature is 880-910℃, the soaking section temperature is 840-880℃, the total heating time is 2.5-3.0h, of which the soaking section time is 0.5-1.0h; then weak cooling is first, so that the surface metal of the rim tread is cooled at a rate of 0.2℃ / s-0.4℃ / s, then strong cooling, the rim cooling rate is 6-10℃ / s, and finally tempering. Although the higher quenching temperature improves the strength, it increases the heat energy consumption and causes energy waste. At the same time, the higher quenching heating temperature leads to lower impact toughness. In addition, the use of microalloying element V increases the smelting cost.
[0008] The Chinese patent with publication number CN 114107823 A and publication date March 1, 2022, discloses a high-speed wheel steel and its heat treatment method and a method for preparing a high-speed wheel using the same, with the composition of C0.52-0.56%, Si0.20-0.40%, Mn0.60-0.90%, Cr0.15-0.25, V0.06-0.15, Nb0.02-0.04%, P≤0.015%, S≤0.015%, Al0.01-0.02%, W0.3~0.6%, Mo0.03-0.05%, N60-80ppm, and the balance is Fe and unavoidable impurities. Although the impact toughness is high, the tensile strength and yield strength need to be improved. In addition, a small amount of microalloying elements V and Nb increase the toughness to a certain extent, but increase the smelting cost.
[0009] A Chinese patent with publication number CN 111270154 A and publication date June 12, 2020, discloses a medium-carbon wheel steel suitable for trucks in high-cold areas and a method for producing wheels using the same, with components of C 0.55-0.63%, Si 0.25-0.45%, Mn 0.65-0.90%, Cr≤0.30%, V≤0.10%, Nb0.02-0.04%, P≤0.030%, S≤0.025%, Ni≤0.30%, N 0.0050-0.0100%, and the balance is Fe and unavoidable impurities. The production method includes cyclic quenching and tempering processes. Although cyclic quenching improves the tensile strength and yield strength to a certain extent, it is mainly due to the precipitation strengthening effect of high carbon and vanadium carbides. The addition of V increases the smelting cost to a certain extent. Secondly, the patent does not test the impact performance at -20℃ and -40℃, and cannot ensure that the low-temperature toughness is qualified.
[0010] The Chinese patent with publication number CN 110616374 A and publication date December 27, 2019, discloses a high-carbon wheel steel and its heat treatment method and a method for preparing wheels using the same, with the composition of C0.60-0.70%, Si≤0.60%, Mn0.70-0.90%, P≤0.015%, S≤0.015%, Als≤0.035%, N 50-150ppm, and the balance is Fe and unavoidable impurities. Its heat treatment method includes the following steps: normalizing + quenching + tempering process. Although the pre-normalizing brings about a significant improvement in strength and hardness, continuous high-temperature and long-term normalizing will not only increase heat energy consumption, but may also cause coarsening of grains and thus deteriorate performance. Performance data also show that impact toughness needs to be improved. The patent did not test the -40℃ impact performance, and cannot ensure that the impact toughness of wheels in extremely cold areas with ambient temperatures close to -40℃ is still qualified. Summary of the invention
[0011] In order to solve the above technical problems, the present invention provides a high-speed wheel with high strength and toughness matching suitable for low-temperature environment and a heat treatment method and preparation method thereof. The high-speed wheel has both high strength and high hardness and high and low-temperature impact toughness, thereby ensuring that the high-speed wheel has good safety performance in low-temperature service conditions.
[0012] The technical solution adopted by the present invention is as follows:
[0013] A heat treatment method for high-speed wheels with high strength and toughness matching under low temperature environment, the heat treatment method comprising the following steps:
[0014] S1: The rolled wheel is heated to 850-870℃, then slowly cooled to 810-830℃ and kept warm, and then cooled naturally in the air; the heating at 850-870℃ is to ensure that the austenite is fully transformed, and the low-temperature soaking at 810-830℃ can avoid the growth and coarsening of grains under long-term high temperature, which may cause the deterioration of wheel performance;
[0015] S2: The wheel obtained in step S1 is heated again to 810-830°C and kept warm; too high a temperature will lead to a decrease in ferrite content and a larger grain size, thereby causing a decrease in toughness, while too low a temperature will lead to insufficient strength and increased difficulty in on-site stability control;
[0016] S3: taking out the wheel obtained in step S2 and transferring it to a quenching station, first spraying the wheel tread with hot water to cool the 5 mm below the wheel tread to below 500° C. at a cooling rate of ≤4° C. / s, and then spraying the wheel tread with cold water to quickly cool the metal inside the rim to below 500° C. at a cooling rate of 3-6° C. / s, so that the pearlite structure transformation is completed;
[0017] S4: The wheel obtained in step S3 is tempered at 500-520° C. for 4.0-4.5 hours. Too high a tempering temperature may easily cause pearlite to deform and break, thereby deteriorating the strength performance of the wheel.
