Iron-based gradient metal ceramic material and preparation method thereof
By preparing iron-based gradient cermet materials and combining the sol-gel method with calcination, a porous structure similar to human bone is formed, overcoming the shortcomings of existing materials and providing a high-strength, low-risk osteolysis bone and joint replacement material, thus improving patients' quality of life.
Patent Information
- Application Number
- CN202410993720.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
Existing artificial joint materials have drawbacks in the treatment of osteoarthritis, such as high risk of osteolysis, tissue inflammation, high cost, and high brittleness, making it difficult to combine the advantages of metals and ceramics.
Using iron-based gradient cermet materials, a porous structure with a gradient distribution is prepared by mixing the metal phase and ceramic phase in a certain proportion and mimicking the structure of human bone. Combined with the sol-gel method and calcination treatment, mechanical properties similar to human bone are formed.
This technology achieves high strength and low risk of osteolysis in artificial joint materials, improving comfort and quality of life, with mechanical properties close to those of human bone.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomedical implant materials, and in particular to an iron-based gradient metal ceramic material and a preparation method thereof. Background Art
[0002] Bone and joint diseases have become common and frequently-occurring diseases among the middle-aged and elderly population, which limits the basic mobility of patients and seriously affects the quality of life of patients. Artificial joint replacement is considered to be the best treatment for treating bone and joint diseases and restoring the function of damaged joints. The artificial joints used in the initial artificial joint replacement were metal joints. Metal joints have the advantages of high strength and hardness, excellent wear resistance, ability to withstand large loads, and low cost. However, metal joints also have the disadvantages of high risk of osteolysis, long-term use can cause inflammatory reactions in surrounding tissues, large weight, and poor comfort. For this reason, people began to develop ceramic joints, which have good biocompatibility and low risk of osteolysis. However, ceramic joints are expensive and brittle. If a fall, accident or improper joint installation occurs, the joint may break. The broken joint fragments may be embedded in the joint capsule, which is difficult to remove by surgery. It can be seen that both metal joints and ceramic joints have certain defects. Therefore, seeking a joint replacement material that combines the advantages of metal and ceramics to better relieve joint pain for patients with bone and joint diseases and improve the quality of life has become the research and development focus of this field. Summary of the invention
[0003] The purpose of the present invention is to provide an iron-based gradient metal ceramic material and a preparation method thereof. The iron-based gradient metal ceramic material provided by the present invention imitates the structure of human bones and can have mechanical properties similar to those of human bones. After being prepared into artificial joints, it can better relieve joint pain for patients with osteoarthritis and improve their quality of life.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] One of the technical solutions of the present invention:
[0006] An iron-based gradient metal ceramic material is formed by mixing a metal phase and a ceramic phase in a mass ratio of 2:1, and from the center to the periphery, the metal phase content gradually decreases from 100% to 5-10%, and the ceramic phase content gradually increases from 0% to 90-95%.
[0007] Further, the chemical composition of the metal phase is: Cr 17-19wt.%, Mo 2.5-3.0wt.%, Ni 13-15wt.%, Mn 1-2wt.%, N 0.01-0.1wt.%, Fe balance;
[0008] Preferably, the chemical composition of the metal phase is: Cr 18wt.%, Mo 2.75wt.%, Ni 14wt.%, Mn 1.5wt.%, N 0.05wt.%, and Fe as the balance.
[0009] Furthermore, the ceramic phase is zirconium oxide.
[0010] The second technical solution of the present invention:
[0011] The method for preparing the above-mentioned iron-based gradient metal ceramic material comprises the following steps:
[0012] 1) according to the chemical composition of the metal phase, using iron powder as a raw material, adding chromium, molybdenum, nickel, manganese and nitrogen elements to the iron powder to obtain a metal phase raw material premix, then adding the metal phase raw material premix to citric acid, mixing, and obtaining a metal phase mixed solution;
[0013] 2) performing gel treatment on the metal phase mixed solution obtained in step 1) to obtain a metal phase gel;
[0014] 3) Adding a ceramic phase to the metal phase gel obtained in step 2), and subjecting the mixture to centrifugation and calcination to obtain the iron-based gradient metal ceramic material.
