CoFe-coated NC core-shell structure catalyst, preparation method and performance prediction method

Through the CoFe@NC core-shell structure catalyst, the synergistic effect of conductive CoFe alloy core and nitrogen-codoped carbon shell is used to solve the problems of corrosion and low efficiency caused by chloride ions in seawater electrolysis, and high OER activity and long-term stability are achieved , suitable for industrial seawater electrolysis.

CN118932398APending Publication Date: 2024-11-12HUAIYIN TEACHERS COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411013632.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In seawater electrolytic hydrogen production technology, the presence of chloride ions leads to side reactions and corrosion problems, reducing the durability of the anode catalyst and the efficiency of OER, and achieving high currents under alkaline conditions is more challenging.

Method used

The CoFe@NC core-shell structure catalyst is used to optimize the adsorption strength and electronic structure of the intermediate by co-doping the carbon shell by conducting CoFe alloy core and nitrogen. The ultramicroporous structure of the shell hinders the transfer of Cl- and protects the core from corrosion.

Benefits of technology

It achieves high OER activity and selectivity and durability in alkaline seawater. The catalyst runs at 1.85V for 330 hours and can be synthesized in large quantities, providing a good solution for industrial seawater electrolysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932398A_ABST
    Figure CN118932398A_ABST
Patent Text Reader

Abstract

The invention discloses a CoFe-coated NC core-shell structure catalyst, a preparation method and a performance prediction method, the core of the catalyst is a CoFe alloy, the shell of the catalyst is a carbon material co-doped with N, Co and Fe elements, Co / Fe-N4-C active sites in the shell optimize the adsorption strength of an intermediate, and the Co / Fe-N4-C active sites and the core have a synergistic effect, so that the catalyst is endowed with high OER activity and selectivity; and abundant ultra-micropores in the shell show a remarkable screening effect, and transfer of Cl <-> is hindered, so that internal Co / Fe-N4-C active sites and an inner core are prevented from being corroded by Cl <->.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a CoFe@NC core-shell structure catalyst, a preparation method and a performance prediction method, and belongs to the technical field of seawater electrolysis hydrogen production. Background Art

[0002] Making full use of water resources and producing green hydrogen through water splitting is a pollution-free technology, and green hydrogen is considered to be a sustainable energy carrier that may play an important role in the future zero-carbon society. Given factors such as cost-effectiveness, technological maturity and environmental friendliness, alkaline water electrolysis remains one of the most promising methods for green hydrogen generation. So far, water splitting has always used fresh water, but due to the increasing shortage of fresh water, this may become a bottleneck for its widespread industrial application. Considering the abundance of seawater resources, seawater electrolysis may provide an ideal solution for large-scale, low-cost hydrogen production.

[0003] In fact, the presence of a large amount of chloride ions in seawater brings many challenges, such as side reactions and corrosion. On the one hand, the competitive chlorine evolution reaction (CER) leads to low Faradaic efficiency of OER, and on the other hand, severe corrosion caused by chloride ions and generated hypochlorite ions has a negative impact on the durability of anode catalysts, especially for metal-based catalysts.

[0004] One approach to achieve direct seawater electrolysis is to develop electrode materials with high intrinsic activity for OER (anodic oxygen evolution reaction) but poor activity for CER, such as gold and metal-doped carbon-based catalysts. Adjusting the pH of seawater is another important strategy to improve the OER selectivity. It is well known that in acidic media and neutral electrolytes, the difference between the CER and OER potentials is much less than 480 mV, which makes it more challenging to achieve high currents at electrode potentials where CER is thermodynamically unsuitable. Therefore, alkaline conditions (0.5 M NaCl with 0.1 M or 1.0 M KOH) are more suitable for seawater oxidation. In addition to the electrolyte pH, the modification of the electrolyte composition can also significantly affect the OER selectivity. It has been reported that the addition of SO4 2- The OER selectivity of NiFe LDH nanoarrays can be improved by 4-5 times and their stability can be prolonged because the SO4 adsorbed on the electrode 2- It can hinder Cl through electrostatic repulsion - Similarly, SO4 formed in situ during the OER catalytic process 2- It can preferentially adsorb on the surface of NiFe / NiSx catalyst and exclude Cl in the electrolyte. - But SO4 2- Layer may be OH - The diffusion of OH into the active catalyst region produces a negative repulsion effect. -The diffusion rate and number are reduced. Modifying the catalyst surface by introducing functional groups or coatings can enhance the adsorption and activation of oxygen species while minimizing competing reactions. For example, Lewis acids such as Cr2O3 can be loaded on transition metal oxides to induce local basicity, thereby avoiding chloride attack and improving the selectivity of OER. In addition, MnO x Layers can be deposited on IrO x The surface acts as an anion deflection top layer during the acidic seawater oxidation process, allowing the transport of electroneutral or electronegative species (such as H2O, O2, and H) between the IrOx layer and the electrolyte. + ), but hinders the electronegativity of Cl - diffusion, thus significantly improving the OER selectivity and durability of the catalyst. x The barrier effect of the shell and IrO x and semiconductor MnO x The limited charge transfer between the two layers significantly reduces the activity of the catalyst. Similarly, the poor conductivity of the diffusion of anion defect layers can also lead to limited charge transfer. Summary of the invention