[0018] In step S1, the total wheel heating time is 2.0 to 3.0 hours, and the heat preservation time at 810 to 830° C. is 1.0 to 1.5 hours.
[0019] In step S2, the total wheel heating time is 2.0 to 3.0 hours, and the heat preservation time at 810 to 830° C. is 1.0 to 1.5 hours.
[0020] In step S2, after the second stage of quenching, the surface temperature of the wheel tread is lower than 150°C.
[0021] In step S3, the temperature of the hot water is 55-60°C, and the spraying time is 60-80s; the temperature of the cold water is 5-10°C, and the spraying time is 190-210s.
[0022] In step S3, the wheel rotates along with the quenching table roller, and the roller speed is 40 to 60 revolutions per minute.
[0023] The present invention also provides a high-speed wheel with high strength and toughness matching suitable for use in a low-temperature environment, which is obtained by heat treatment using the heat treatment method of the present invention.
[0024] The steel composition and weight percentage of the high-speed wheel are: C 0.50-0.56%, Si 0.30-1.10%, Mn 0.70-0.80%, Cr 0.20-0.30%, Al≤0.020%, P≤0.015%, S≤0.015%, Ti≤0.002%, and the rest are Fe and unavoidable impurity elements.
[0025] The metallographic structure of the high-speed wheel is ferrite and pearlite; the grain size in the microstructure of the area from the wheel tread surface to 35 mm below the tread is greater than or equal to grade 8.0, the ferrite volume fraction is 8.5% to 10.5%, and the pearlite plate spacing is 115 to 127 nm.
[0026] The rim Rm of the high-speed wheel is 1100-1120 MPa, R P0.2 720~735MPa, A19.0~21%; Hardness of wheel rim 5mm from tread ≥310HB, hardness 35mm from tread ≥280HB; K Q Single value ≥90MPa.m 1 / 2 , average value ≥94MPa.m 1 / 2 ; -20℃ KV single value ≥19J, average ≥21.0J; -40℃ KV single value ≥12J, average ≥13.5J; -60℃ KU single value ≥90MPa·m 1 / 2 , average value ≥ 100MPa·m 1 / 2 .
[0027] The present invention also provides a method for preparing the high-speed wheel with high strength and toughness matching suitable for low-temperature environment, and the preparation method comprises the following steps: electric furnace smelting → LF furnace refining → vacuum degassing → round billet continuous casting → slow cooling treatment → ingot cutting → heating before rolling → forging and rolling → slow cooling → heat treatment → processing → finished product inspection.
[0028] In the heat treatment method for high-speed wheels with high strength and toughness matching under low temperature environment provided by the present invention, a pretreatment is added before quenching, which is essentially complete austenitization plus eutectoid transformation. The phenomenon that the internal grains of the rolled wheel rim are coarse, the edge grains are fine, and the size distribution is extremely uneven is improved through a recrystallization. The heating at 840℃~860℃ is to ensure that the complete austenite transformation zone is reached to avoid insufficient transformation caused by the difference between the furnace temperature and the steel temperature and the furnace temperature and the instrument temperature during heating. Then, the furnace is slowly cooled to 810~830℃ for uniform heat preservation, so that small and uniformly distributed austenite grains can be obtained, which is convenient for obtaining a relatively large inter-sheet spacing during subsequent quenching and cooling. Fine pearlite lays a good organizational foundation. It should be noted that the absorptive temperature cannot be lower than 800℃, which is close to Ac3, which is not conducive to component homogenization and stability of on-site production control; the ferrite content is increased by appropriately reducing the quenching heating temperature, thereby achieving high plasticity and toughness; different water temperatures are used for graded quenching, and the tread surface in the high temperature zone is slowly cooled by hot water spray quenching, which inhibits or eliminates the bainite structure near the surface of the wheel tread, and the tread surface in the medium and low temperature zone is quickly cooled by cold water spray quenching. The faster the cooling rate, the greater the supercooling, which can provide more energy to increase the interface formed by ferrite and cementite. The finer the pearlite sheet spacing, the higher the strength.