[0015] Further, in step 1), the molar ratio of the metal phase raw material premix to citric acid is 1:(5-15);
[0016] Preferably, the molar ratio of the metal phase raw material premix to citric acid is 1:10;
[0017] Furthermore, in step 1), the mixing is to control the stirring speed to 500 rpm and stir for 30 to 60 minutes;
[0018] Preferably, the mixing is performed by controlling the stirring speed to 500 rpm and stirring for 45 min;
[0019] Furthermore, in step 2), before the metal phase mixed solution is subjected to gel treatment, the pH of the metal phase mixed solution is adjusted to 6 to 8 using an alkaline solution;
[0020] Furthermore, in step 2), the gel treatment is to heat the metal phase mixed solution to 100-130° C. under nitrogen protection, then control the stirring speed to 500 rpm, and continuously stir the metal phase mixed solution until the metal phase mixed solution becomes a gel state;
[0021] Preferably, the gel treatment is to heat the metal phase mixed solution to 110° C. under nitrogen protection, then control the stirring speed to 500 rpm, and continuously stir the metal phase mixed solution until the metal phase mixed solution becomes a gel state;
[0022] Furthermore, in step 3), the centrifugal speed is 500-1500 rpm, and the time is 3-7 min;
[0023] Preferably, the centrifugal speed is 1000 rpm and the time is 5 min;
[0024] Furthermore, in step 3), the gel needs to be dried before calcination;
[0025] Furthermore, the drying is performed at 60 to 80° C. for 5 to 10 minutes;
[0026] Furthermore, in step 3), the calcination is performed at 500-600° C. for 20-30 min.
[0027] Preferably, the calcination is carried out at 550° C. for 25 min.
[0028] The third technical solution of the present invention:
[0029] Application of the above-mentioned iron-based gradient metal ceramic materials in biomedical implants.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] Human bones are tough on the outside and porous on the inside. The iron-based gradient metal ceramic material provided by the present invention imitates the structure of human bones and has mechanical properties similar to those of human bones. Its Mohs hardness can reach 5.5 and its average tensile strength can reach 138.32×10 6 N / m 2 The average compressive strength can reach 189.79×10 6 N / m 2 ;
[0032] The iron-based gradient metal ceramic material provided by the present invention can better relieve joint pain for patients with osteoarthritis and improve their quality of life after being prepared into artificial joints. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] In the following examples, the raw materials are commercially available unless otherwise specified.
[0035] In the following embodiments, a method for preparing an iron-based gradient metal ceramic material comprises the following steps:
[0036] 1) according to the chemical composition of the metal phase, Cr 17-19wt.%, Mo 2.5-3.0wt.%, Ni 13-15wt.%, Mn 1-2wt.%, N 0.01-0.1wt.%, Fe balance, using iron powder as raw material, adding chromium, molybdenum, nickel, manganese and nitrogen elements into the iron powder to obtain a metal phase raw material premix;
[0037] 2) adding the metal phase raw material premix obtained in step 1) to citric acid at a molar ratio of the metal phase raw material premix to citric acid of 1:(5-15), controlling the stirring speed to 500 rpm, stirring for 30-60 minutes, and obtaining a metal phase mixed solution;
[0038] 3) adjusting the pH of the metal phase mixed solution obtained in step 2) to 6-8 using a 0.1 M sodium hydroxide solution, and then subjecting the metal phase mixed solution obtained in step 2) to a gel treatment to obtain a metal phase gel;
[0039] The gel treatment is to heat the metal phase mixed solution to 100-130° C. under nitrogen protection, then control the stirring speed to 500 rpm, and continuously stir the metal phase mixed solution until the metal phase mixed solution becomes a gel state;
[0040] 4) adding the ceramic phase to the metal phase gel obtained in step 3) at a mass ratio of the metal phase to the ceramic phase of 2:1, controlling the stirring speed to 200 rpm, stirring for 5 to 10 minutes, and obtaining a mixed gel;
[0041] Wherein, the ceramic phase is zirconium oxide;
[0042] 5) transferring the mixed gel obtained in step 4) to a centrifuge, controlling the centrifugal speed to be 500 to 1500 rpm, and centrifuging the mixed gel for 3 to 7 minutes to obtain a gradient metal ceramic gel;
[0043] 6) Drying the gradient metal ceramic gel obtained in step 5) at 60-80° C. for 5-10 min, and then calcining at 500-600° C. for 20-30 min to obtain the iron-based gradient metal ceramic material.
