Ore blending structure and smelting method of whole-process vanadium-titanium sinter
By optimizing the ore blending structure and sintering process of vanadium-titanium sinter throughout the entire process, the problems of high ore blending cost and declining quality of sinter have been solved, achieving stability and cost reduction in blast furnace smelting, increasing the vanadium content in molten iron, and resulting in high economic benefits.
Patent Information
- Application Number
- CN202411010063.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Existing sinter blending methods are costly, making blast furnace smelting difficult. Furthermore, the use of cost-effective materials to reduce costs leads to a decline in sinter quality.
The ore blending structure of vanadium-titanium sinter is adopted through the whole process. By adjusting the raw material ratio, high-content foreign ore powder, iron concentrate, high vanadium-titanium iron powder and boron-magnesium iron powder are used, along with a certain amount of steel slag and aluminum powder. The amount of low-grade ore powder added is increased, the sintering process parameters are optimized, and a coke-coated ore structure is formed, which promotes the uniformity of mixing and the reduction reaction.
This has achieved stable sinter quality, reduced ironmaking costs, increased vanadium content in molten iron, reduced the amount of vanadium-titanium alloy used, lowered overall process costs, and enhanced the company's market competitiveness.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of smelting, and in particular to an ore blending structure and a smelting method for a full-process vanadium-titanium sintered ore. Background Art
[0002] In the field of iron and steel metallurgy, iron ore powder, coke, flux, etc. are mixed with water, mixed and granulated by a drum mixer to obtain small balls of mixed material with a certain particle size distribution, and then sintered by exhaust on a trolley to finally obtain the sintered ore required for blast furnace ironmaking. Sintered ore is an important component of blast furnace charge, and its quality directly affects the production efficiency and cost of the blast furnace. Sintered ore usually accounts for more than 80% of the charge, so its quality plays a decisive role in the production and smooth operation of the blast furnace.
[0003] In recent years, due to the rapid expansion of the steel industry, serious overcapacity, fierce competition in the industry, and the influence of resources and market factors, the prices of raw materials and fuels have risen sharply. At the same time, with the fluctuation of steel market prices, the production costs of steel companies have been under great pressure. The steel industry is facing an extremely severe production and operation situation, and some steel companies are even in a loss-making state. In order to turn losses into profits, most companies adopt the method of reducing the cost of iron materials at the sintering end and transition from fine materials to economic materials. However, the use of cost-effective economic materials will inevitably lead to the increase of harmful elements (such as titanium, potassium, sodium, zinc, etc.) in iron ore, reduce the quality of sintered ore, and bring difficulties to blast furnace smelting. Therefore, providing a sintered ore blending method with stable sintered ore quality and reduced production costs is of great significance to guiding sintering production to reduce costs and increase efficiency. Summary of the invention
[0004] In view of the high cost of the ore blending method of sintered ore in the prior art, and the fact that the quality of sintered ore will be reduced in order to reduce the cost, which brings difficulties to blast furnace smelting, the present invention provides a full-process vanadium-titanium sintered ore blending structure and smelting method. The sintered ore obtained by sintering with the ore blending structure provided by the present invention has stable quality, and under this charge structure, the blast furnace can be operated stably for a long time, the ironmaking cost is reduced, and it has good economic benefits and high practical value.
[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0006] In a first aspect, the present invention provides a full-process vanadium-titanium sintered ore blending structure, wherein the raw materials of the vanadium-titanium sintered ore include sintered iron material, flux and fuel.
[0007] Taking the raw material of the vanadium-titanium sintered ore as 100%, the sintered iron material includes the following raw material components in percentage by mass: 4% to 7% iron concentrate, 7% to 11% high vanadium-titanium iron powder, 29% to 40% external ore powder, 1% to 2.5% steel slag, 0% to 2% iron sheet, 2% to 3% aluminum powder, 1% to 3% boron-magnesium-iron powder and 0% to 2% depreciation powder;
[0008] The iron concentrate includes ordinary iron powder and 69 iron powder; the mass percentage of the high vanadium titanium iron powder is: TFe 65% to 67%, SiO2 2.6% to 3.6%, CaO 0.9% to 1.9%, MnO 0.08% to 0.12%, MgO 0.2% to 0.5%, Al2O3 0.8% to 1.1%, TiO2 0.8% to 2.2%, V 0.19% to 0.24%, and the balance is unavoidable impurities;
[0009] The mass percentage of the external mineral powder components is: TFe 55%-65%, SiO2 3.6%-6.6%, CaO 0.01%-0.21%, MnO 0.08%-0.8%, MgO 0.1%-0.17%, Al2O3 0.6%-5.9%, TiO2 0.02%-0.23%, V 0.001%-0.012%, and the remainder is inevitable impurities.
[0010] Compared with the prior art, the ore blending structure of the full-process vanadium-titanium sintered ore provided by the present invention adjusts the ore blending structure and proportion, uses high-content external ore powder and a small amount of iron concentrate, high vanadium-titanium iron vanadium and boron-magnesium-iron powder as the main raw materials, and adds a certain amount of steel slag and aluminum powder. Under the premise of ensuring the quality of the sintered ore and smooth blast furnace smelting, the amount of low-grade ore powder added is increased, the resource utilization of steel slag is realized, and the ore blending cost of the sintered ore is effectively reduced; in addition, the above-mentioned ore blending structure can effectively increase the vanadium content in molten iron, and the vanadium content in molten iron can reach more than 0.14%, thereby reducing the use of vanadium-titanium alloy, the molten iron cost can be reduced by 11 yuan / ton, and the steelmaking cost can be reduced by 0.68 yuan / ton, thereby effectively improving the market competitiveness of the enterprise and having high practical value.