[0029] In the high-speed wheel with high strength and toughness matching suitable for low-temperature environment provided by the present invention, the functions and controls of various components are as follows:
[0030] C: C is an austenite-forming element, which can be dissolved in the matrix or exist in the form of carbides. It plays a major role in the strength and hardness of the material and is the most important component of wheel steel. On the one hand, we hope to increase the C content as much as possible within the possible range to reduce the wear of the wheel tread and extend the service life of the wheel; but on the other hand, the increase in C content will cause the toughness and thermal fatigue resistance of the wheel steel to drop sharply, and the network cementite is a structure that the wheel steel absolutely avoids forming. Therefore, the C content control range of the high-speed wheel needs to be between 0.4-0.7. A comprehensive evaluation of the influence of C content on the overall performance of wheel steel within this composition range shows that the C content between 0.50-0.56% can obtain the best performance match. The present invention designs the C content to be 0.50-0.56%.
[0031] Si: Judging from the relationship between chemical composition and Ac1 and Ac3 points, increasing the Si content helps to prevent austenite transformation and martensite transformation from occurring when the wheel is heated and cooled, thereby improving the wheel material's resistance to thermal damage. However, too high Si content will increase the material's thermal sensitivity and brittleness. Reducing the Si content can improve the steel's toughness, because Si can promote the formation of Laves phase in steel. As long as the Si content in the wheel steel does not exceed 1%, the steel's impact toughness will not be significantly lost.
[0032] Mn: The main purpose of adding Mn to wheel steel is to improve the strength and hardness of the wheel and improve the wear resistance of the wheel. Studies have shown that when the Mn content is higher than 1%, the impact toughness and processing performance of the wheel will deteriorate, so the Mn content is controlled at 0.70% to 0.80%.
[0033] Cr: Cr is a secondary contributing element to the solid solution strengthening of wheel steel. Adding Cr makes the pearlite structure more stable, slows down the rate of transformation of the original structure to austenite to a certain extent, and fundamentally reduces the possibility of martensitic phase transformation in the subsequent cooling process, thereby improving the anti-stripping performance of the wheel. The present invention designs the Cr content to be 0.20-0.30%.
[0034] Al element: Al, as a deoxidizer in steel, can combine with N to form AlN, which can not only reduce the free nitrogen content in the steel, but also refine the austenite grains to a certain extent and improve the toughness. However, if the Al content is too high, it is easy to form alumina inclusions. Therefore, the Al content of the steel of the present invention is controlled within 0.020%.
[0035] Ti: Ti is a strong carbide-forming element, which can easily affect the precipitation of M(CN) in wheel steel. Ti will also compete with Al in steel for N to generate TiN, which weakens the fine grain strengthening effect of AlN and affects the final performance of the steel. Therefore, the Ti content of the steel of the present invention is controlled within 0.002%.
[0036] P, S: P and S are impurity elements, so the content of P and S in the steel of the present invention is controlled within 0.015%.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The wheel prepared by the present invention innovatively proposes a new product manufacturing scheme based on the ER8 wheel material. On the basis of not increasing the C content, by adjusting the content of Si and Cr elements, pre-quenching pretreatment and graded quenching at different water temperatures, the wheel obtains good strength and toughness matching performance, especially excellent low-temperature impact toughness of -40°C, wherein: rim Rm1100~1120MPa, R P0.2 720~735MPa, A19.0~21%; Hardness of wheel rim 5mm from tread ≥310HB, hardness 35mm from tread ≥280HB; K Q Single value ≥90MPa.m 1 / 2 , average value ≥94MPa.m 1 / 2 ; -20℃ KV single value ≥19J, average ≥21.0J; -40℃ KV single value ≥12J, average ≥13.5J; -60℃ KU ≥90MPa·m 1 / 2 , average value ≥ 100MPa·m 1 / 2, ensuring that the wheel has good safety performance under low temperature service conditions. In addition, the wheel made by the present invention can maintain the ferrite-pearlite structure of the original wheel, while reducing or eliminating the non-pearlite structure near the surface of the wheel tread, reducing the amount of cutting processing, and not increasing the difficulty of wheel preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is the original austenite grain of the wheel in Example 1.
[0040] Figure 2 This is the original austenite grain of the wheel in comparative example 1.
[0041] Figure 3 This is the original austenite grain of the wheel in comparative example 3. Figure 4 This is the metallographic structure of the wheel in Example 1.
[0042] Figure 5 This is the metallographic structure of the wheel of comparative example 1.