[0044] Example 1
[0045] An iron-based gradient metal ceramic material
[0046] 1) according to the chemical composition of the metal phase: Cr 18wt.%, Mo 2.75wt.%, Ni 14wt.%, Mn 1.5wt.%, N 0.05wt.%, Fe balance, using iron powder as raw material, adding chromium, molybdenum, nickel, manganese and nitrogen elements into the iron powder to obtain a metal phase raw material premix;
[0047] 2) adding the metal phase raw material premix obtained in step 1) to citric acid at a molar ratio of the metal phase raw material premix to citric acid of 1:10, controlling the stirring speed to 500 rpm, stirring for 45 minutes, and obtaining a metal phase mixed solution;
[0048] 3) adjusting the pH of the metal phase mixed solution obtained in step 2) to 7 using a 0.1 M sodium hydroxide solution, and then performing a gel treatment on the metal phase mixed solution obtained in step 2) to obtain a metal phase gel;
[0049] The gel treatment is to heat the metal phase mixed solution to 110° C. under nitrogen protection, then control the stirring speed to 500 rpm, and continuously stir the metal phase mixed solution until the metal phase mixed solution becomes a gel state;
[0050] 4) adding the ceramic phase to the metal phase gel obtained in step 3) at a mass ratio of the metal phase to the ceramic phase of 2:1, controlling the stirring speed to 200 rpm, stirring for 8 minutes, and obtaining a mixed gel;
[0051] Wherein, the ceramic phase is zirconium oxide;
[0052] 5) transferring the mixed gel obtained in step 4) into a centrifuge, controlling the centrifugal speed to 900 rpm, and centrifuging the mixed gel for 5 minutes to obtain a gradient metal ceramic gel;
[0053] 6) The gradient metal ceramic gel obtained in step 5) is dried at 70° C. for 8 min, and then calcined at 550° C. for 25 min to obtain the iron-based gradient metal ceramic material.
[0054] The iron-based gradient metal ceramic material prepared in Example 1 of the present invention was subjected to SEM electron microscope scanning and cross-sectional SEM electron microscope scanning; from the SEM electron microscope scanning results, it can be seen that the iron-based gradient metal ceramic material prepared in Example 1 of the present invention is in a relatively regular spherical shape; from the cross-sectional SEM electron microscope scanning results, it can be seen that the metal phase and the ceramic phase of the iron-based gradient metal ceramic material prepared in Example 1 of the present invention are distributed in a gradient manner, specifically, from the center position of the sphere to the surrounding area, the metal phase content gradually decreases from 100% to 5%, and the ceramic phase content gradually increases from 0% to 95%; in addition, from the cross-sectional SEM electron microscope scanning results, it can also be known that the metal phase in the iron-based gradient metal ceramic material prepared in Example 1 of the present invention exists in the form of a porous structure similar to the internal structure of human bones.
[0055] Example 2
[0056] An iron-based gradient metal ceramic material
[0057] 1) according to the chemical composition of the metal phase, Cr 17wt.%, Mo 2.5wt.%, Ni 13wt.%, Mn 1wt.%, N0.01wt.%, Fe balance, using iron powder as raw material, adding chromium, molybdenum, nickel, manganese and nitrogen elements into the iron powder to obtain a metal phase raw material premix;
[0058] 2) adding the metal phase raw material premix obtained in step 1) to citric acid at a molar ratio of the metal phase raw material premix to citric acid of 1:5, controlling the stirring speed to 500 rpm, stirring for 30 minutes, and obtaining a metal phase mixed solution;
[0059] 3) adjusting the pH of the metal phase mixed solution obtained in step 2) to 7 using a 0.1 M sodium hydroxide solution, and then performing a gel treatment on the metal phase mixed solution obtained in step 2) to obtain a metal phase gel;
[0060] The gel treatment is to heat the metal phase mixed solution to 100° C. under nitrogen protection, then control the stirring speed to 500 rpm, and continuously stir the metal phase mixed solution until the metal phase mixed solution becomes a gel state;
[0061] 4) adding the ceramic phase to the metal phase gel obtained in step 3) at a mass ratio of the metal phase to the ceramic phase of 2:1, controlling the stirring speed to 200 rpm, stirring for 5 minutes, and obtaining a mixed gel;
[0062] Wherein, the ceramic phase is zirconium oxide;
[0063] 5) transferring the mixed gel obtained in step 4) into a centrifuge, controlling the centrifugal speed to 500 rpm, and centrifuging the mixed gel for 3 minutes to obtain a gradient metal ceramic gel;
[0064] 6) The gradient metal ceramic gel obtained in step 5) is dried at 60° C. for 5 min, and then calcined at 500° C. for 20 min to obtain the iron-based gradient metal ceramic material.