[0011] Furthermore, based on 100% of the raw material of the vanadium-titanium sintered ore, the content of the ordinary iron powder is 3% to 5%, and the content of the 69 iron powder is 1% to 2%; wherein the mass percentage of the ordinary iron powder components is: TFe 65% to 67%, SiO2 4% to 4.5%, CaO 1.3% to 1.5%, MnO0.08% to 0.12%, MgO 0.3% to 0.5%, Al2O3 0.7% to 0.9%, TiO2 0.8% to 1.0%, V0.13% to 0.14%, and the remainder is unavoidable impurities.
[0012] Furthermore, the mass percentage of the 69 iron powder components is: TFe 68%-70%, SiO2 1.9%-2%, CaO 0.3%-0.5%, MnO 0.08%-0.12%, MgO 0.1%-0.3%, Al2O3 0.6%-0.7%, TiO2 0.6%-0.7%, V 0.08%-0.09%, and the remainder is inevitable impurities.
[0013] Furthermore, based on 100% of the raw material of the vanadium-titanium sintered ore, the high-vanadium-titanium iron powder includes 2% to 3% of the first iron powder, 3% to 4% of the second iron powder, 1% to 2% of the third iron powder and 1% to 2% of the fourth iron powder;
[0014] Among them, the mass percentage content of the first iron powder component is: TFe 65%-66%, SiO2 3.5%-3.6%, CaO 1.7%-1.9%, MnO 0.08%-0.12%, MgO 0.3%-0.5%, Al2O3 0.9%-1.1%, TiO2 0.9%-1.1%, V 0.23%-0.24%, and the remainder is inevitable impurities.
[0015] As a specific implementation of the present invention, the first iron powder can be Baotong high vanadium iron powder produced by Beijing Huaxia Jianlong Mining Technology Co., Ltd.
[0016] Furthermore, the mass percentage of the second iron powder component is: TFe 66%-67%, SiO2 2.6%-2.8%, CaO 0.9%-1.1%, MnO 0.08%-0.12%, MgO 0.2%-0.4%, Al2O3 0.8%-0.9%, TiO2 2%-2.2%, V 0.19%-0.2%, and the remainder is unavoidable impurities.
[0017] As a specific implementation of the present invention, the second iron powder can be Yuantong Jianlong high vanadium iron powder produced by Beijing Huaxia Jianlong Mining Technology Co., Ltd.
[0018] Furthermore, the mass percentage of the third iron powder component is: TFe 65%-67%, SiO2 3%-3.5%, CaO 1.6%-1.8%, MnO 0.08%-0.12%, MgO 0.2%-0.4%, Al2O3 0.9%-1.1%, TiO2 0.8%-0.9%, V 0.23%-0.24%, and the remainder is inevitable impurities.
[0019] As a specific implementation of the present invention, the third iron powder can be the Baitong Jianlong high vanadium iron powder produced by Beijing Huaxia Jianlong Mining Technology Co., Ltd.
[0020] Furthermore, the mass percentage of the third iron powder component is: TFe 65%-66%, SiO2 3%-3.5%, CaO 1.4%-1.5%, MnO 0.08%-0.12%, MgO 0.3%-0.5%, Al2O3 0.9%-1.1%, TiO2 1.6%-1.7%, V 0.23%-0.24%, and the remainder is inevitable impurities.
[0021] As a specific implementation of the present invention, the third iron powder can be Luanping Jianlong high vanadium iron powder produced by Beijing Huaxia Jianlong Mining Technology Co., Ltd.
[0022] Furthermore, based on 100% of the raw material of the vanadium-titanium sintered ore, the high-vanadium-titanium iron powder includes 2% to 4% of the first ore powder, 5% to 7% of the second ore powder, 5% to 6% of the third ore powder, 10% to 12% of the fourth iron powder, 5% to 7% of the fifth ore powder and 2% to 4% of the sixth ore powder;
[0023] The mass percentage of the first mineral powder component is: TFe 62% to 64%, SiO2 3.6% to 3.8%, CaO 0.19% to 0.21%, MnO 0.08% to 0.12%, MgO 0.12% to 0.14%, Al2O3 2.1% to 2.3%, TiO2 0.04% to 0.06%, V 0.001% to 0.003%, and the remainder is unavoidable impurities.
[0024] As a specific implementation of the present invention, the first mineral powder is the non-standard card powder of Hebei Jinxi International Trade Co., Ltd.
[0025] The mass percentage content of the second mineral powder component is: TFe 60%-62%, SiO2 3.8%-4%, CaO0.08%-0.1%, MnO 0.2%-0.4%, MgO 0.14%-0.16%, Al2O3 2.2%-2.4%, TiO20.04%-0.06%, V 0.002%-0.004%, and the balance is unavoidable impurities.
[0026] As a specific implementation of the present invention, the second mineral powder is Rio Tinto's PB powder.