[0005] The purpose of the present invention is to provide a CoFe@NC core-shell structure catalyst, a preparation method and a performance prediction method. The Co / Fe-N4-C active site in the catalyst shell optimizes the adsorption strength of the intermediate and synergizes with the core to give the catalyst high OER activity and selectivity. The abundant ultramicropores in the shell show a significant screening effect, which hinders the Cl - transfer, thereby protecting the internal Co / Fe-N4-C active sites and the inner core from Cl - corrosion.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A CoFe@NC core-shell structure catalyst comprises a core and an outer shell, wherein the core is a CoFe alloy, the outer shell is a carbon material co-doped with N, Co, and Fe elements, and there is Co-N in the outer shell. x -C coordination structure and Fe-N x -C coordination structure.

[0008] Preferably, the shell has a thickness of 5-50 nm, and has a microporous structure with a micropore diameter ranging from 0.1-0.7 nm.

[0009] Preferably, in the catalyst, the molar ratio of Co to Fe is 1:(0.5-2.5).

[0010] The preparation method of any of the above-mentioned CoFe@NC core-shell structure catalysts comprises the following steps:

[0011] S1, dissolving a cobalt source, an iron source, and a nitrogen-containing carbon source in a solvent, stirring evenly, and evaporating the solvent to obtain a precursor;

[0012] S2. calcining the precursor to obtain a catalyst.

[0013] Preferably, the cobalt source is one or a mixture of cobalt nitrate, cobalt chloride, cobalt sulfate, cobalt citrate; the iron source is one or a mixture of iron nitrate, iron oxide, iron sulfate, iron citrate; and the nitrogen-containing carbon source is selected from melamine.

[0014] Preferably, the molar ratio of Co in the cobalt source to Fe in the iron source is 1:(0.5-2.5); the added amounts of the cobalt source, iron source and nitrogen-containing carbon source are calculated based on the total added molar amount of Co and Fe and the added amount of the nitrogen-containing carbon source: (2-5) mmol:(10-50) g.

[0015] Preferably, the calcination conditions are: under nitrogen or inert atmosphere, heating to 700-950° C. at 3-8° C. / min, and keeping the temperature for 1.5-3 h.

[0016] Application of any of the above-mentioned CoFe@NC core-shell structure catalysts in hydrogen production by seawater electrolysis.

[0017] Preferably, the loading amount of CoFe@NC core-shell catalyst on the electrode surface is 3-12 mg cm -2 .

[0018] A method for predicting the OER selectivity of a core-shell catalyst comprises the following steps:

[0019] By constructing the chemical structure of the catalyst and then calculating the electrode potential difference △U between the chlorine evolution reaction (CER) and the oxygen evolution reaction (OER) through DFT, the catalyst with the highest electrode potential difference △U is taken as the catalyst with the best OER selectivity.

[0020] The beneficial effects of the present invention are:

[0021] The catalyst consists of a conductive CoFe core and an ion screening metal (Co, Fe) and nitrogen co-doped catalytic carbon shell. The electrons of the conductive metal core can pass through the carbon layer, adjust the electronic structure of the interfacial active sites, and enhance its OER catalytic activity. The ion screening metal (Co, Fe) and nitrogen co-doped catalytic carbon shell is rich in ultra-micropores of about 0.34 nm, which is very effective for OH - It has a significant size screening effect, thus hindering the Cl - mass transfer to the interfacial carbon layer and the conductive metal alloy core, and further prevent Cl- species from accelerating oxygen corrosion through depassivation reactions.