[0065] The iron-based gradient metal ceramic material prepared in Example 2 of the present invention was subjected to SEM electron microscope scanning and cross-sectional SEM electron microscope scanning; it can be seen from the SEM electron microscope scanning results that the iron-based gradient metal ceramic material prepared in Example 2 of the present invention is in a relatively regular spherical shape; it can be seen from the cross-sectional SEM electron microscope scanning results that the metal phase and the ceramic phase of the iron-based gradient metal ceramic material prepared in Example 2 of the present invention are distributed in a gradient manner, specifically, from the center position of the sphere to the surrounding area, the metal phase content gradually decreases from 100% to 8%, and the ceramic phase content gradually increases from 0% to 92%; in addition, it can also be seen from the cross-sectional SEM electron microscope scanning results that the metal phase in the iron-based gradient metal ceramic material prepared in Example 2 of the present invention exists in the form of a porous structure similar to the internal structure of human bones.
[0066] Example 3
[0067] An iron-based gradient metal ceramic material
[0068] 1) according to the chemical composition of the metal phase, Cr 19wt.%, Mo 3.0wt.%, Ni 15wt.%, Mn 2wt.%, N0.1wt.%, Fe balance, using iron powder as raw material, adding chromium, molybdenum, nickel, manganese and nitrogen elements into the iron powder to obtain a metal phase raw material premix;
[0069] 2) adding the metal phase raw material premix obtained in step 1) to citric acid at a molar ratio of the metal phase raw material premix to citric acid of 1:10, controlling the stirring speed to 500 rpm, stirring for 60 minutes, and obtaining a metal phase mixed solution;
[0070] 3) adjusting the pH of the metal phase mixed solution obtained in step 2) to 7 using a 0.1 M sodium hydroxide solution, and then performing a gel treatment on the metal phase mixed solution obtained in step 2) to obtain a metal phase gel;
[0071] The gel treatment is to heat the metal phase mixed solution to 130° C. under nitrogen protection, then control the stirring speed to 500 rpm, and continuously stir the metal phase mixed solution until the metal phase mixed solution becomes a gel state;
[0072] 4) adding the ceramic phase to the metal phase gel obtained in step 3) at a mass ratio of the metal phase to the ceramic phase of 2:1, controlling the stirring speed to 200 rpm, stirring for 10 minutes, and obtaining a mixed gel;
[0073] Wherein, the ceramic phase is zirconium oxide;
[0074] 5) transferring the mixed gel obtained in step 4) into a centrifuge, controlling the centrifugal speed to 1500 rpm, and centrifuging the mixed gel for 7 minutes to obtain a gradient metal ceramic gel;
[0075] 6) The gradient metal ceramic gel obtained in step 5) is dried at 80° C. for 10 min, and then calcined at 600° C. for 30 min to obtain the iron-based gradient metal ceramic material.
[0076] The iron-based gradient metal ceramic material prepared in Example 3 of the present invention was subjected to SEM electron microscope scanning and cross-sectional SEM electron microscope scanning; it can be seen from the SEM electron microscope scanning results that the iron-based gradient metal ceramic material prepared in Example 3 of the present invention is in a relatively regular spherical shape; it can be seen from the cross-sectional SEM electron microscope scanning results that the metal phase and the ceramic phase of the iron-based gradient metal ceramic material prepared in Example 3 of the present invention are distributed in a gradient manner, specifically, from the center position of the sphere to the surrounding area, the metal phase content gradually decreases from 100% to 10%, and the ceramic phase content gradually increases from 0% to 90%; in addition, it can also be seen from the cross-sectional SEM electron microscope scanning results that the metal phase in the iron-based gradient metal ceramic material prepared in Example 3 of the present invention exists in the form of a porous structure similar to the internal structure of human bones.
[0077] Comparative Example 1
[0078] An iron-based gradient metal ceramic material
[0079] The same as Example 1, the only difference is that in step 1, the addition of chromium element is omitted.
[0080] Comparative Example 2
[0081] An iron-based gradient metal ceramic material
[0082] The same as Example 1, the only difference is that in step 1, the addition of molybdenum element is omitted.
[0083] Comparative Example 3
[0084] An iron-based gradient metal ceramic material
[0085] The same as Example 1, the only difference is that in step 1, the addition of nickel element is omitted.