[0027] The mass percentage content of the third mineral powder component is: TFe 57%-59%, SiO2 5.7%-5.9%, CaO0.01%-0.02%, MnO 0.2%-0.4%, MgO 0.14%-0.16%, Al2O3 2.7%-2.8%, TiO2 0.04%-0.06%, V 0.008%-0.012%, and the remainder is unavoidable impurities.
[0028] As a specific implementation of the present invention, the third mineral powder is the mixed powder of Hebei Jinxi International Trade Co., Ltd.
[0029] The mass percentage content of the fourth mineral powder component is: TFe 55%-57%, SiO2 6.1%-6.3%, CaO0.07%-0.09%, MnO 0.2%-0.4%, MgO 0.12%-0.14%, Al2O35.7%-5.9%, TiO20.21%-0.23%, V 0.005%-0.007%, and the balance is unavoidable impurities.
[0030] As a specific implementation of the present invention, the fourth mineral powder is 56 Indian powder produced by Hebei Jinxi International Trade Co., Ltd.
[0031] The mass percentage content of the fifth mineral powder component is: TFe 55%-56%, SiO2 6.1%-6.3%, CaO0.08%-0.1%, MnO 0.6%-0.8%, MgO 0.15%-0.17%, Al2O3 2.8%-3%, TiO2 0.08%-0.12%, V 0.003%-0.005%, and the balance is unavoidable impurities.
[0032] As a specific implementation of the present invention, the fifth mineral powder is the super special powder of Hebei Jinxi International Trade Co., Ltd.
[0033] The mass percentage of the sixth mineral powder component is: TFe 63%-65%, SiO2 6.5%-6.6%, CaO0.07%-0.09%, MnO 0.08%-0.12%, MgO 0.1%-0.12%, Al2O3 0.6%-0.7%, TiO2 0.02%-0.04%, V 0.003%-0.005%, and the balance is unavoidable impurities.
[0034] As a specific implementation of the present invention, the sixth mineral powder is Australian powder from Hebei Jinxi International Trade Co., Ltd.
[0035] Furthermore, the mass percentage of the steel slag components is: TFe 21%-23%, SiO2 11%-13%, CaO 23%-25%, MnO 1%-3%, MgO 4%-6%, Al2O3 3%-5%, TiO2 2.5%-2.7%, V0.84%-0.86%, and the remainder is inevitable impurities.
[0036] Furthermore, the mass percentage of the iron sheet components is: TFe 72% to 73%, SiO2 1.4% to 1.6%, CaO 0.01% to 0.02%, MnO 0.2% to 0.4%, MgO 0.1% to 0.2%, Al2O3 0.9% to 1.1%, TiO2 0.05% to 0.07%, V 0.01% to 0.03%, and the remainder is inevitable impurities.
[0037] Furthermore, the mass percentage of the aluminum powder components is: TFe 47% to 48%, SiO2 3.1% to 3.2%, CaO 0.5% to 0.7%, MnO 0.08% to 0.12%, MgO 0.18% to 0.2%, Al2O3 10% to 12%, TiO2 4.1% to 4.3%, V 0.11% to 0.13%, and the remainder is inevitable impurities.
[0038] Furthermore, the mass percentage of the deteriorating powder components is: TFe 60%-61%, SiO2 3%-5%, CaO 0.1%-0.3%, MnO 0.1%-0.3%, MgO 0.1%-0.13%, Al2O3 2.1%-2.3%, TiO2 0.05%-0.07%, V 0.001%-0.003%, and the remainder is inevitable impurities.
[0039] Furthermore, the mass percentage of the boron magnesium iron powder components is: TFe 54% to 55%, SiO2 4% to 6%, CaO 0.2% to 0.4%, MnO 0.08% to 0.12%, MgO 10% to 11%, Al2O3 0.2% to 0.3%, TiO2 0.08% to 0.1%, V 0.004% to 0.006%, and the remainder is unavoidable impurities.
[0040] Furthermore, the mass percentage of the vanadium-titanium sintered ore in the blast furnace charge is 70% to 75%, the mass percentage of the pelletized ore is 15% to 20%, and the mass percentage of the lump ore is 5% to 15%.
[0041] Furthermore, the particle size of the vanadium-titanium sintered ore is 18-22 mm, the particle size of the pelletized ore is 8-12 mm, and the particle size of the lump ore is 14-18 mm.
[0042] Furthermore, based on 100% of the raw material of the vanadium-titanium sintered ore, the flux includes 1% to 1.5% of limestone, 4% to 4.5% of quicklime and 5% to 5.5% of dolomite powder; the content of the fuel is 3.5% to 4%.
[0043] Specifically, the main components of the dolomite powder are: SiO2 2%, CaO 30%, MgO2 0.8%, and Al2O3 0.33%.
[0044] Specifically, the fuel is coke powder.
[0045] In order to reduce the cost, a certain amount of aluminum powder is added in the present invention, but the high aluminum content in the blast furnace slag will cause the slag to have high viscosity, which affects the smoothness of blast furnace smelting. In order to increase the permeability of the blast furnace soft melting zone and the blast furnace slag discharge capacity, the content of dolomite powder is increased, which is conducive to improving the smoothness of blast furnace smelting under the ore distribution structure of the present invention.
