Method for extracting lithium from electrolytic aluminum lithium-rich waste residues
The first acidified leachate is generated by reacting hydrochloric acid, water, aluminum chloride, and lithium-containing electrolyte. After filtration, sodium carbonate is added for neutralization. The third waste residue is recycled to replace part of the aluminum chloride, which solves the problem of waste residue treatment in the lithium extraction process of lithium-rich electrolytes and achieves efficient recovery of lithium resources and cost reduction.
Patent Information
- Application Number
- CN202411333579.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies generate a large amount of waste residue with a pH of around 7 during lithium extraction using lithium-rich electrolytes, resulting in lithium resource loss. Furthermore, they require a large amount of chemical raw materials, leading to high production costs and making it difficult to effectively utilize the waste residue.
The first acidified leachate is generated by reacting hydrochloric acid, water, aluminum chloride and lithium-containing electrolyte. After filtration, sodium carbonate is added for neutralization. The third waste residue is recycled to replace part of the aluminum chloride. Lithium carbonate is obtained by lithium precipitation crystallization.
This approach enables full utilization of lithium resources, reduces waste residue disposal, lowers production costs, and improves lithium yield and product purity.
Smart Images

Figure CN118932190A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrolytic aluminum waste slag treatment, and specifically relates to a method for extracting lithium from electrolytic aluminum lithium-rich waste slag. Background Art
[0002] In aluminum electrolysis production, in order to improve the properties of the electrolyte and achieve the purpose of improving current efficiency and reducing energy consumption, in addition to adding aluminum fluoride or cryolite to the electrolyte, some salts such as fluoride or chloride are also added to the electrolyte. One of the commonly used additives is lithium fluoride. Lithium-containing fluoride salts are currently used in the electrolytic aluminum industry to good effect. They can effectively reduce the initial crystallization temperature of the electrolyte, reduce fluorine emissions, and promote energy conservation and consumption reduction in electrolytic aluminum enterprises. Using lithium-containing electrolytic aluminum waste slag and concentrated sulfuric acid as raw materials, battery-grade lithium carbonate is prepared through a series of processes such as acid leaching, and cryolite is produced as a by-product.
[0003] In recent years, with the rise of lithium prices, the use of lithium-rich electrolyte waste slag from aluminum plants to extract lithium has occupied a place in the domestic lithium industry. For example, the Chinese patent with publication number CN105293536A discloses a method for extracting lithium from electrolytic aluminum waste slag, which includes the following steps: reacting lithium-containing electrolytic aluminum waste slag with concentrated sulfuric acid at 200-400°C to obtain a mixture A; leaching the mixture A with water and filtering to obtain a filtrate A and a filter residue A; adding sodium carbonate to the filtrate A to perform an alkaline hydrolysis reaction at 20-40°C, and then filtering to obtain a filtrate B and a filter residue B; adding water to the filter residue B to make a slurry and then adding lime for causticization reaction, and then filtering to obtain a filtrate C and a filter residue C. In step 4), CO2 is introduced into the filtrate C for carbonization reaction, and then filtered, washed, and dried to obtain. The obtained battery-grade lithium carbonate has low impurity ion content and excellent product quality, which solves the current problems of low yield, high production cost and weak market competitiveness in the preparation of battery-grade lithium carbonate from ore lithium extraction; it opens up a new process for producing high-value-added, high-quality lithium products from low-grade lithium resources, with a simple process, easy industrial operation, and significant economic and social benefits.
[0004] However, it requires the addition of more chemical raw materials, and during the lithium extraction process of lithium-rich electrolytes, the waste slag produced by solution neutralization and impurity removal has always been a difficult problem in the industry, especially the large amount of waste slag generated at around pH = 7 in the process, and the lithium content is high, most of which is sent to the processing plant, causing certain losses; Based on the above problems, how to comprehensively and effectively utilize the waste slag from lithium-containing electrolytes needs to be urgently solved.
[0005] Therefore, those skilled in the art are committed to developing a method for extracting lithium from lithium-rich waste slag from aluminum electrolysis that fully utilizes the waste slag and has a good lithium extraction effect. Summary of the invention
[0006] The present invention aims to provide a method for extracting lithium from lithium-rich waste slag from aluminum electrolysis, which fully utilizes the waste slag and has a good lithium extraction effect.