[0022] The catalyst was assembled on an electrode with a geometric area of ​​254 cm 2 In an alkaline seawater electrolyzer, 3000Am can be generated at 1.85V. -2 The current density was 1.370 Å for 330 hours. Moreover, the catalyst can be synthesized in large quantities (hundred grams), providing a good opportunity for industrial seawater electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Schematic diagram of CoFe@NC core-shell structure catalyst;

[0024] Figure 2 Electrochemical performance of the prepared samples; (A) Linear sweep voltammetry curves, (B) stability test, and (C) Faradaic efficiency of oxygen evolution reaction (OER) of samples with different cobalt-iron molar ratios (CoFe01@NC, CoFe37@NC, CoFe55@NC, CoFe73@NC, and CoFe10@NC) at 2.46 V relative to the reversible hydrogen electrode (RHE) in 0.1M KOH+0.6M NaCl solution;

[0025] Figure 3 (A and B)CoFeO x HAADF-STEM images of @NC and (C and D)CoFe55@C;

[0026] Figure 4 Structural characterization of CoFe55@NC; (A) HAADF-STEM image of CoFe55@NC; (B) Atomic ratio of N in CoFe55@NC and Co / Fe-N in N1s at different XPS depths x Relative content; (C) NK edge soft XAS spectra of CoFe55@NC and BN; (D) CK edge soft XAS spectra of CoFe55@NC, CoFe55@C and HOPG; (E) Co R space EXAFS spectrum fitting of CoFe55@NC;

[0027] Figure 5 Element mapping image of CoFe55@NC;

[0028] Figure 6 CoFe55@NC, CoFeO x XRD patterns of @NC and CoFe2O4;

[0029] Figure 7(A) The atomic ratio of Fe in CoFe55@NC and the relative content of Fe-Nx in Fe 2p3 / 2; (B) The atomic ratio of Co in CoFe55@NC and the relative content of Co-Nx in Co 2p3 / 2 for different XPS depth profiles; (C) The atomic ratio of N, Fe and Co in CoFe55@NC, and the error bars for 0, 6 and 12 nm etching depths;

[0030] Figure 8 XPS depth profiles of Fe 2p (A), Co 2p (B), and N1s (C) of CoFe55@NC;

[0031] Fig. 9 (A) Co K-edge and (B) Fe K-edge X-ray absorption spectra (XAS) of CoFe55@NC and CoFe55@C; (C) Co K-edge and (D) Fe K-edge linear combination fitting analysis of CoFe55@NC;

[0032] Fig.10 Fitting of the extended X-ray absorption fine structure (EXAFS) spectrum in the Fe R space of CoFe55@NC;

[0033] Fig.11 For the preparation of CoFe55@NC, RuO2, CoFe2O4, CoFe55@C and CoFeO x Electrochemical performance of @NC catalyst; (A) in 0.1 M KOH + 0.6 M NaCl at 10 mV s -1 LSV curves obtained at scan rates of 2000 ℃ and 4000 ℃; Inset: comparison of overpotentials (η); (B) OER selectivity in electrolytes containing 0.1 M KOH and different concentrations of NaCl (from 0.2 to 3.0 M); (C, D) Long-term stability of CoFe55@NC supported on carbon paper in 0.1 M KOH + 0.6 M NaCl (C) and 1.0 M KOH + 0.6 M NaCl (D) electrolytes; (E) TEM images of CoFe55@NC before and after 2000 h of catalytic reaction; (F) Monolithic simulated seawater electrolyzer assembled by CoFe55@NC / / Raney nickel was tested at 25 °C using 30% KOH + 0.6 M NaCl as electrolyte; Inset: CoFe55@NC sprayed onto nickel foam (Φ18 cm, 8 mg cm -2 , left) and a photo of a seawater splitting electrolyzer (right);

[0034] Fig.12 is the oxygen evolution reaction (OER) selectivity at 1.66 V and 2.46 V relative to the reversible hydrogen electrode (RHE);

[0035] Fig.13 The stability test was conducted in alkaline simulated seawater (0.1 M KOH + 0.6 M NaCl) at a potential of 1.66 V relative to the reversible hydrogen electrode (RHE) for 10 hours;