[0046] In a second aspect, the present invention also provides a method for blast furnace smelting of vanadium-titanium magnetite, which comprises blast furnace smelting of blast furnace charge, wherein the blast furnace charge has an ore blending structure of the full-process vanadium-titanium sintered ore as described in any one of the above items.
[0047] Furthermore, during the sintering process of the blast furnace charge, the material layer height is controlled to be 790mm~810mm, the moisture content of the mixed material is controlled to be 7.1%~7.3%, the sintering machine speed is 2.1m / min~2.3m / min, the sintering speed is 19mm / min~20mm / min, the sintering temperature is 1250℃~1280℃, and the insulation time is 120s~180s.
[0048] Furthermore, the pressure of the sintering process is -14kPa to -15KPa, the sintering end point temperature is 410°C to 430°C, and the drum is 77% to 78%.
[0049] Optimized blast furnace sintering process control can improve the quality of sintered ore and ensure the strength of sintered ore.
[0050] Furthermore, the distribution angles of blast furnace charge are: 5°~9.5° for ore platform, 8°~11° for coke platform; the maximum coke distribution angle is greater than the maximum ore distribution angle, and the minimum coke distribution angle is less than the minimum ore distribution angle; the ore gear and the coke gear include 5~6 gears, and as the gear increases, the coke distribution angle and the ore distribution angle decrease successively, and the ore distribution angles of two adjacent gears differ by 1°~3°, except for the center coke, the coke distribution angles of two adjacent gears differ by 1°~3°; the center coke angle is 10°~15°, and the proportion of center coke to the total coke is 24%~26%.
[0051] Furthermore, the minimum coke distribution angle is 1° smaller than the minimum ore distribution angle, and the maximum coke distribution angle is 0.5° to 1° larger than the maximum ore distribution angle.
[0052] Specifically, the ore distribution method is divided into 5 gears, and the distribution angles are 42°~42.8°, 40°~41°, 38°~39°, 36°~37°, 33°~34°, and the corresponding numbers of turns are 1~3 turns, 2~4 turns, 2~4 turns, 1~3 turns, and 1~3 turns. The coke distribution method is divided into 5 gears, and the distribution angles are 43°~44°, 40°~41°, 38°~39°, 34°~35°, 32°~33°, and the corresponding numbers of turns are 1~3 turns, 2~4 turns, 2~4 turns, 1~3 turns, and 1~3 turns.
[0053] As a specific embodiment of the present invention, the ore distribution method is: divided into 5 gears, the distribution angles are 42.8°, 40.8°, 38.8°, 36.3°, 33.3°, and the corresponding number of circles are 2 circles, 3 circles, 3 circles, 2 circles, and 2 circles. The coke distribution method is: divided into 5 gears, the distribution angles are 43.3°, 40.8°, 38.3°, 35.3°, 32.3°, and the corresponding number of circles are 2 circles, 3 circles, 3 circles, 2 circles, and 2 circles. The angle of the center focus is 13°, and the corresponding number of circles is 4 circles.
[0054] It should be noted that the ore platform is the angle difference between the outermost ring ore and the innermost ring ore; the coke platform is the outer ring coke angle minus the inner ring coke angle (excluding the center coke).
[0055] Low-grade iron powder and ore powder usually have a high Ti content. According to the blast furnace charge structure of the present invention, the Ti content in the molten iron will reach more than 0.1%, resulting in increased viscosity and poor fluidity of the molten iron, affecting the blast furnace permeability and molten iron output.
[0056] The blast furnace feeding method provided by the present invention can form a structure in which coke wraps ore, promote the mixing uniformity of coke and sintered ore, and promote the coke to fully reduce the sintered ore. The reduction and pulverization of the sintered ore can reach more than 68%, and the full progress of the reduction reaction is conducive to the formation of molten iron filings and slag on the top of the blast furnace, which is beneficial to the smooth flow of materials and gases in the blast furnace, promotes the smooth smelting of the blast furnace, and ensures the output of molten iron.
[0057] Furthermore, during the smelting process, the temperature of the molten steel entering the converter is ≥1350°C, and then the temperature of the molten steel is raised to 1400°C to 1450°C within 80s to 100s for converter smelting.
[0058] The rapid heating method can reduce the oxidation of vanadium in the molten iron during the smelting process, increase the vanadium content in the molten iron, and reduce the amount of vanadium-iron alloy added.
[0059] The present invention comprehensively considers the quality of sintered ore, the smooth progress of blast furnace smelting, and the quality and efficiency improvement of the whole process of molten iron smelting and steelmaking, and provides a new ore matching structure of vanadium-titanium sintered ore. By adjusting the ore matching structure and matching ratio, a variety of raw materials are mixed and used in specific contents, which not only ensures the grade of sintered ore and the smooth progress of blast furnace smelting, but also makes full use of low-priced low-quality iron ore resources and steel slag waste, thereby effectively reducing the smelting cost; at the same time, the ore matching structure provided by the present invention can also effectively increase the vanadium content in molten iron and reduce the use of vanadium-iron alloy; in addition, the steel slag obtained by smelting can be recycled as the steel slag raw material of the ore matching structure, reducing the ore matching cost and the generation of waste. By adopting the unique ore matching structure, blast furnace distribution and smelting process provided by the present invention, the whole process of sintered ore raw material cost, molten iron smelting and steelmaking alloy cost is reduced, the molten iron cost is reduced by 11 yuan / ton, and the steelmaking cost can be reduced by 0.68 yuan / ton of steel. While improving the quality, the cost of the whole process is reduced, which has high economic and environmental benefits and high promotion and application value. DETAILED DESCRIPTION
[0060] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0061] In order to better illustrate the present invention, further examples are given below.