[0086] Comparative Example 4
[0087] An iron-based gradient metal ceramic material
[0088] The same as Example 1, the only difference is that in step 1, the addition of manganese element is omitted.
[0089] Comparative Example 5
[0090] An iron-based gradient metal ceramic material
[0091] The same as Example 1, the only difference is that in step 1, the addition of nitrogen is omitted.
[0092] Comparative Example 6
[0093] An iron-based gradient metal ceramic material
[0094] Same as Example 1, except that in step 2), the molar ratio of the metal phase raw material premix to citric acid is 1:2.
[0095] Comparative Example 7
[0096] An iron-based gradient metal ceramic material
[0097] Same as Example 1, except that in step 2), the molar ratio of the metal phase raw material premix to citric acid is 1:20.
[0098] Comparative Example 8
[0099] An iron-based gradient metal ceramic material
[0100] Same as Example 1, except that in step 5), the centrifugal speed is 300 rpm.
[0101] Comparative Example 9
[0102] An iron-based gradient metal ceramic material
[0103] Same as Example 1, except that in step 5), the centrifugal speed is 2000 rpm.
[0104] Comparative Example 10
[0105] An iron-based gradient metal ceramic material
[0106] Same as Example 1, except that in step 5), the centrifugation time is 1 min.
[0107] Comparative Example 11
[0108] An iron-based gradient metal ceramic material
[0109] Same as Example 1, except that in step 5), the centrifugation time is 10 min.
[0110] Comparative Example 12
[0111] An iron-based gradient metal ceramic material
[0112] Same as Example 1, except that in step 6), the calcination temperature is 400°C.
[0113] Comparative Example 13
[0114] An iron-based gradient metal ceramic material
[0115] Same as Example 1, except that in step 6), the calcination temperature is 700°C.
[0116] Comparative Example 14
[0117] An iron-based gradient metal ceramic material
[0118] Same as Example 1, except that in step 6), the calcination time is 10 min.
[0119] Comparative Example 15
[0120] An iron-based gradient metal ceramic material
[0121] Same as Example 1, except that in step 6), the calcination time is 40 min.
[0122] Effect verification
[0123] Mechanical properties of the iron-based gradient metal ceramic materials prepared in Examples 1 to 3 and Comparative Examples 1 to 15 were tested;
[0124] The mechanical properties test method is as follows: the iron-based gradient metal ceramic material is divided into four equal parts along the longitudinal direction, and a sample is taken at the center of each part. The sampling size is 0.5 cm × 0.5 cm × 0.5 cm. The sample is tested for Mohs hardness, tensile strength and compressive strength. The average value of the four samples is taken as the mechanical properties test result of the iron-based gradient metal ceramic material. The test is carried out in parallel three times.
[0125] The mechanical properties test results are shown in Table 1;
[0126] Table 1 Mechanical properties test results
[0127]
[0128] It can be seen from the data in Table 1 that the average Mohs hardness of the iron-based gradient metal ceramic material prepared by the present invention can reach 5.5, and the average tensile strength can reach 138.32×10 6 N / m 2 The average compressive strength can reach 189.79×10 6 N / m 2 , has mechanical properties similar to those of human bones;
[0129] The reason why the iron-based gradient metal ceramic material prepared by the present invention can have mechanical properties similar to those of human bones is that the present invention adopts a sol-gel method to prepare the metal gel, and combines calcination treatment to prepare the metal ceramic material, so that a microporous structure similar to the structure of human bones is formed inside the metal ceramic material, thereby achieving better mechanical properties;
[0130] It can be seen from Comparative Examples 1 to 5 that if the addition of chromium, molybdenum, nickel, manganese or nitrogen is omitted during the preparation of the iron-based gradient metal ceramic material, the Mohs hardness, tensile strength and compressive strength of the iron-based gradient metal ceramic material will be reduced to varying degrees; the reason is that there is a synergistic effect between the chromium, molybdenum, nickel, manganese, nitrogen and iron elements added in the present invention, and omitting any one of the elements will result in the subsequent sol-gel method for preparing an internal structure with a microporous structure, and the microporous structure cannot be effectively formed, thereby reducing the mechanical properties of the iron-based gradient metal ceramic material;
[0131] It can be seen from Comparative Examples 6 to 7 that when preparing a metal phase mixed solution, the amount of citric acid added will also have a significant effect on the final mechanical properties. Specifically, the purpose of adding citric acid in the present invention is to form an acidic environment to complex metal ions. Too little addition of citric acid will result in the metal ions being unable to be effectively complexed, thereby resulting in the inability to achieve subsequent gel formation. Excessive addition of citric acid will result in excessive addition of alkaline solution during subsequent neutralization of the acidity, causing citric acid to remain in the system in the form of citrate. When calcining to form a microporous structure, the citrate will cover the microporous structure, thereby being detrimental to the mechanical properties of the iron-based gradient metal ceramic material.
