Preparation method of carbon-nitrogen-doped nickel-molybdenum-based hydrogen evolution cathode catalyst
The carbon-nitrogen-doped nickel-molybdenum-based hydrogen evolution cathode catalyst was prepared through co-precipitation reaction and high-temperature heat treatment, which solved the problems of high temperature and high pressure and uneven doping during the preparation of nickel-molybdenum precursor, and achieved low-cost and high-stability cathode catalyst preparation , suitable for electrolyzing water to produce hydrogen.
Patent Information
- Application Number
- CN202310516153.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing electrolytic hydrogen production technology, the preparation process of nickel-molybdenum precursor requires high temperature and high pressure, and the subsequent nitriding, phosphating or vulcanization is uneven, resulting in high cost and insufficient stability of the cathode catalyst.
The precursor is prepared by co-precipitation reaction of nitrogen-containing organic matter and nickel-molybdenum oxide, and in-situ doped by high-temperature heat treatment to form a carbon-nitrogen-doped nickel-molybdenum-based hydrogen evolution cathode catalyst, simplifying the preparation process and achieving uniform doping of carbon-nitrogen.
It is easy to prepare a carbon-nitrogen-doped nickel-molybdenum-based hydrogen evolution cathode catalyst under normal temperature and pressure, with low overpotential and high stability, and is suitable for use in proton exchange membrane electrolysis and hydrogen production of alkaline water electrolysis.
Smart Images

Figure CN118932388A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogen production by electrolysis of water, and in particular to a method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst. Background Art
[0002] Fossil energy, which currently occupies the main energy structure, has problems such as non-renewable and serious pollution. At the same time, renewable resources such as wind energy and solar energy are greatly affected by factors such as climate and geographical environment, and their direct use has problems of intermittent discontinuity and instability. Hydrogen, which has the advantages of high energy density, zero pollution and renewability, is considered to be an excellent medium for storing large-scale renewable electricity (photovoltaic, wind power) in the future. The current methods of hydrogen production include coal-to-hydrogen, natural gas-to-hydrogen, biomass-to-hydrogen, and water electrolysis. Among them, the use of renewable energy to electrolyze water to produce hydrogen has the advantages of simple raw materials, environmental protection, high hydrogen production efficiency, and high purity. It is also called "green hydrogen."
[0003] The water electrolysis reaction consists of two electrode reactions, namely the cathode hydrogen evolution reaction (HER) and the anode oxygen evolution reaction (OER). Currently, the HER catalysts for commercial proton exchange membrane water electrolysis are mostly Pt, Pd, Ru and their alloy materials. These precious metal catalysts have small reserves and high costs, which limits their development and industrial application. In alkaline water electrolysis for hydrogen production, non-precious metal nickel alloys can be used as hydrogen evolution cathode catalysts, such as nickel-molybdenum, nickel-cobalt, nickel-copper, nickel-aluminum, nickel-zinc and other catalysts, which greatly reduces the cost of cathode catalysts, but there are disadvantages such as high overpotential, insufficient stability or complex preparation process. Taking the hydrothermal method for preparing the precursor of the nickel-based hydrogen evolution cathode as an example, it is often necessary to use a high-pressure reactor for high-temperature and high-pressure hydrothermal reaction preparation, which is energy-intensive and dangerous. For example, CN115404493 A prepares a β-phase nickel hydroxide / nickel phosphide heterojunction for electrocatalytic hydrogen evolution, wherein nickel foam is used as a substrate, placed in a mixed solution of nickel nitrate, urea, and ammonium fluoride, and reacted in a reactor at 110°C to 130°C for 6 to 10 hours to prepare a β-phase nickel hydroxide precursor, and after drying, sodium hypophosphite and the β-phase nickel hydroxide precursor are placed upstream and downstream in a high-temperature tube furnace filled with inert gas, reacted at 300°C to 350°C for 1 to 2 hours, and high-temperature phosphating is performed to prepare a heterostructure nanoarray composed of β-phase nickel hydroxide nanosheets and nickel phosphide nanoparticles. CN111617780A discloses growing a nickel-molybdenum precursor on nickel foam through a high-temperature and high-pressure reaction in a hydrothermal reactor, and then preparing a self-supporting microrod array structure of nitrogen-doped nickel-molybdenum-based composite sulfide through high-temperature sulfidation and nitridation.