[0043] Figure 6 This is the metallographic structure of the wheel in comparative example 3.
[0044] Figure 7 This is the pearlite lamellar spacing of the wheel in Example 1.
[0045] Figure 8 This is the pearlite lamellar spacing of the wheel in comparative example 1.
[0046] Fig. 9 This is the pearlite lamellar spacing of the wheel in comparative example 3.
[0047] Fig.10 This is the original austenite grain of the wheel in Example 2.
[0048] Fig.11 This is the original austenite grain of the wheel in comparative example 2.
[0049] Fig.12 This is the original austenite grain of the wheel in comparative example 4.
[0050] Fig.13 This is the metallographic structure of the wheel in Example 2.
[0051] Fig.14 This is the metallographic structure of the wheel in comparative example 2.
[0052] Fig.15 This is the metallographic structure of the wheel in comparative example 4.
[0053] Fig.16 This is the pearlite lamellar spacing of the wheel in Example 2.
[0054] Fig.17 This is the pearlite lamellar spacing of the wheel in comparative example 2.
[0055] Fig.18 This is the pearlite lamellar spacing of the wheel in comparative example 4. DETAILED DESCRIPTION
[0056] The present invention is described in detail below with reference to the embodiments.
[0057] Example 1
[0058] A high-speed wheel with high strength and toughness matching suitable for low-temperature environments, the chemical composition of which is shown in Table 1.
[0059] The preparation process of the high-speed wheel is: electric furnace smelting → LF furnace refining → RH or VD vacuum degassing → round billet continuous casting → slow cooling treatment → ingot cutting → heating before rolling → forging and rolling → stacking slow cooling → heat treatment → processing → finished product testing.
[0060] Among them, the heat treatment process includes: overall pretreatment → overall pre-quenching heating → graded spray quenching at different water temperatures → overall tempering. The specific operation steps are as follows:
[0061] S1: The blank wheel with an outer diameter of 915 mm is obtained by rolling. The blank wheel is placed in a ring heating furnace, heated to 850°C, and then slowly cooled to 810°C with the furnace and kept warm for 1.5 hours. It is then taken out by a robot and naturally cooled to room temperature in the air.
[0062] S2: The wheel obtained in step S1 is placed in the annular heating furnace again, the temperature is raised to 810°C and kept at this temperature for 1.5 hours.
[0063] S3: The wheel obtained in step S2 is taken out from the annular heating furnace and transferred to a quenching table, and the tread is continuously spray-quenched by different water temperatures in stages. The water temperature in the first stage is 60°C, and the spray-quenching time is 60s, so as to ensure that the temperature of the 5mm below the wheel tread is reduced to below 500°C at a cooling rate of ≤4°C / s while the temperature of the center of the rim remains in the austenite zone. The water temperature in the second stage is 10°C, and the spray-quenching time is 200s. During the spray-quenching process, the wheel rotates with the roller at a speed of 50 rpm, so as to ensure that the surface temperature of the wheel tread is lower than 150°C after the spray-quenching is completed, and the metal inside the rim is rapidly cooled to below 500°C at a cooling rate of 3-6°C / s, so as to ensure that the pearlite structure transformation is completed in the entire wear-limited area;
[0064] S4: The wheel obtained in step S3 is transferred from the chain plate bed to the annular tempering furnace, and is placed in the tempering furnace. The tempering temperature is set to 520° C. and the tempering time is set to 4.0 h.
[0065] Example 1: Based on the composition of the traditional ER8 wheel, the content of Cr element is increased to 0.29%, which slows down the rate of transformation of the original structure to austenitization and increases the degree of supercooling in the cooling phase transformation stage, thereby obtaining a relatively fine pearlite sheet spacing. At the same time, the Ti and Al contents are strictly controlled to promote the effective combination of Al and N to form the AlN second phase, pin the grain boundaries, and effectively hinder the growth and coarsening of austenite grains, thereby achieving high strength while also having good toughness. In addition, in the heat treatment process, by adding a pretreatment, the coarseness and uneven distribution of the original grains are significantly improved. By means of graded quenching and cooling, the generation of abnormal tissue near the surface of the wheel tread is reduced, and the pearlite structure is refined, thereby achieving a simultaneous improvement in strength and toughness.
[0066] Example 2
[0067] A high-speed wheel with high strength and toughness matching suitable for low-temperature environments, the chemical composition of which is shown in Table 1.