[0036] Fig.14 Characterization of the structural evolution and catalytic mechanism of CoFe55@NC; (A) Co atomic ratio of CoFe55@NC-A / B obtained from different X-ray photoelectron spectroscopy (XPS) depth analysis; (B) NK edge soft X-ray absorption spectra (Soft XAS) of CoFe55@NC-A / B and boron nitride (BN); (C) Co K edge X-ray near edge structure (XANES) spectra of CoFe55@NC-A / B and CoFe2O4-A / B; (D) Limited Cl formed in situ during seawater oxidation - / OH - Schematic diagram of leaching the outer layer of carbon; (E) Calculated OER overpotential (ηOER) at different sites of alkaline seawater oxidation; (F) Comparison of OER selectivity using the descriptor ΔU (potential difference between chlorine evolution reaction and oxygen evolution reaction);

[0037] Fig.15 For the iron atomic ratio of CoFe55@NC-A / B, O1s of CoFe55@NC-A / B (B), and Fe 2p and Co 2p of CoFe55@NC-A (C) according to different XPS depth profiles;

[0038] Fig.16 Schematic diagrams of four structural models (Co / Fe@NC, Co / Co@NC, Fe / Fe@NC and CoFe2O4);

[0039] Fig.17 is the adsorption energy of Co active site to CER intermediate;

[0040] Fig.18 Mechanistic analysis of the four model OER and CER reaction pathways; free energy of possible pathways of CER-1 (A), CER-2 (B) and OER (C) at zero potential;

[0041] Fig.19 is the CER overpotential (η) of the four models in alkaline simulated seawater CER );

[0042] Fig. 20Effects of the carbon outer layer and core-shell structure on the OER activity; (A) Transmission electron microscopy (TEM) images of CoFe / NG before and after stability test; (B) Linear sweep voltammetry (LSV) curves of CoFe / NG and CoFe / NG-A after catalysis in 0.1 M KOH + 0.6 M NaCl for 1 h at a scan rate of 10 mV s -1 ; (C) Nyquist plots of CoFe55@NC and CoFe55@NC-AW; (D) Linear sweep voltammetry (LSV) curves of CoFe55@NC and CoFe55@NC-AW in 0.1 M KOH + 0.6 M NaCl at a scan rate of 10 mV s -1 ; Inset: reaching 10.0 mA cm -2 Comparison of required overpotential (η);

[0043] Fig.21 At 10 mA cm -2 Transmission electron microscopy (TEM) images and X-ray diffraction (XRD) patterns of CoFe2O4-B (before) and CoFe2O4-A (after) were analyzed at a current density of 10 h;

[0044] Fig. 22 Transmission electron microscope image of CoFe55@NC-AW;

[0045] Fig.23 (A) Co / Fe-N in direct contact with cobalt-iron alloy (CoFe55@NC) x -C layer density of states (DOS), and (B) Co / Fe-N not in contact with metal alloy x - Density of states of the C layer (CoFe55@NC-AW), the inset is the corresponding model;

[0046] Fig.24 Transmission electron microscope images of CoFe55@NC and CoFe55@NC-thin;

[0047] Fig.25 Raman spectra of CoFe55@NC and CoFe55@NC-thin;

[0048] Fig.26Figure 3: Ion screening mechanism of carbon shell and practical application potential of CoFe55@NC. (A) Analysis of pore size distribution by CO2 adsorption isotherm. (B) Relationship between the number of different anions and working time. Inset: Snapshot of molecular dynamics simulation of electrolyte system above electrode surface. (C) Concentration distribution of OH- and Cl- ions in CoFe55@NC simulated channel model at nearly 20,000 picoseconds based on finite element method (FEM). (D) Concentration distribution of OH- and Cl- ions in CoFe55@NC-thin simulated channel model at nearly 3,500 picoseconds based on finite element method (FEM). - and Cl - Concentration distribution of ions;

[0049] Fig. 27 CO2 adsorption isotherms of CoFe55@NC and CoFe55@NC-thin measured at standard temperature and pressure (STP, 298.15 K and 101.325 kPa, respectively);

[0050] Fig.28 Comparison of the number of various anions with the working time; Inset: Molecular dynamics simulation snapshot of the electrolyte system above the electrode surface;

[0051] Fig.29 To conduct pore size distribution analysis by CO2 adsorption isotherm;