[0004] In the above-reported work, it is common that the preparation of the precursor requires a high temperature and high pressure process, and the subsequent nitridation, phosphation or sulfurization doping leads to uneven nitridation, phosphation or sulfurization due to uneven contact between the nitrogen source, phosphorus source, sulfur source and the precursor. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst. In view of the harsh conditions of the nickel-molybdenum precursor preparation process and the uneven subsequent nitridation doping, a method for preparing a nickel-molybdenum-based hydrogen evolution cathode catalyst by simply preparing a nitrogen-containing organic in-situ doped nickel-molybdenum precursor is proposed to achieve in-situ uniform carbon-nitrogen doping. Among them, carbon and nitrogen are obtained by pyrolysis of nitrogen-containing organic matter, and nickel-molybdenum-based components are obtained by in-situ reduction, nitridation, and carbonization of nickel-molybdenum oxide to obtain nickel-molybdenum metal and metal nitrides and carbides. In the precursor preparation stage, the two precursors of nitrogen-containing organic matter and nickel-molybdenum oxide are compounded by co-precipitation reaction, which helps to form a nickel-molybdenum-based hydrogen evolution cathode composite material doped with carbon and nitrogen in situ during the heat treatment process.
[0006] The present invention is achieved by adopting the following technical solutions:
[0007] (1) A coprecipitation reaction occurs by rapidly mixing a nitrogen-containing organic substance, a nickel salt solution and a molybdenum salt solution under stirring. The nitrogen-containing organic substance is one or two of melamine, dicyandiamide, urea and polypyrrole; the nickel salt is one or two of nickel chloride, nickel nitrate, nickel sulfate or nickel acetate; the molybdenum salt is one or two of ammonium molybdate and sodium molybdate; the molar ratio of the nitrogen-containing organic substance, the nickel salt and the molybdenum salt is in the range of 0.1 to 3:0.5 to 5:1; the two solutions refer to a nitrogen-containing organic substance-nickel salt solution and a molybdenum salt solution, or a nitrogen-containing organic substance-molybdenum salt solution and a nickel salt solution; the coprecipitation reaction temperature ranges from 0°C to room temperature during rapid mixing.
[0008] (2) The precipitate is freeze-dried at low temperature, the soluble salt is washed, and then dried to obtain a complex of nitrogen-containing organic matter and nickel-molybdenum oxide. The freeze-drying is to firstly cool rapidly with liquid nitrogen, and then freeze-dry the frozen solid in the vacuum atmosphere of a freeze dryer; the washing is to use ethanol or water as a solvent to wash away the inorganic salt formed by the molybdenum salt cation and the nickel salt anion.
[0009] (3) Then the composite of the nitrogen-containing organic matter and the nickel-molybdenum oxide is placed in an atmosphere furnace into which hydrogen and an inert gas protective gas are introduced, and the nitrogen-containing organic matter is pyrolyzed, carbonized, and the nickel-molybdenum oxide is in situ reduced and nitrided by high-temperature heat treatment, so as to finally prepare a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst. The volume percentage of the hydrogen gas is in the range of 2-15%, and the inert gas is one of nitrogen and argon; the high-temperature heat treatment temperature is 400-700°C, the heating rate is 1-10°C / min, and the high-temperature constant temperature stage heat treatment time is 0.5-6h; the pyrolysis of the nitrogen-containing organic matter and the in-situ reduction and nitridation of the nickel-molybdenum oxide are due to the coprecipitation process of step (1) in which the nitrogen-containing organic matter is doped in the precursor of the nickel-molybdenum oxide.
[0010] Beneficial effects of the present invention: The present invention provides a method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst, the preparation process is simple and controllable, and a precipitation reaction is carried out in a normal temperature and pressure environment to quickly prepare nitrogen-containing organic matter and NiMoO4 precursor. Through high-temperature heat treatment, the nitrogen-containing organic matter is pyrolyzed to form a carbon-nitrogen component doping, and nickel-molybdenum metal and metal nitrides and carbides (nickel-molybdenum-based components) are formed through in-situ reduction, nitridation, and carbonization of nickel-molybdenum oxide. Thanks to the pre-compounding of the two components of the precursor, the successful preparation of a nickel-molybdenum-based hydrogen evolution cathode catalyst uniformly doped with carbon and nitrogen is achieved.