[0062] The embodiment of the present invention provides a blast furnace charge structure, which includes a sintering ore distribution structure and a blast furnace charge structure, which includes 70% to 75% vanadium-titanium sintered ore, 15% to 20% pelletized ore, and 5% to 15% lump ore.
[0063] The particle size of the vanadium-titanium sintered ore is 18-22 mm, the particle size of the pelletized ore is 8-12 mm, and the particle size of the lump ore is 14-18 mm.
[0064] The raw materials of the vanadium-titanium sintered ore include sintered iron material, flux and fuel.
[0065] Taking the raw material of the vanadium-titanium sintered ore as 100%, the sintered iron material includes the following raw material components in percentage by mass: 4% to 7% iron concentrate, 7% to 11% high vanadium-titanium iron powder, 29% to 40% external ore powder, 1% to 2.5% steel slag, 0% to 2% iron sheet, 2% to 3% aluminum powder, 1% to 3% boron-magnesium-iron powder and 0% to 2% depreciation powder;
[0066] The flux comprises 1% to 1.5% limestone, 4% to 4.5% quicklime and 5% to 5.5% dolomite powder; the content of the fuel is 3.5% to 4%.
[0067] The components of the raw materials of the sintered iron material are shown in Table 1.
[0068] Table 1 Raw material composition (%)
[0069]
[0070]
[0071] Solution 1
[0072] The ingredients are mixed in the following manner to obtain sintered iron powder 1.
[0073] Ordinary iron powder 4%, 69 iron powder 2%, high vanadium iron powder 1 (Baotong) 2.5%, high vanadium iron powder 2 (Yuantong Jianlong) 3.5%, high vanadium iron powder 4 (Baitong Jianlong) 1.2%, high vanadium iron powder 5 (Luanping Jianlong) 1%, non-standard card powder 3%, PB powder 6%, mixed powder 5.18%, 56 Indian powder 11%, super special powder 6%, Australian powder 3%, iron sheet 1%, aluminum powder 2.5%, boron magnesium iron powder 1.5%, steel slag 1.8%, depreciation powder 1%.
[0074] The flux is 1% limestone, 4.2% quicklime and 5.2% dolomite powder; 3.6% fuel coke powder; 11% elevated return ore, 14% internal return ore, and the remainder is gas ash and dust removal ash.
[0075] Internal return refers to the screening of sintered ore after leaving the sintering machine. Those with a size of ≥5mm enter the blast furnace frame, and those with a size of <5mm are screened out and returned for sintering. In other words, internal return refers to the sintered ore with a size of <5mm that is screened out after sintering in the sintering machine. The sintered ore entering the blast furnace frame is squeezed out of the frame cabin and then screened. Those with a size of ≥5mm enter the blast furnace metallurgy, and those with a size of <5mm are returned to the frame for sintering.
[0076] The sintered iron powder, flux, fuel and other sintered ore components are sintered according to the process shown in Table 2.
[0077] Table 2 Sintering parameters and technical indicators
[0078]
[0079] The blast furnace charging method is as follows: Ore distribution: divided into 5 gears, the distribution angles are 42.8°, 40.8°, 38.8°, 36.3°, 33.3°, and the corresponding number of circles are 2 circles, 3 circles, 3 circles, 2 circles, and 2 circles. Coke distribution: divided into 5 gears, the distribution angles are 43.3°, 40.8°, 38.3°, 35.3°, 32.3°, and the corresponding number of circles are 2 circles, 3 circles, 3 circles, 2 circles, and 2 circles. The angle of the center focus is 13°, and the corresponding number of circles is 4 circles.
[0080] During the smelting process, the temperature of the molten steel entering the converter is ≥1350℃, and then the temperature of the molten steel is raised to 1400℃~1450℃ within 80s~100s for converter smelting.
[0081] The composition of the sintered ore, basicity R2, low-temperature reduction pulverization rate (referred to as low pulverization), vanadium content in molten iron and molten iron cost obtained by smelting are shown in Table 3.
[0082] Table 3
[0083]
[0084] Note: The testing standard for low-temperature reduction powdering rate is GB / T13242-91.
[0085] Solution 2
[0086] The ingredients are mixed in the following manner to obtain sintered iron powder 2.
[0087] Ordinary iron powder 5%, 69 iron powder 2%, high vanadium iron powder 1 (Baotong) 2.5%, high vanadium iron powder 5 (Luanping Jianlong) 0.5%, non-standard card powder 3%, PB powder 6%, mixed powder 10.215%, 56 Indian powder 11%, super special powder 6%, Australian powder 3%, iron sheet 1%, aluminum powder 2.5%, boron magnesium iron powder 1.0% and depreciation powder 1%.
[0088] The flux is 1% limestone, 4.2% quicklime and 5.2% dolomite powder; 3.6% fuel coke powder; 11% elevated return ore, 14% internal return ore, and the remainder is gas ash and dust removal ash.
[0089] The sintered iron powder, flux, fuel and other sintered ore components are sintered according to the process shown in Table 4.