[0068] The preparation process of the high-speed wheel is: electric furnace smelting → LF furnace refining → RH or VD vacuum degassing → round billet continuous casting → slow cooling treatment → ingot cutting → heating before rolling → forging and rolling → stacking slow cooling → heat treatment → processing → finished product testing.
[0069] Among them, the heat treatment process includes: overall pretreatment → overall pre-quenching heating → graded spray quenching at different water temperatures → overall tempering. The specific operation steps are as follows:
[0070] S1: The blank wheel with an outer diameter of 915 mm is obtained by rolling. The blank wheel is loaded into a ring heating furnace, heated to 870°C, and then slowly cooled to 830°C with the furnace and kept warm for 1.0 h. It is then taken out by a robot and naturally cooled to room temperature in the air.
[0071] S2: The wheel obtained in step S1 is placed in the annular heating furnace again, the temperature is raised to 830°C and kept at this temperature for 1.0h.
[0072] S3: The wheel obtained in step S2 is taken out from the annular heating furnace and transferred to a quenching table, and the tread is continuously spray-quenched by different water temperatures in stages. The water temperature in the first stage is 60°C, and the spray-quenching time is 55s, so as to ensure that the lower 5mm of the wheel tread is cooled to below 500°C at a cooling rate of ≤4°C / s while the temperature of the center of the rim remains in the austenite zone. The water temperature in the second stage is 5°C, and the spray-quenching time is 190s. During the spray-quenching process, the wheel rotates with the roller at a speed of 50 rpm, so as to ensure that the surface temperature of the wheel tread is lower than 150°C after the spray-quenching is completed, and the metal inside the rim is rapidly cooled to below 500°C at a cooling rate of 3-6°C / s, so as to ensure that the pearlite structure transformation is completed in the entire wear-limited area;
[0073] S4: The wheel obtained in step S3 is transferred from the chain plate bed to the annular tempering furnace, and is put into the tempering furnace. The tempering temperature is set to 500° C. and the tempering time is set to 4.5 hours.
[0074] Example 2 Based on the composition of the traditional ER8 wheel, the content of Si element is increased from 0.35% to 0.95%, which increases the solid solution strengthening effect of ferrite and the difficulty of rearrangement of alloy elements during phase transformation, and refines the pearlite interlamellar spacing, thereby achieving an improvement in the overall strength of the steel. In addition, in the heat treatment process, by adding a pretreatment, the coarseness and uneven distribution of the original grains are significantly improved, and by means of graded quenching and cooling, the generation of abnormal organization near the surface of the wheel tread is reduced, and the pearlite organization is refined, thereby achieving a simultaneous improvement in strength and toughness.
[0075] Comparative Example 1
[0076] A high-speed wheel, whose chemical composition is the same as that of embodiment 1.
[0077] The preparation process of the high-speed wheel is the same as that of Example 1, and the heat treatment process includes: heating before overall quenching → graded spray quenching with different water temperatures → overall tempering. No pretreatment is performed before heating before overall quenching, which is specifically as follows:
[0078] S1: The blank wheel with an outer diameter of 915 mm is obtained by rolling, and the blank wheel is placed in a ring heating furnace, heated to 810°C and kept warm for 1.5 hours.
[0079] S2: The wheel obtained in step S1 is taken out from the annular heating furnace and transferred to a quenching table by a robot. The tread is cooled by continuous spray quenching at different water temperatures in stages. The control measures are the same as those in Example 1.
[0080] S3: After the quenching is completed, tempering treatment is performed, and the tempering system is the same as in Example 1.
[0081] Comparative Example 2
[0082] A high-speed wheel, whose chemical composition is the same as that of embodiment 2.
[0083] The preparation process of the high-speed wheel is the same as that of Example 2. The heat treatment process includes: overall pretreatment → overall pre-quenching heating → graded spray quenching at different water temperatures → overall tempering. The difference from Example 2 is that in step S1, after heating to 870°C, no cooling treatment is performed, and the temperature is kept for 1.0h, and then quenching and tempering are performed, as follows:
[0084] S1: The blank wheel with an outer diameter of 915 mm is obtained by rolling. The blank wheel is placed in a ring heating furnace, heated to 870°C and kept warm for 1 hour, and then taken out by a robot and naturally cooled to room temperature in the air.
[0085] S2: The wheel obtained in step S1 is placed in the annular heating furnace again, the temperature is raised to 830°C and kept at this temperature for 1.0h.
[0086] S3: The wheel obtained in step S2 is taken out from the annular heating furnace and transferred to a quenching table, and the tread is cooled by continuous spray quenching in stages with different water temperatures, and the control measures are the same as those in Example 2;
[0087] S4: After the quenching is completed, a tempering treatment is performed, and the tempering system is the same as that in Example 2.