[0011] The present invention provides a method for preparing a carbon-nitrogen-doped nickel-molybdenum-based hydrogen evolution cathode catalyst, wherein the overpotential of the prepared cathode catalyst is less than 120mV@100mA / cm 2 , and the overpotential increase does not exceed 10mV after 1000h. It has the dual advantages of high activity and stability, and is an excellent cathode catalytic material suitable for proton exchange membrane water electrolysis and alkaline water electrolysis to produce hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 This is a SEM picture of the composite of nitrogen-containing organic matter and nickel-molybdenum oxide obtained by the preparation method Example 1 of the present invention;
[0013] Figure 2 The SEM image of the carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst obtained after step (1) of the preparation method of the present invention; DETAILED DESCRIPTION
[0014] The present invention will be further described in detail below with reference to the embodiments.
[0015] Example 1
[0016] Prepare 100 mL of a mixed solution of melamine and nickel nitrate at a substance amount ratio of 0.2:1, and prepare 100 mL of a 1 mol / L sodium molybdate solution. Place the melamine-nickel salt mixture on a constant temperature stirring table, control the reaction temperature to 25°C, and quickly pour the molybdenum salt solution into the melamine-nickel salt mixture under stirring for a coprecipitation reaction for 3 minutes. The suspension after the coprecipitation reaction is frozen with liquid nitrogen, and then freeze-dried in a freeze dryer for 24 hours. After washing the freeze-dried product with an appropriate amount of anhydrous ethanol, the material is placed in a 70°C vacuum oven and dried for 12 hours to obtain a complex of nitrogen-containing organic matter and nickel-molybdenum oxide, which is used as a precursor. The SEM of the complex is as follows Figure 1 As shown, it is composed of uniformly distributed nanoparticles.
[0017] Take 2g of the above precursor, place it in a crucible porcelain boat, and calcine it at high temperature in a reducing atmosphere of Ar and H2, with a hydrogen content of 10%, a heating rate of 5℃ / min, a heat treatment temperature of 550℃, and a constant temperature reaction for 1h to obtain a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst (CN / NiMo-550). Figure 2 The SEM image of the catalyst shows that uniformly distributed short carbon nanotubes appear between the nanoparticles. Combined with the introduction of nitrogen-containing organic matter in the present invention, the carbon nanotubes are nitrogen-doped carbon materials, indicating that a carbon-nitrogen-doped nickel-molybdenum-based material is formed.
[0018] Example 2
[0019] Prepare 100 mL of a mixture of dicyandiamide and nickel chloride at a mass ratio of 0.3:1, and prepare 100 mL of a 1.2 mol / L sodium molybdate solution. Place the dicyandiamide-nickel salt mixture on a constant temperature stirring table, control the reaction temperature to 5°C, and quickly pour the molybdenum salt solution into the dicyandiamide-nickel salt mixture under stirring for a coprecipitation reaction for 3 minutes. The suspension after the coprecipitation reaction is frozen with liquid nitrogen, and then placed in a freeze dryer for freeze drying for 24 hours. After washing the freeze-dried product with an appropriate amount of anhydrous ethanol, place the material in a 70°C vacuum oven and dry it for 12 hours to obtain a complex of nitrogen-containing organic matter and nickel-molybdenum oxide as a precursor.
[0020] Take 2g of the above-mentioned precursor, place it in a crucible porcelain boat, and calcine it at high temperature in a reducing atmosphere of Ar and H2, with a hydrogen content of 10%, a heating rate of 5℃ / min, a heat treatment temperature of 650℃, and a constant temperature reaction for 1h to obtain a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst (CN / NiMo-650).
[0021] Example 3
[0022] In the comparative example, no nitrogen-containing organic matter was added. Nickel chloride was prepared into a mixed solution of 100 mL according to the amount of substance of 0:1, and 100 mL of 1.2 mol / L sodium molybdate solution was also prepared. The nickel salt solution was placed on a constant temperature stirring table, and the reaction temperature was controlled to 5°C. The molybdenum salt solution was quickly poured into the nickel salt solution under stirring for a co-precipitation reaction, and the reaction time was 3 minutes. The suspension after the co-precipitation reaction was frozen with liquid nitrogen, and then placed in a freeze dryer for freeze drying for 24 hours. After washing the freeze-dried product with an appropriate amount of anhydrous ethanol, the material was placed in a 70°C vacuum oven and dried for 12 hours to obtain nickel-molybdenum oxide as a precursor.
[0023] Take 2g of the above-mentioned precursor, place it in a crucible porcelain boat, and calcine it at high temperature in a reducing atmosphere of Ar and H2, with a hydrogen content of 10%, a heating rate of 5℃ / min, a heat treatment temperature of 650℃, and a constant temperature reaction for 1h to obtain a carbon-free and nitrogen-doped nickel-molybdenum-based hydrogen evolution cathode catalyst (NiMo-650).