[0052] Fig.30 (A) LSV curves and (B) stability tests of CoFe55@NC-thin (4nm), CoFe55@NC-7nm, CoFe55@NC (12nm), CoFe55@NC-26nm and CoFe55@NC-32nm in 0.1M KOH+0.6M NaCl solution;

[0053] Fig.31 Transmission electron microscope image and X-ray diffraction pattern of CoFe55@NC prepared in large quantities (hundred grams);

[0054] Fig.32 The electrochemical properties of the prepared Ni@NC, NF@NC, NFW@NC and CFW@NC. DETAILED DESCRIPTION

[0055] The present invention prepares a synergistic core-shell structure catalyst by adopting an ion screening strategy, which simultaneously achieves high activity and excellent durability for direct seawater electrolysis. The catalyst consists of a metallic CoFe alloy core and a microporous N, Co and Fe co-doped carbon shell (CoFe@NC). The conductive alloy core significantly improves the conductivity of the material, thereby promoting electron transfer between the core and the shell, while the interfacial Co / Fe-N4-C coordination on the inner wall of the porous shell makes the catalyst highly active and selective for OER ( Figure 1 In addition, according to molecular dynamics (MD) and finite element method (FEM) simulation calculations, the abundant ultramicropores of about 0.34 nm in the shell layer have a significant impact on the OH - The catalyst exhibits a significant sieving effect, thereby protecting the active Co / Fe-N4-C sites in the metal core and the interfacial carbon shell from Cl- corrosion. As a result, the optimal catalyst exhibits excellent long-term stability for more than 2000 h in OER catalysis (three-electrode configuration) in a salt water environment and a high effective geometric anode surface area of ​​254 cm 2 (25℃), 3000Am is stably provided at a cell voltage of about 1.85V in an alkaline simulated seawater electrolyzer -2 The high current density lasted for more than 330 hours. In addition, the simple and scalable (hundred-gram scale) preparation strategy of the core-shell catalyst makes it possible to achieve large-scale application.

[0056] The total amount of metal nitrate was kept constant at 4 mmol and melamine was 30 g, the molar ratios of Co(NO3)2·6H2O and Fe(NO3)3·9H2O were set to 0:10, 3:7, 5:5, 7:3 and 10:0, respectively, the cobalt source, iron source and nitrogen-containing carbon source were dissolved in a solvent, stirred evenly and then the solvent was evaporated to obtain a precursor; then the precursor was heated in a tube furnace under a N2 atmosphere at 5 °C min -1 The heating rate was set at 800 °C for 2 h to obtain CoFe01@NC, CoFe37@NC, CoFe55@NC, CoFe73@NC and CoFe10@NC samples.

[0057] For the CoFe55@NC-thin sample, the preparation method is basically the same as the above, except that it is prepared by heating at 800°C for 1h, and the amount of melamine used is 10g.

[0058] Large batches (hundred-gram scale) of CoFe55@NC were prepared using a large-capacity mixer that could add about 5 kg of raw materials at a time and then heated in a tube furnace at 5 °C min under N2 atmosphere. -1 The heating rate was 800 °C for 2 h.

[0059] Since CoFe55@NC has the best performance ( Figure 2 ), so it was selected as a model catalyst for further study. For comparison, nitrogen-free graphitic carbon shell-coated CoFe alloy (CoFe55@C), nitrogen-doped graphitic carbon-coated CoFeOx (CoFeOx@NC) ( Figure 3 ) and bare CoFe2O4 without carbon shell.

[0060] The preparation of CoFe55@C (without nitrogen doping) control sample was carried out under the same synthetic conditions as CoFe55@NC using polydextrose (30 g) as the carbon source.

[0061] In addition, nitrogen-doped graphitic carbon-encapsulated CoFeO was obtained by oxidizing CoFe55@NC at 300 °C for 2 h in an air atmosphere in a muffle furnace. x CoFeO in @NC x ; Bare CoFe2O4 was obtained by calcining CoFe55@NC at 800℃ for 2 hours in a muffle furnace under air atmosphere.

[0062] CoFe / NG was prepared by argon plasma treatment.

[0063] For CoFe55@NC-AW, CoFe55@NC (~1.0 g) was washed with about 100 mL (3.0 M, 25°C) of hydrochloric acid for 100 h to partially remove the metal core to obtain the sample.