[0090] Table 4 Sintering parameters and technical indicators
[0091]
[0092] The blast furnace charging and smelting methods are controlled according to Scheme 1.
[0093] The composition of the sintered ore, basicity R2, low-temperature reduction pulverization rate (referred to as low pulverization), vanadium content in molten iron and molten iron cost obtained by smelting are shown in Table 5.
[0094] Table 5
[0095]
[0096] Note: The testing standard for low-temperature reduction powdering rate is GB / T13242-91.
[0097] Option 3
[0098] The ingredients are mixed in the following manner to obtain sintered iron powder 3.
[0099] Ordinary iron powder 5%, 69 iron powder 2%, high vanadium iron powder 1 (Baotong) 2.5%, high vanadium iron powder 3 (Enshunqiang (Dingxin)) 2%, high vanadium iron powder 5 (Luanping Jianlong) 0.5%, non-standard card powder 3%, PB powder 6%, mixed powder 8.445%, 56 Indian powder 11%, super special powder 6%, Australian powder 3%, iron sheet 1%, aluminum powder 2.5%, boron magnesium iron powder 1.5%, steel slag 1.0%, and depreciation powder 1%.
[0100] The flux is 1% limestone, 4.2% quicklime and 5.2% dolomite powder; 3.6% fuel coke powder; 11% elevated return ore, 14% internal return ore, and the remainder is gas ash and dust removal ash.
[0101] The above-mentioned sintered iron powder, flux, fuel and other sintered ore components are sintered according to the process shown in Table 6.
[0102] Table 6 Sintering parameters and technical indicators
[0103]
[0104] The blast furnace charging and smelting methods are controlled according to Scheme 1.
[0105] The composition of the sintered ore, basicity R2, low-temperature reduction pulverization rate (referred to as low pulverization), vanadium content in molten iron and molten iron cost obtained by smelting are shown in Table 7.
[0106] Table 7
[0107]
[0108] Note: The testing standard for low-temperature reduction powdering rate is GB / T13242-91.
[0109] Option 4
[0110] The ingredients are mixed in the following manner to obtain sintered iron powder 4.
[0111] Ordinary iron powder 8.7%, 69 iron powder 2%, high vanadium iron powder 1 (Baotong) 2.5%, high vanadium iron powder 3 (Enshunqiang (Dingxin)) 2%, high vanadium iron powder 5 (Luanping Jianlong) 0.5%, non-standard card powder 3%, PB powder 6%, mixed powder 5.065%, 56 Indian powder 11%, super special powder 6%, Australian powder 3%, iron sheet 1%, aluminum powder 2.5%, boron magnesium iron powder 1.5%, steel slag 1.5%, and depreciation powder 1%.
[0112] The flux is 1% limestone, 4.2% quicklime and 5.2% dolomite powder; 3.6% fuel coke powder; 11% elevated return ore, 14% internal return ore, and the remainder is gas ash and dust removal ash.
[0113] The above-mentioned sintered iron powder, flux, fuel and other sintered ore components are sintered according to the process shown in Table 8.
[0114] Table 8 Sintering parameters and technical indicators
[0115]
[0116]
[0117] The blast furnace charging and smelting methods are controlled according to Scheme 1.
[0118] The composition of the sintered ore, basicity R2, low-temperature reduction pulverization rate (referred to as low pulverization), vanadium content in molten iron and molten iron cost obtained by smelting are shown in Table 9.
[0119] Table 9
[0120]
[0121] Note: The testing standard for low-temperature reduction powdering rate is GB / T13242-91.
[0122] Option 5
[0123] The existing traditional ore blending scheme is as follows:
[0124] Fuzhen full iron powder 8%, ordinary iron powder 7%, iron sheet 2%, mixed powder 18%, 56 Indian powder 11%, super special powder 5%, depreciation powder 1%.
[0125] The V content in the molten iron obtained by smelting is 0.025%, and the cost of the molten iron is 2612 yuan / ton.
[0126] The flux is 2.5% limestone, 4.6% quicklime and 4.8% dolomite powder; 3.6% fuel coke powder; 11% elevated return ore, 15% internal return ore, and the remainder is gas ash and dust removal ash.
[0127] In summary, under the blast furnace charge structure provided by the present invention, while ensuring that the quality of the sintered ore meets the requirements of blast furnace smelting, the amount of expensive high-grade iron powder can be reduced to the maximum proportion, which can not only ensure that the sintered ore has sufficient strength, but also greatly reduce the cost of the entire process, and has good economic benefits.
[0128] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A full-process vanadium-titanium sintered ore blending structure, wherein the raw materials of the vanadium-titanium sintered ore include sintered iron material, flux and fuel, characterized in that: Taking the raw material of the vanadium-titanium sintered ore as 100%, the sintered iron material includes the following raw material components in percentage by mass: 4% to 7% iron concentrate, 7% to 11% high vanadium-titanium iron powder, 29% to 40% external ore powder, 1% to 2.5% steel slag, 0% to 2% iron sheet, 2% to 3% aluminum powder, 1% to 3% boron-magnesium-iron powder and 0% to 2% depreciation powder; The iron concentrate includes ordinary iron powder and 69 iron powder; the mass percentage of the high vanadium titanium iron powder components is: TFe 65% to 67%, SiO2 2.6% to 3.6%, CaO 0.9% to 1.9%, MnO0.08% to 0.12%, MgO 0.2% to 0.5%, Al2O3 0.8% to 1.1%, TiO2 0.8% to 2.2%, V0.19% to 0.24%, and the balance is unavoidable impurities; The mass percentage of the external mineral powder components is: TFe 55%-65%, SiO2 3.6%-6.6%, CaO 0.01%-0.21%, MnO 0.08%-0.8%, MgO 0.1%-0.17%, Al2O3 0.6%-5.9%, TiO2 0.02%-0.23%, V 0.001%-0.012%, and the remainder is inevitable impurities.