[0007] In order to solve the above problems, the present invention provides a method for extracting lithium from lithium-rich waste slag of electrolytic aluminum, comprising the following steps:
[0008] S1. adding hydrochloric acid, water, aluminum chloride and a lithium-containing electrolyte to the initial waste residue to react and obtain a first acidified leachate, wherein the pH of the initial waste residue is 7;
[0009] S2. filtering the first acidified leachate to obtain a first filtrate and a first waste residue, wherein the first waste residue is discarded and collected;
[0010] S3. adding sodium carbonate to the first filtrate for neutralization to obtain a neutralized first filtrate, filtering the neutralized first filtrate to obtain a second filtrate and a second waste residue, and adding sodium carbonate to the second filtrate for neutralization to obtain a neutralized second filtrate;
[0011] S4. After filtering the neutralized second filtrate, a third filtrate and a third waste residue are obtained, and the third waste residue is added to step S1 to replace part of the aluminum chloride to participate in the reaction, and the replacement mass is 20-60% of the aluminum chloride used in step S1;
[0012] S5. The third waste residue is subjected to lithium precipitation and crystallization to obtain lithium carbonate.
[0013] Furthermore, in step S1, the reaction temperature is 80-90° C., and the reaction time is 5-7 h.
[0014] Furthermore, the mass volume ratio of some raw materials used in the whole method steps is: lithium-containing electrolyte lithium extraction waste residue: hydrochloric acid: aluminum chloride: lithium-containing electrolyte: pure water = 250-400g: 250-400mL: 150-400g: 500-700g: 800-1000mL.
[0015] Furthermore, the third waste residue in step S4 is recycled once.
[0016] Further, the method steps of obtaining lithium carbonate by precipitating lithium crystals in step S5 are as follows:
[0017] S6. Mix the following raw materials in a mass volume ratio: the third waste residue: pure water: hydrochloric acid = 300 g: 600 mL: 100-200 mL, and then stir at 80 ° C for 1.5-3 h to obtain a second acidified leachate, wherein the pH of the second waste residue is 7;
[0018] S7. The second acidified leachate is filtered and concentrated 4 times to obtain a concentrate after two neutralization reactions;
[0019] S8. The concentrated solution is subjected to lithium crystallization to obtain lithium carbonate.
[0020] Furthermore, the concentration of the sodium carbonate is 210-240 g / l.
[0021] The beneficial effects of the present invention are as follows: the method for extracting lithium from lithium-rich waste slag of aluminum electrolysis of the present invention comprises the following steps: S1. adding hydrochloric acid, water, aluminum chloride and lithium-containing electrolyte to the initial waste slag to react and obtain a first acidified leachate, wherein the pH of the initial waste slag is 7; S2. filtering the first acidified leachate to obtain a first filtrate and a first waste slag, and the first waste slag is discarded and collected; S3. adding sodium carbonate to the first filtrate to neutralize and obtain a neutralized first filtrate, filtering the neutralized first filtrate to obtain a second filtrate and a second waste slag, and adding sodium carbonate to the second filtrate to neutralize and obtain a neutralized second filtrate; S4. filtering the neutralized second filtrate to obtain a third filtrate and a third waste slag, and the third waste slag is added to step S1 to replace part of the aluminum chloride to participate in the reaction; S5. the third waste slag is crystallized by lithium precipitation to obtain lithium carbonate. The third waste slag replaces part of the aluminum chloride, fully utilizes the waste slag, and achieves the purpose of saving resources and utilizing waste. The waste slag generated in the production process can be effectively utilized to fully utilize lithium resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 One of the process flow charts of the present invention:
[0023] Figure 2 This is the second process flow chart of the present invention. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0025] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, may be combined in any manner and, unless otherwise stated, may be replaced by other equivalent or alternative features having similar purposes, that is, unless otherwise stated, each feature is merely one embodiment of a series of equivalent or similar features.
[0026] Example 1
[0027] The auxiliary material aluminum chloride hexahydrate used in traditional lithium recovery is a major production cost, and the amount used is about 0.8 times the mass of the raw material lithium-containing electrolyte. The flow chart of this embodiment is as follows: Figure 1 and Figure 2 As shown, the lithium-containing electrolyte is acidified and leached and then filtered. After filtration, the filtrate is neutralized and impurities are removed by adding sodium carbonate, and the filter residue is collected; after the filtrate is neutralized and impurities are removed, it is filtered again, and the waste residue after filtration is added to the lithium-containing electrolyte in the reaction system for repeated use.