[0024] Electrochemical testing,
[0025] The CN / NiMo-550, CN / NiMo-650, and NiMo-650 hydrogen evolution catalyst-coated nickel foam prepared in the examples were used as working electrodes. 2 Three-electrode hydrogen evolution reaction test was carried out at room temperature with graphite as the counter electrode, saturated calomel as the reference electrode and 1 M KOH as the electrolyte.
[0026] The test results show that during the hydrogen evolution reaction, CN / NiMo-550, CN / NiMo-650 and NiMo-650 have a high -2 , tested for 1000h, wherein the overpotentials of hydrogen evolution at 1000h were 110.5mV, 117mV, and 235mV, respectively, wherein the overpotentials of the first two increased by no more than 10mV compared with the first hour, while the overpotential of NiMo-650 without carbon and nitrogen doping increased by more than 100mV. This indicates that the carbon and nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst prepared by the present invention has the significant advantages of high activity, especially high stability, and is an excellent cathode catalyst suitable for hydrogen production by water electrolysis.
[0027] The above are only preferred embodiments of the present invention. The protection scope of the present invention is not limited to the above embodiments. Various process schemes that are not substantially different from the concept of the present invention are within the protection scope of the present invention.
Claims
1. A method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst, characterized in that: The following steps are involved: (1) rapidly mixing the nitrogen-containing organic matter, the nickel salt solution and the molybdenum salt solution under stirring to cause a coprecipitation reaction; (2) subjecting the precipitate to low-temperature freeze-drying, washing soluble salts, and drying to obtain a complex of nitrogen-containing organic matter and nickel-molybdenum oxide; (3) placing the complex in a high-temperature furnace into which hydrogen and inert gas are introduced, and subjecting the complex to high-temperature heat treatment to thermal decomposition of the nitrogen-containing organic matter and in-situ reduction and nitridation of the nickel-molybdenum oxide, thereby finally preparing a carbon-nitrogen-doped nickel-molybdenum-based hydrogen evolution cathode catalyst.
2. The method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst according to claim 1, characterized in that: The nitrogen-containing organic matter in step (1) is one or two of melamine, dicyandiamide, urea, and polypyrrole; the nickel salt is one or two of nickel chloride, nickel nitrate, nickel sulfate, or nickel acetate; the molybdenum salt is one or two of ammonium molybdate and sodium molybdate; and the molar ratio of the nitrogen-containing organic matter, the nickel salt, and the molybdenum salt is in the range of 0.1 to 3:0.5 to 5:
1.
3. The method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst according to claim 1, characterized in that: The two solutions described in step (1) are a nitrogen-containing organic matter-nickel salt solution and a molybdenum salt solution, or a nitrogen-containing organic matter-molybdenum salt solution and a nickel salt solution. The rapid mixing is a coprecipitation reaction at a temperature of 0°C to room temperature.
4. The method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst according to claim 1, characterized in that: The freeze drying in step (2) is to firstly rapidly cool the solid by liquid nitrogen and then freeze dry the solid in the vacuum atmosphere of a freeze dryer.
5. The method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst according to claim 1, characterized in that: The washing described in step (2) is to use ethanol or water as a solvent to wash away the inorganic salt formed by the molybdenum salt cation and the nickel salt anion.
6. The method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst according to claim 1, characterized in that: The volume percentage of hydrogen described in step (3) is in the range of 2 to 15%; the inert gas is one of nitrogen and argon; the high-temperature heat treatment temperature is 400 to 700°C, the heating rate is 1 to 10°C / min, and the high-temperature constant temperature stage heat treatment time is 0.5 to 6h.
7. The method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst according to claim 1, characterized in that: The pyrolysis of nitrogen-containing organic matter and the in-situ reduction and nitridation of nickel-molybdenum oxide described in step (3) utilize the coprecipitation process of step (1) to dope the nitrogen-containing organic matter into the precursor of nickel-molybdenum oxide.
8. The method for preparing a carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst according to claim 1, characterized in that: The carbon-nitrogen doped nickel-molybdenum-based hydrogen evolution cathode catalyst has the dual advantages of high activity and high stability, and is an excellent cathode catalyst suitable for hydrogen production by proton exchange membrane water electrolysis and alkaline water electrolysis.
Citation Information
Cited By
Synthesis method of nickel-based non-noble metal catalyst, hydrogen electrode and preparation method thereof, and nickel-hydrogen secondary battery
CN119695181A
Preparation method of non-noble metal doped nickel-molybdenum-nitrogen-carbon multi-element hydrogen evolution catalyst
CN120060907A