[0064] like Figure 4 Middle A area and Figure 5 The scanning electron microscope (SEM), transmission electron microscope (TEM) images and energy dispersive X-ray (EDX) mapping shown in the figure confirm the core-shell structure of CoFe55@NC. The carbon shell thickness of CoFe55@NC is about 12nm, the diameter of the metal core is about 180nm, and the lattice spacing is 0.2020nm, which is very consistent with the (011) crystal plane of CoFe alloy. Elemental mapping image ( Figure 5 ) further confirmed the metal core and nitrogen-doped carbon shell structure of the particles. X-ray diffraction (XRD) Rietveld refinement patterns demonstrated the presence of a CoFe alloy main phase in CoFe55@NC (Pm-3m space group) and CoFe55@C (Im-3m space group) samples, while the bare CoFe2O4 sample was a pure single structure (Fd-3m space group). For the oxidized CoFeOx@NC sample, new peaks appeared at 2θ of 30.2°, 35.6°, 57.3°, and 62.7°, which can be well attributed to the CoFe2O4 spinel phase ( Figure 6 ).

[0065] To gain insight into the composition and element distribution within the carbon shell, the chemical composition and state at the surface and at different depths of CoFe55@NC (0, 3, 6, 9, and 12 nm) were investigated by depth profiling X-ray photoelectron spectroscopy (via argon ion etching). Figure 4 Middle B area and Figure 7 In addition to C atoms, N, Co, Fe and O atoms were also detected in the shell, with relative contents ranging from 1.2-4.0 at.%, and the content of N was slightly higher than that of Co and Fe. In CoFe55@NC, the atomic ratio of N decreased slightly from the surface (4.1 at.%) to the interior (3.7 at.%). Figure 4 (B area in the middle). N 1s spectrum ( Figure 8 ) can be decomposed into pyridinic N (398.7 eV), porphyrin-like metal-N coordinated M-Nx (399.7 eV), pyrrolic N (400.9 eV), graphitic N (402.9 eV), and oxidized N (405.1 eV). When approaching the interior, the M-Nx part (corresponding to the Co / Fe-Nx-C coordination in CoFe55@NC) moves positively to higher binding energies. Importantly, when the etching depth exceeds 9 nm, the relative content of the Co / Fe-Nx part increases significantly ( Figure 4 In the Fe2p and Co 2p spectra ( Figure 8 ), where the Fe-Nx (about 708 eV) and Co-Nx (about 779 eV) species gradually increase from the shell surface to the inner core. In addition, the binding energies of the Fe-Nx and Co-Nx peaks are negatively shifted by 1.4 eV and 0.6 eV, respectively. According to the Mott-Schottky heterojunction, this shift indicates that electrons are efficiently transferred from the metal core to the nitrogen-doped carbon layer. All other CoFe@NC samples have similar core-shell structures, but with different cobalt-iron ratios in the core and NC shell.

[0066] In addition, hard X-ray absorption spectroscopy (XAS) and soft XAS (total electron yield (TEY) mode, probing depth of about 5 nm) were used to further investigate the structure and coordination environment of the active sites in CoFe55@NC. Figure 4 In the C region, it can be found that compared with the boron nitride (BN) reference sample, CoFe55@NC has a new peak at about 395eV, indicating that Co / Fe 3d electrons can interact with N atoms. At the same time, the CK edge soft XAS spectra of CoFe55@NC and CoFe55@C ( Figure 4The D region in the middle is similar to that of highly oriented pyrolytic graphite (HOPG, reference sample), confirming that the Co / Fe doped in the carbon is through the formation of Co / Fe-N bonds rather than Co / Fe-C bonds in the carbon shell. This is easy to understand, because the N atoms doped in the carbon shell have stronger electronegativity and electron affinity than C atoms, and are more likely to serve as anchoring sites for positive Co / Fe ions to form Co / Fe-Nx-C coordination on the carbon shell of CoFe55@NC. In contrast, on the nitrogen-free carbon shell, it is difficult for the electrically neutral C atoms to capture Co / Fe elements, resulting in the loss of coordination sites. Since the introduction of N atoms can cause the adjacent metal or C atoms to carry partial positive charge, in the X-ray absorption near edge structure (XANES) spectrum, the Co and Fe K edges of CoFe55@NC are higher than those of CoFe55@C ( Fig. 9 In the Co / Fe-Nx-C coordination, the higher oxidation state of Co / Fe can greatly improve the electron transfer efficiency and promote the adsorption of OH* intermediates during water dissociation.