[0132] It can be seen from Comparative Examples 8 to 11 that when the mixed gel is centrifuged, the rotation speed and time of the centrifugation will affect the mechanical properties of the finally prepared iron-based gradient metal ceramic material; specifically, too low a centrifugal speed and too short a centrifugal time will make it impossible for the ceramic phase to be effectively gradient dispersed, so that the ceramic phase is more evenly dispersed in the metal gel, thereby resulting in a decrease in mechanical properties; while too high a centrifugal speed and too long a centrifugal time will cause the ceramic phase to be distributed in large quantities around due to the strong centrifugal force, and will also damage the metal gel, thereby affecting the mechanical properties of the gradient metal ceramic material;
[0133] It can be seen from Comparative Examples 12 to 15 that when the gradient metal ceramic gel is calcined, the calcination time and temperature will affect the mechanical properties of the finally prepared iron-based gradient metal ceramic material; specifically, if the calcination time is too short or the temperature is too low, micropores cannot be generated in the metal phase, thereby reducing the mechanical properties of the gradient metal ceramic material. If the calcination time is too long or the temperature is too high, the micropore structure that has been generated will be destroyed, thereby reducing the mechanical properties.
[0134] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. An iron-based gradient metal ceramic material, It is characterized in that The iron-based gradient metal ceramic material is formed by mixing a metal phase and a ceramic phase in a mass ratio of 2:1, and from the center to the periphery, the metal phase content gradually decreases from 100% to 5-10%, and the ceramic phase content gradually increases from 0% to 90-95%.
2. The iron-based gradient metal ceramic material according to claim 1, It is characterized in that The chemical composition of the metal phase is: Cr 17-19wt.%, Mo 2.5-3.0wt.%, Ni 13-15wt.%, Mn 1-2wt.%, N 0.01-0.1wt.%, and Fe as the balance.
3. The iron-based gradient metal ceramic material according to claim 1, It is characterized in that The ceramic phase is zirconium oxide.
4. A method for preparing the iron-based gradient metal ceramic material as claimed in claims 1 to 3, It is characterized in that The following steps are involved: 1) according to the chemical composition of the metal phase, using iron powder as a raw material, adding chromium, molybdenum, nickel, manganese and nitrogen elements to the iron powder to obtain a metal phase raw material premix, then adding the metal phase raw material premix to citric acid, mixing, and obtaining a metal phase mixed solution; 2) performing gel treatment on the metal phase mixed solution obtained in step 1) to obtain a metal phase gel; 3) Adding a ceramic phase to the metal phase gel obtained in step 2), and subjecting the mixture to centrifugation and calcination to obtain the iron-based gradient metal ceramic material.
5. The preparation method according to claim 4, It is characterized in that In step 1), the molar ratio of the metal phase raw material premix to citric acid is 1:(5-15); the mixing is performed by controlling the stirring speed to 500 rpm and stirring for 30-60 minutes.
6. The preparation method according to claim 4, It is characterized in that In step 2), before the metal phase mixed solution is subjected to gel treatment, the pH of the metal phase mixed solution needs to be adjusted to 6-8 using an alkaline solution.
7. The preparation method according to claim 4, It is characterized in that In step 2), the gel treatment is to heat the metal phase mixed solution to 100-130° C. under nitrogen protection, then control the stirring speed to 500 rpm, and continuously stir the metal phase mixed solution until the metal phase mixed solution becomes a gel state.
8. The preparation method according to claim 4, It is characterized in that In step 3), the centrifugal speed is 500-1500 rpm, and the time is 3-7 min; the calcination is performed at 500-600° C. for 20-30 min.
9. The preparation method according to claim 4, It is characterized in that In step 3), the gel needs to be dried before calcination.
10. Use of the iron-based gradient metal ceramic material as claimed in claims 1 to 3 in biomedical implants.