[0028] The specific steps are as follows:
[0029] A method for extracting lithium from lithium-rich waste slag from aluminum electrolysis, comprising the following steps:
[0030] S1. Add hydrochloric acid, water, aluminum chloride and lithium-containing electrolyte to the initial waste residue to react and obtain the first acidified leaching solution, wherein the pH of the initial waste residue is 7, wherein the initial waste residue (PH=7, Al content is 28435ppm) 250g, hydrochloric acid 250ml, aluminum chloride 360g, raw material lithium-containing electrolyte 600g, water 950ml; the reaction temperature is controlled at 85°C, and the reaction time is 6h. Obtain 800mL of the first acidified leaching solution, the lithium content is 12.08g / L, and the acid leaching yield is 80.02%.
[0031] S2. filtering the first acidified leachate to obtain a first filtrate and a first waste residue, wherein the first waste residue is discarded and collected;
[0032] S3. adding sodium carbonate to the first filtrate for neutralization to obtain a neutralized first filtrate, filtering the neutralized first filtrate to obtain a second filtrate and a second waste residue, adding sodium carbonate to the second filtrate for neutralization to obtain a neutralized second filtrate, wherein the concentration of the sodium carbonate is 210 to 240 g / l.
[0033] S4. The neutralized second filtrate is filtered to obtain a third filtrate and a third waste residue, and the third waste residue is added to step S1 to replace part of the aluminum chloride to participate in the reaction, and the replacement mass is 20-60% of the aluminum chloride used in step S1; the third waste residue is recycled once, and the mass of the third waste residue is 832g, the lithium content in the residue is 0.29%, the total amount of lithium in the solution is calculated to be 9.664g, and the total amount of lithium in the residue is 2.413g;
[0034] S5. The third waste residue is crystallized by lithium precipitation to obtain lithium carbonate;
[0035] S6. Mix the following raw materials in a mass volume ratio: the third waste residue: pure water: hydrochloric acid = 300 g: 600 mL: 100 mL, and then stir at 80 ° C for 1.5 to obtain a second acidified leachate, wherein the pH of the third waste residue is 7;
[0036] S7. The second acidified leachate was filtered and concentrated 4 times after two neutralization reactions to obtain a concentrate having a lithium content of 15 g / L;
[0037] S8. The concentrated solution is crystallized with lithium to obtain lithium carbonate. The obtained lithium carbonate is 9.02 g. The test results meet the national standard GB / T 11075-2013 Li2CO3-2 standard, with a main content of 98.68%.
[0038] The following three embodiments have the same steps as those in Embodiment 1 and will not be described in detail.
[0039] Embodiment 2: Initial waste residue (pH=7, Al content is 32423ppm) 300g, hydrochloric acid 300ml, aluminum chloride 270g, raw material lithium electrolyte 600g, water 900mL, reaction temperature control 85 ℃, reaction time 6h end. The test results are that the volume of the first acidified leaching solution is 810mL, the lithium content is 13.26g / L, the third waste residue mass is 908g, the lithium content in the residue is 0.203%, the total amount of lithium in the solution is 10.741g, the total amount of lithium in the residue is 1.843g, and the acid leaching yield is 85.35%.
[0040] 300g of lithium-containing electrolyte lithium extraction waste residue (PH=7), 600mL of water, 130mL of hydrochloric acid, heated to 80°C, stirred for 2h, filtered the filtrate and subjected to two neutralization reactions. After filtration, the solution was concentrated 4 times, the lithium content was 15g / L, lithium was precipitated and crystallized, and the obtained lithium carbonate was 9.55g. The test results met the national standard GB / T 11075-2013Li2CO3-2, with a main content of 98.88%.
[0041] Embodiment 3: Initial waste residue (PH=7, containing Al 65322ppm) 350g, hydrochloric acid 350ml, aluminum chloride 180g, raw material containing lithium electrolyte 600g, water 850mL, reaction temperature control 85 ℃, reaction time 6h end. Test results are acid leaching volume 800mL, lithium content 14.68g / L, slag mass 935g, lithium content in slag 0.151%, calculated solution lithium total amount 11.744g, total amount of lithium in slag 1.412g, acid leaching yield 89.27%.