[0067] In order to better study the influence of CoFe alloy and Co / Fe-N on the structural composition, a linear combination fitting (CoFe55@NC) analysis was further performed ( Fig. 9 The trends of XANES data were analyzed (C and D regions in the figure), where CoFe alloy and Co / Fe-N were used as references. In addition, the extended X-ray absorption fine structure (EXAFS) of Co R space and Fe R space was well fitted using CoFe alloy (FeCo_mp-2090, Pm-3m

[221] space group) and Co / Fe-N4-C (inset model) with Co and Fe as fitting centers, respectively. Figure 4 Middle E area and Fig.10 ). In this model, the coordination numbers of Co-N and Fe-N centers are about 4. In Co / Fe-N4-C, the bond lengths of Co-N, Co-Fe, Co-Co, Fe-Fe, and Fe-N are approximately and They make a major contribution to the EXAFS signal of the first coordination shell. In contrast, the fitting effect of Co K-edge EXAFS spectrum only using CoFe alloy (FeCo_mp-2090) is not satisfactory.

[0068] In alkaline simulated seawater (0.1 M KOH + 0.6 M NaCl), a three-electrode configuration and 10 mV s -1 The oxygen evolution reaction (OER) activity and selectivity of the synthesized catalysts were evaluated at a scan rate of , and a commercial RuO2 catalyst was tested for comparison. Fig.11The linear sweep voltammetry (LSV) curves in the middle A region show that CoFe55@NC reaches 10.0 mA cm -2 The overpotential (η) required for the current density is the smallest (285mV), which is much smaller than CoFe55@C (402mV), bare RuO2 (490mV), CoFeO x @NC (520mV) and CoFe2O4 (1190mV). At the same time, compared with CoFe55@C (102.5mV dec -1 )、RuO2(76.2mVdec -1 ), CoFeO x @NC(96.6mV dec -1 ) and CoFe2O4 (107.2mV dec -1 ), CoFe55@NC also exhibits the lowest Tafel slope value (58.7 mV dec -1 ), indicating that its OER kinetics is the fastest. The OER activity of CoFeOx@NC is significantly lower than that of CoFe55@NC, which indicates that the synergistic effect between the highly conductive metal core and the NC shell may play an important role in promoting the OER activity of CoFe55@NC. x Compared with CoFe55@NC (109.6Ω), the charge transfer resistance of CoFe55@NC (7.3Ω) is much lower, indicating that the introduction of the metal core can significantly enhance the charge transfer.

[0069] In alkaline simulated seawater, the OER selectivity of the catalyst was further tested at 1.66 V vs RHE (<1.71 V vs RHE, OER-dominated region) and 2.46 V vs RHE (>1.71 V vs RHE, chlorine evolution reaction, CER, may occur). Fig.12 As shown in Figure 2, at 1.66 V vs RHE, the OER selectivity of all electrocatalysts is close to 100%, but at 2.46 V vs RHE, the OER selectivity of CoFe55@NC (~99.5%) is significantly better than that of CoFe55@C (91.5%), RuO2 (81.5%), CoFeO x @NC (92.0%) and CoFe2O4 (50.5%). In addition, at 2.46 V vs RHE, as the NaCl concentration in alkaline simulated seawater increased from 0.2 M to 3.0 M, the OER selectivity of all samples decreased ( Fig.11 However, only CoFe55@NC maintains more than 90% OER selectivity, indicating its superiority in high-concentration brine decomposition.

[0070] The long-term stability of electrocatalysts in alkaline seawater is an important factor in evaluating the Cl - or ClO - An important indicator of corrosion resistance. In alkaline simulated seawater, the chronoamperometric curve was obtained at a constant potential of 1.66 V vs RHE ( Fig.13 ). After 10 hours, the current density of CoFe55@NC and CoFeOx@NC showed almost no decay, while the current density of CoFe55@C, RuO2, and CoFe2O4 decreased by 10%, 20%, and 60%, respectively. In addition, CoFe55@NC was loaded on a carbon paper (CP) substrate to enhance the adhesion of the substrate and the catalyst, and it could achieve a high current density of 10.0 mA cm in 0.1 M KOH + 0.6 M NaCl. -2 Stable operation for 700 hours ( Fig.11 C area), stable operation in 1.0M KOH+0.6M NaCl for 2000 hours ( Fig.11 Importantly, after 2000 h of operation (marked as A), the crystal structure and core-shell morphology of the used CoFe55@NC (CoFe55@NC-A) remain well maintained ( Fig.11 The charge transfer resistance is 7.8Ω, which is only slightly higher than the charge transfer resistance (7.3Ω) of CoFe55@NC (labeled as CoFe55@NC-B) before the stability test.