2. The ore blending structure of the full-process vanadium-titanium sintered ore according to claim 1 is characterized in that: Taking the raw material of the vanadium-titanium sintered ore as 100%, the content of the common iron powder is 3% to 5%, and the content of the 69 iron powder is 1% to 2%; wherein the mass percentage of the common iron powder components is: TFe 65% to 67%, SiO2 4% to 4.5%, CaO 1.3% to 1.5%, MnO 0.08% to 0.12%, MgO 0.3% to 0.5%, Al2O3 0.7% to 0.9%, TiO2 0.8% to 1.0%, V 0.13% to 0.14%, and the remainder is unavoidable impurities; The mass percentage of the 69 iron powder components is: TFe 68%-70%, SiO2 1.9%-2%, CaO 0.3%-0.5%, MnO 0.08%-0.12%, MgO 0.1%-0.3%, Al2O3 0.6%-0.7%, TiO2 0.6%-0.7%, V 0.08%-0.09%, and the remainder is inevitable impurities.
3. The ore blending structure of the full-process vanadium-titanium sintered ore according to claim 1 is characterized in that ,, based on the raw material of the vanadium-titanium sintered ore as 100%, the high-vanadium-titanium iron powder includes 2% to 3% of the first iron powder, 3% to 4% of the second iron powder, 1% to 2% of the third iron powder and 1% to 2% of the fourth iron powder; The mass percentage of the first iron powder component is: TFe 65% to 66%, SiO2 3.5% to 3.6%, CaO 1.7% to 1.9%, MnO 0.08% to 0.12%, MgO 0.3% to 0.5%, Al2O3 0.9% to 1.1%, TiO2 0.9% to 1.1%, V 0.23% to 0.24%, and the balance is unavoidable impurities; The mass percentage of the second iron powder component is: TFe 66%-67%, SiO2 2.6%-2.8%, CaO0.9%-1.1%, MnO 0.08%-0.12%, MgO 0.2%-0.4%, Al2O3 0.8%-0.9%, TiO2 2%-2.2%, V 0.19%-0.2%, and the balance is unavoidable impurities; The mass percentage of the third iron powder component is: TFe 65%-67%, SiO2 3%-3.5%, CaO 1.6%-1.8%, MnO 0.08%-0.12%, MgO 0.2%-0.4%, Al2O3 0.9%-1.1%, TiO2 0.8%-0.9%, V 0.23%-0.24%, and the balance is unavoidable impurities; The mass percentage of the third iron powder component is: TFe 65%-66%, SiO2 3%-3.5%, CaO 1.4%-1.5%, MnO 0.08%-0.12%, MgO 0.3%-0.5%, Al2O3 0.9%-1.1%, TiO2 1.6%-1.7%, V 0.23%-0.24%, and the remainder is inevitable impurities.
4. The ore blending structure of the full-process vanadium-titanium sintered ore according to claim 1, characterized in that: Taking the raw material of the vanadium-titanium sintered ore as 100%, the high-vanadium-titanium iron powder includes 2% to 4% of the first ore powder, 5% to 7% of the second ore powder, 5% to 6% of the third ore powder, 10% to 12% of the fourth iron powder, 5% to 7% of the fifth ore powder and 2% to 4% of the sixth ore powder; The mass percentage of the first mineral powder component is: TFe 62%-64%, SiO2 3.6%-3.8%, CaO 0.19%-0.21%, MnO 0.08%-0.12%, MgO 0.12%-0.14%, Al2O3 2.1%-2.3%, TiO2 0.04%-0.06%, V 0.001%-0.003%, and the balance is unavoidable impurities; The mass percentage content of the second mineral powder component is: TFe 60%-62%, SiO2 3.8%-4%, CaO 0.08%-0.1%, MnO 0.2%-0.4%, MgO 0.14%-0.16%, Al2O3 2.2%-2.4%, TiO2 0.04%-0.06%, V 0.002%-0.004%, and the balance is unavoidable impurities; The mass percentage of the third mineral powder component is: TFe 57%-59%, SiO2 5.7%-5.9%, CaO 0.01%-0.02%, MnO 0.2%-0.4%, MgO 0.14%-0.16%, Al2O3 2.7%-2.8%, TiO2 0.04%-0.06%, V 0.008%-0.012%, and the balance is unavoidable impurities; The mass percentage of the fourth mineral powder component is: TFe 55%-57%, SiO2 6.1%-6.3%, CaO 0.07%-0.09%, MnO 0.2%-0.4%, MgO 0.12%-0.14%, Al2O3 5.7%-5.9%, TiO2 0.21%-0.23%, V 0.005%-0.007%, and the balance is unavoidable impurities; The mass percentage of the fifth mineral powder component is: TFe 55%-56%, SiO2 6.1%-6.3%, CaO0.08%-0.1%, MnO 0.6%-0.8%, MgO 0.15%-0.17%, Al2O3 2.8%-3%, TiO2 0.08%-0.12%, V 0.003%-0.005%, and the balance is unavoidable impurities; The mass percentage of the sixth mineral powder component is: TFe 63%-65%, SiO2 6.5%-6.6%, CaO0.07%-0.09%, MnO 0.08%-0.12%, MgO 0.1%-0.12%, Al2O3 0.6%-0.7%, TiO2 0.02%-0.04%, V 0.003%-0.005%, and the balance is unavoidable impurities.