[0088] Comparative Example 3
[0089] A high-speed wheel, the chemical composition of which is shown in Table 1.
[0090] The preparation process of the high-speed wheel is: electric furnace smelting → LF furnace refining → RH or VD vacuum degassing → round billet continuous casting → slow cooling treatment → ingot cutting → heating before rolling → forging and rolling → stacking slow cooling → heat treatment → processing → finished product testing.
[0091] The heat treatment process is the same as that in Example 1, except that different water temperature graded cooling is not performed in the cooling stage, and specifically includes: overall pretreatment → overall pre-quenching heating → continuous spray quenching at the same water temperature → overall tempering, specifically as follows:
[0092] S1: The blank wheel with an outer diameter of 915 mm is obtained by rolling. The blank wheel is placed in a ring heating furnace, heated to 850°C, and then slowly cooled to 810°C with the furnace and kept warm for 1.5 hours. It is then taken out by a robot and naturally cooled to room temperature in the air.
[0093] S2: The wheel obtained in step S1 is placed in the annular heating furnace again, the temperature is raised to 810°C and kept at this temperature for 1.5 hours.
[0094] S3: taking the wheel obtained in step S2 out of the annular heating furnace and transferring it to a quenching table, and using continuous water spray cooling to rapidly cool the metal inside the rim to below 500° C. at a cooling rate of 3-5° C. / s;
[0095] S4: After the quenching is completed, a tempering treatment is performed, and the tempering system is the same as that in Example 1.
[0096] Comparative Example 4
[0097] A high-speed wheel, the chemical composition of which is shown in Table 1.
[0098] The preparation process of the high-speed wheel is: electric furnace smelting → LF furnace refining → RH or VD vacuum degassing → round billet continuous casting → slow cooling treatment → ingot cutting → heating before rolling → forging and rolling → stacking slow cooling → heat treatment → processing → finished product testing.
[0099] The heat treatment process includes: overall pretreatment → overall pre-quenching heating → graded spray quenching at different water temperatures → overall tempering, as follows:
[0100] S1: The blank wheel with an outer diameter of 915 mm is obtained by rolling, and the blank wheel is placed in a ring heating furnace, heated to 870°C and kept warm for 1.0 h;
[0101] S2: The wheel obtained in step S1 is placed in the annular heating furnace again, the temperature is raised to 870°C and kept at this temperature for 1.5 hours;
[0102] S3: The wheel obtained in step S2 is taken out from the annular heating furnace and transferred to a quenching table, and the tread is cooled by continuous spray quenching in stages with different water temperatures, and the control measures are the same as those in Example 2;
[0103] S4: After the quenching is completed, a tempering treatment is performed, and the tempering system is the same as that in Example 2.
[0104] Table 1 Main chemical components of wheels of the embodiment and comparative example (wt%)
[0105]
[0106] The original austenite grain morphology of the wheels in Example 1 and Comparative Examples 1 and 3 is as follows: Figure 1 , 2 , 3. It can be seen that compared with the wheel of comparative example 1, the grains of the wheel of embodiment 1 are obviously finer and more evenly distributed. These fine and even grain structures are the key to obtaining a good match between strength and toughness.
[0107] The metallographic structures at 5 mm below the wheel tread of Example 1 and Comparative Examples 1 and 3 are as follows Figure 4 , 5 As shown in Figure 6, it is mainly fine pearlite + a small amount of ferrite. The ferrite volume fraction of the wheel in Example 1 is about 10.7%, the ferrite volume fraction of the wheel in Comparative Example 1 is about 8.8%, and the ferrite volume fraction of the wheel in Comparative Example 3 is about 8.4%. The difference between the two is not big. Comparative Example 3 has obvious feathery bainite structure, and the abnormal structure accounts for nearly 10%.
[0108] The pearlite lamellar spacing of the wheels of Example 1 and Comparative Examples 1 and 3 is as follows: Figure 7 , 8 As shown in Figures 9 and 10, the pearlite lamellae spacing of the wheel of Example 1 is 116-130nm, and the fine pearlite lamellae spacing is the main reason for its high strength and toughness. The pearlite lamellae spacing of the wheel of Comparative Example 1 is 137-142nm, and the pearlite lamellae spacing of the wheel of Comparative Example 3 is 122-221nm, which is obviously coarsened compared with Example 1. In addition, Comparative Example 3 has obvious structural unevenness due to the use of traditional continuous quenching cooling.