[0042] 300g of lithium-containing electrolyte lithium extraction waste residue (PH=7), 600mL of water, 180mL of hydrochloric acid, heated to 80°C, stirred for 2.5h, filtered the filtrate and subjected to two neutralization reactions. After filtration, the solution was concentrated 4 times, the lithium content was 15g / L, lithium was precipitated and crystallized, and the obtained lithium carbonate was 10.11g. The test results met the national standard GB / T 11075-2013Li2CO3-1, with a main content of 99.06%.
[0043] Example 4: Lithium-containing electrolyte lithium extraction waste residue (PH = 7, containing Al 71499ppm) 400g, hydrochloric acid 400ml, aluminum chloride 150g, raw material lithium electrolyte 600g, water 800mL, reaction temperature control 85 ° C, reaction time 6h end. The test results are acid leaching volume 805mL, lithium content 15.95g / L, slag mass 987g, slag lithium content 0.085%, calculated solution lithium total 12.84g, slag total lithium 0.839g, acid leaching yield 93.87%.
[0044] 300g of lithium-containing electrolyte lithium extraction waste residue (PH=7), 600mL of water, and 200mL of hydrochloric acid were heated to 80°C and stirred for 3h. The filtrate was filtered and subjected to two neutralization reactions. After filtration, the solution was concentrated 4 times, and the lithium content was 15g / L. Lithium was precipitated and crystallized, and the obtained lithium carbonate was 10.81g. The test results met the national standard GB / T 11075-2013Li2CO3-0, with a main content of 99.33%.
[0045] It can be concluded from the above 4 groups of experiments that experiment 4 is the best ratio, lithium carbonate quality, and yield.
[0046] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for extracting lithium from lithium-rich waste slag from aluminum electrolysis, characterized in that: The following steps are involved: S1. adding hydrochloric acid, water, aluminum chloride and a lithium-containing electrolyte to the initial waste residue to react and obtain a first acidified leachate, wherein the pH of the initial waste residue is 7; S2. filtering the first acidified leachate to obtain a first filtrate and a first waste residue, wherein the first waste residue is discarded and collected; S3. adding sodium carbonate to the first filtrate for neutralization to obtain a neutralized first filtrate, filtering the neutralized first filtrate to obtain a second filtrate and a second waste residue, and adding sodium carbonate to the second filtrate for neutralization to obtain a neutralized second filtrate; S4. After filtering the neutralized second filtrate, a third filtrate and a third waste residue are obtained, and the third waste residue is added to step S1 to replace part of the aluminum chloride to participate in the reaction, and the replacement mass is 20-60% of the aluminum chloride used in step S1; S5. The third waste residue is subjected to lithium precipitation and crystallization to obtain lithium carbonate.
2. The method for extracting lithium from lithium-rich waste slag from aluminum electrolysis according to claim 1, characterized in that: In step S1, the reaction temperature is 80-90°C and the reaction time is 5-7h.
3. The method for extracting lithium from lithium-rich waste slag from aluminum electrolysis according to claim 2, characterized in that: The mass volume ratio of some raw materials used in the whole method steps is: lithium-containing electrolyte lithium extraction waste residue: hydrochloric acid: aluminum chloride: lithium-containing electrolyte: pure water = 250-400g: 250-400mL: 150-400g: 500-700g: 800-1000mL.
4. The method for extracting lithium from lithium-rich waste slag from aluminum electrolysis according to claim 1, characterized in that: The third waste residue in step S4 is recycled once.
5. The method for extracting lithium from lithium-rich waste slag from aluminum electrolysis according to claim 1, characterized in that: In step S5, the method steps of obtaining lithium carbonate by precipitation of lithium crystals are as follows: S6. Mix the following raw materials in a mass volume ratio: the third waste residue: pure water: hydrochloric acid = 300 g: 600 mL: 100-200 mL, and then stir at 80 ° C for 1.5-3 h to obtain a second acidified leachate, wherein the pH of the second waste residue is 7; S7. The second acidified leachate is filtered and concentrated 4 times to obtain a concentrate after two neutralization reactions; S8. The concentrated solution is subjected to lithium crystallization to obtain lithium carbonate.
6. The method for extracting lithium from lithium-rich waste slag from aluminum electrolysis according to claim 1, characterized in that: The concentration of the sodium carbonate is 210-240 g / l.