5. The ore blending structure of the full-process vanadium-titanium sintered ore according to claim 1, characterized in that: The mass percentage of the steel slag components is: TFe 21%-23%, SiO2 11%-13%, CaO23%-25%, MnO 1%-3%, MgO4%-6%, Al2O3 3%-5%, TiO2 2.5%-2.7%, V0.84%-0.86%, and the balance is unavoidable impurities; The mass percentage of the iron scale components is: TFe 72%-73%, SiO2 1.4%-1.6%, CaO 0.01%-0.02%, MnO 0.2%-0.4%, MgO 0.1%-0.2%, Al2O3 0.9%-1.1%, TiO2 0.05%-0.07%, V 0.01%-0.03%, and the remainder is inevitable impurities.
6. The ore blending structure of the full-process vanadium-titanium sintered ore according to claim 1, characterized in that: The mass percentage of the aluminum powder components is: TFe 47% to 48%, SiO2 3.1% to 3.2%, CaO 0.5% to 0.7%, MnO 0.08% to 0.12%, MgO 0.18% to 0.2%, Al2O3 10% to 12%, TiO2 4.1% to 4.3%, V 0.11% to 0.13%, and the balance is unavoidable impurities; The mass percentage of the depreciation powder components is: TFe 60%-61%, SiO2 3%-5%, CaO 0.1%-0.3%, MnO 0.1%-0.3%, MgO 0.1%-0.13%, Al2O3 2.1%-2.3%, TiO2 0.05%-0.07%, V 0.001%-0.003%, and the balance is unavoidable impurities; The mass percentage of the boron magnesium iron powder components is: TFe 54%-55%, SiO2 4%-6%, CaO 0.2%-0.4%, MnO 0.08%-0.12%, MgO 10%-11%, Al2O3 0.2%-0.3%, TiO2 0.08%-0.1%, V 0.004%-0.006%, and the remainder is inevitable impurities.
7. The ore blending structure of the full-process vanadium-titanium sintered ore according to claim 1, characterized in that: The mass percentage of the vanadium-titanium sintered ore in the blast furnace charge is 70% to 75%, the mass percentage of the pelletized ore is 15% to 20%, and the mass percentage of the lump ore is 5% to 15%.
8. The ore blending structure of the full-process vanadium-titanium sintered ore according to claim 1, characterized in that: Taking the raw material of the vanadium-titanium sintered ore as 100%, the flux includes 1% to 1.5% limestone, 4% to 4.5% quicklime and 5% to 5.5% dolomite powder; the content of the fuel is 3.5% to 4%.
9. A method for smelting vanadium-titanium magnetite in a blast furnace, the method comprising smelting a blast furnace charge in a blast furnace, characterized in that: The blast furnace charge includes the ore blending structure of the full-process vanadium-titanium sintered ore as described in any one of claims 1 to 8.
10. The blast furnace smelting method of vanadium-titanium magnetite according to claim 9, characterized in that: During the sintering process of the blast furnace charge, the material layer height is controlled to be 790 mm to 810 mm, the moisture content of the mixed material is controlled to be 7.1% to 7.3%, the sintering machine speed is 2.1 m / min to 2.3 m / min, the sintering speed is 19 mm / min to 20 mm / min, the sintering temperature is 1250° C. to 1280° C., and the holding time is 120 s to 180 s; The angles of blast furnace charge distribution are: ore platform is 5°~9.5°, coke platform angle is 8°~11°; The maximum coke distribution angle is greater than the maximum ore distribution angle, and the minimum coke distribution angle is less than the minimum ore distribution angle; the ore gear and the coke gear include 5 to 6 gears, and as the gear increases, the coke distribution angle and the ore distribution angle decrease successively, and the ore distribution angles of two adjacent gears differ by 1° to 3°. Except for the center coke, the coke distribution angles of two adjacent gears differ by 1° to 3°; the center coke angle is 10° to 15°, and the proportion of the center coke to the total coke is 24% to 26%; During the smelting process, the temperature of the molten steel entering the converter is ≥1350℃, and then the temperature of the molten steel is raised to 1400℃~1450℃ within 80s~100s for converter smelting.
Citation Information
Patent Citations
Method for preparing sinter by sintering titanium-iron concentrate
CN104630457A
Blast furnace smelting method by using vanadium-titanium two-phase sintering ore
CN104673951A
Method for conducting sintering-blast furnace iron making on vanadium-contained solid waste in ore blending manner
CN105238893A
Method for preparing sintered ore from high-grade high-vanadium chromium-containing vanadium-titanium magnetite concentrate mixture
CN107267749A
Blast furnace smelting method of high-grade high-vanadium chromium-contained type vanadium-titanium iron ore concentrates