[0109] The original austenite grain morphology of the wheels of Example 2 and Comparative Examples 2 and 4 is as follows: Fig.10 , 11, 12. It can be seen that compared with the wheels of Example 2, the wheels of Comparative Examples 2 and 4 have significantly coarsened and grown grains due to long-term high-temperature heating and heat preservation.
[0110] The microstructures of the wheels of Example 2 and Comparative Examples 2 and 4 are as follows: Fig.13 , 14 , 15. It can be seen that the microstructures are all fine pearlite + a small amount of ferrite. The ferrite volume fraction of the wheel in Example 2 is about 8.5%, the ferrite volume fraction of the wheel in Comparative Example 2 is about 7.4%, and the ferrite volume fraction of the wheel in Comparative Example 4 is about 5.9%. The difference is obvious. More ferrite is the key to obtaining high toughness. In addition, the size of a single ferrite block in Example 2 is significantly larger than that in Comparative Example 4. The main way of increase is the extension along the long axis of the ferrite. The extension of ferrite reduces the area of direct contact between pearlite pellets, which can also improve toughness.
[0111] The pearlite lamellar spacing of the wheels in Example 2 and Comparative Example 2 is as follows: Fig.16 , 17 As shown in Figures 18, the pearlite lamellae spacing of the wheel of Example 2 is 115-124nm, the pearlite lamellae spacing of the wheel of Comparative Example 2 is 135-139nm, and the pearlite lamellae spacing of the wheel of Comparative Example 4 is 135-139nm, which are quite different. The finer pearlite lamellae spacing is the main reason for Example 2 to obtain high strength and toughness.
[0112] The wheels of Example 1 and Comparative Examples 1 and 3, and Example 2 and Comparative Examples 2 and 4 were subjected to room temperature tensile, series temperature pendulum impact, hardness and fracture toughness tests. Specifically, according to BS EN 13262 "Railway Applications - Wheelsets and Bogies - Wheels - Product Requirements", tensile test specimens, Charpy impact specimens, rim section hardness specimens and fracture toughness compact tensile specimens (6 pieces evenly distributed along the circumference) were taken from the corresponding positions of the rim and the spoke of the finished wheel, and room temperature tensile tests and series temperature pendulum impact tests were carried out in accordance with GB / T 228.1 "Metallic Materials Tensile Test Part 1: Room Temperature Test Method" and GB / T 229 "Metallic Materials Charpy Pendulum Impact Test Method", and the performance results are shown in Table 2-3; hardness tests and fracture toughness tests were carried out in accordance with GB / T 231.1 "Metallic Materials Brinell Hardness Test Part 1: Test Method" and GB / T 4161-2007 "Metallic Materials Plane Strain Fracture Toughness KIC Test Method", and the relevant results are shown in Table 2-4. It can be seen that compared with the traditional ER8 wheel, the solution of the present invention can achieve higher rim cross-section hardness while also having higher impact toughness and fracture toughness, and has good comprehensive performance.
[0113] Table 2 Tensile mechanical properties of wheels of the embodiment and the comparative example
[0114]
[0115] Table 3 Series temperature shock performance of wheel rims of the embodiment and the comparative example
[0116]
[0117]
[0118] Table 4 Hardness and fracture toughness of wheel rim section of the embodiment and comparative example
[0119]
[0120] It can be seen from the above data that the tensile properties, impact toughness, fracture toughness and cross-section hardness of the steel in Examples 1-2 controlled according to the present invention are all good. Compared with Example 1, Comparative Example 1 was not pretreated before quenching and heating, resulting in a coarse grain size and poor distribution uniformity, and a large pearlite interlamellar distance, thereby deteriorating the strength and impact toughness of the wheel; Comparative Example 3 has more bainite abnormal structures, which not only has an adverse effect on strength and toughness, but also requires more processing allowances to be reserved, and has poor economic efficiency. Compared with Example 2, the Si and Cr contents of Comparative Example 4 are relatively low, resulting in poor solid solution strengthening effect of the steel, and Comparative Examples 2 and 4 are in a high temperature environment for a long time, resulting in grain growth. At the same time, the quenching temperature of Comparative Example 4 is relatively high, which is not conducive to obtaining more proeutectoid ferrite, so the comprehensive performance is also poor.
[0121] The above-mentioned reference embodiments provide a detailed description of a high-speed wheel suitable for high-strength and toughness matching in a low-temperature environment, and a heat treatment method and a preparation method thereof. This is illustrative rather than restrictive, and several embodiments may be listed within the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A heat treatment method for high-speed wheels with high strength and toughness matching under low temperature environment, characterized in that: The heat treatment method comprises the following steps: S1: The rolled wheel is heated to 850-870°C, then slowly cooled to 810-830°C in the furnace and kept warm, and then cooled naturally in the air; S2: heating the wheel obtained in step S1 again to 810-830° C. and keeping the temperature constant; S3: taking out the wheel obtained in step S2 and transferring it to a quenching station, first spraying the wheel tread with hot water to cool the 5 mm below the wheel tread to below 500° C. at a cooling rate of ≤4° C. / s, and then spraying the wheel tread with cold water to quickly cool the metal inside the rim to below 500° C. at a cooling rate of 3-6° C. / s; S4: The wheel obtained in step S3 is tempered at 500-520° C. for 4.0-4.5 hours.
2. The heat treatment method according to claim 1, characterized in that In step S1, the total wheel heating time is 2.0 to 3.0 hours, and the heat preservation time at 810 to 830° C. is 1.0 to 1.5 hours.
3. The heat treatment method according to claim 1, characterized in that In step S2, the total wheel heating time is 2.0 to 3.0 hours, and the heat preservation time at 810 to 830° C. is 1.0 to 1.5 hours.
4. The heat treatment method according to claim 1, characterized in that: In step S3, the temperature of the hot water is 55-60°C, and the spraying time is 60-80s; the temperature of the cold water is 5-10°C, and the spraying time is 190-210s.
5. The heat treatment method according to claim 1, characterized in that: In step S3, the wheel rotates along with the quenching table roller, and the roller speed is 40 to 60 revolutions per minute.
6. A high-speed wheel suitable for high strength and toughness matching in low temperature environment, characterized in that: The high-speed wheel is obtained by heat treatment using the heat treatment method described in any one of claims 1 to 5.
7. The high-speed wheel with high strength and toughness suitable for low-temperature environment according to claim 6, characterized in that: The steel composition and weight percentage of the high-speed wheel are: C 0.50-0.56%, Si 0.30-1.10%, Mn 0.70-0.80%, Cr 0.20-0.30%, Al≤0.020%, P≤0.015%, S≤0.015%, Ti≤0.002%, the rest is Fe and inevitable impurity elements.
8. The high-speed wheel with high strength and toughness matching suitable for low-temperature environment according to claim 6, characterized in that: The metallographic structure of the high-speed wheel is ferrite and pearlite; the grain size in the microstructure of the area from the wheel tread surface to 35 mm below the tread is greater than or equal to grade 8.0, the ferrite volume fraction is 8.5% to 10.5%, and the pearlite plate spacing is 115 to 127 nm.
9. The high-speed wheel with high strength and toughness suitable for low-temperature environment according to claim 6, characterized in that: The rim Rm of the high-speed wheel is 1100-1120 MPa, R P0.2 720~735MPa, A19.0~21%; Hardness of wheel rim 5mm from tread ≥310HB, hardness 35mm from tread ≥280HB; K Q Single value ≥90MPa.m 1 / 2 , average value ≥94MPa.m 1 / 2 ; -20℃ KV single value ≥19J, average ≥21.0J; -40℃ KV single value ≥12J, average ≥13.5J; -60℃ KU single value ≥90MPa·m 1 / 2 , average value ≥ 100MPa·m 1 / 2 .
10. The method for preparing a high-speed wheel with high strength and toughness matching suitable for low-temperature environment as claimed in claim 6, characterized in that: The preparation method comprises the following steps: electric furnace smelting→LF furnace refining→vacuum degassing→round billet continuous casting→slow cooling treatment→ingot cutting and unloading→pre-rolling heating→forging and rolling→stove slow cooling→heat treatment→processing→finished product testing.
Citation Information
Patent Citations
Thermal treatment method for high-carbon steel train wheel circular rim surface and heat treatment apparatus
CN101270408A
Heat-treatment cooling process for train wheel
CN110055394A
Medium-carbon wheel steel suitable for freight trains in alpine regions and method for producing wheels by using medium-carbon wheel steel
CN111270154A
Medium-carbon wheel steel with good matching of wear resistance and obdurability, heat treatment method of medium-carbon wheel steel and preparation method of wheel
CN111500925A
High-strength and high-toughness heavy-load wheel steel suitable for alpine region and heat treatment method for wheels produced by steel
CN113337782A