[0071] In addition, a whole simulated seawater decomposition electrolyzer was assembled ( Fig.11 The electrolytic cell uses batch-synthesized CoFe55@NC loaded on a nickel mesh as the anode (Φ18 cm, 254 cm 2 , 400 mesh), Raney nickel loaded on a nickel mesh as the cathode (Φ18 cm, 254 cm 2 , 400 mesh), and 30% KOH + 0.6M NaCl solution as electrolyte. The electrolytic cell can generate up to 3000A m at a low voltage of about 1.85V (25°C). -2 High current density and stable operation for more than 330 hours ( Fig.11 The polarization curves and stability experiments of Raney Nickel / / Raney Nickel and CoFe55@NC / / Raney Nickel show that the performance of CoFe55@NC is better than that of commercial Raney Nickel in alkaline seawater electrolysis.

[0072] As mentioned above, CoFeO has relatively poor conductivity. x Core CoFeO xUnlike CoFe55@NC, CoFe55@NC has a conductive metal core and exhibits significantly higher OER activity. XPS results demonstrate the enhanced electron transfer from the metal core to the nitrogen-doped carbon layer ( Figure 8 ). However, the CoFe core itself should not be the main active site. If so, compared with CoFe55@NC(S BET =48.6m 2 g -1 ) compared to CoFe55@C, which should have a larger specific surface area (S BET =241.2m 2 g -1 ) and better reactant accessibility, which should show better OER performance. However, in fact, in 0.1 M KOH + 0.6 M NaCl, CoFe55@NC achieved 72.3 mA cm at a potential of 1.6 V relative to RHE. -2 The current density is 27.5 times that of CoFe55@C ( Fig.11 Therefore, the active sites should mainly exist on the nitrogen-doped carbon shell and contribute to the excellent activity of CoFe55@NC.

[0073] After long-term stability testing, depth-profiling X-ray photoelectron spectroscopy (XPS) was also applied to study the chemical composition of the layers at 0, 3, 6, 9, and 12 nm from the surface of CoFe55@NC-A. It was found that the contents of Co and Fe dropped sharply when the subsurface layer was less than 6 nm from the outer surface ( Fig.14 Middle A area and Fig.15 ), while the inner part of the shell remains almost unchanged. This suggests that although the Co / Fe atoms in the surface layer of the carbon sublayer may be removed during the catalytic reaction, the inner layer of the shell and the metal core can prevent further Cl- corrosion. In addition, the NK edge soft X-ray absorption spectrum (XAS) of CoFe55@NC-A ( Fig.14 The B region in the middle shifts from 395.4eV to 394.5eV of CoFe55@NC-B, and the spectral weight increases significantly. This further proves the existence of Co / Fe-N4 groups after long-term operation and the strengthening of the covalent bond between Co 3d and N1s with the increase of Co valence state, resulting in the increase of Co 2 + Oxidized to Co 3+ In addition, a significant shift of the Co K-edge X-ray near-edge structure (XANES) to higher energies was observed compared with CoFe55@NC-B ( Fig.14The increased Co valence can be attributed to the oxidation of Co atoms by OH- during the oxygen evolution reaction (OER). In contrast, the Co K-edge X-ray near-edge structure (XANES) of CoFe2O4 shifted to lower energy after durability testing ( Fig.14 From the extended X-ray absorption fine structure (EXAFS) fitting results of the Co K edge of CoFe2O4-A / B, it can be seen that during the oxidation of seawater, Cl - can be embedded in CoFe2O4 to form coordination with Co. The Fe K-edge XANES of CoFe2O4-A / B has a similar shift trend to its Co K-edge XANES. However, the Fe K-edge XANES changes of CoFe55@NC before and after the electrochemical stability experiment are negligible, indicating that the valence state of Fe atoms has not changed significantly during this catalytic process. Based on the above results, it can be concluded that during the alkaline seawater decomposition process, although the Co / Fe-N4-C groups in the sub-surface layer of CoFe55@NC are affected by Cl - However, the inner layer of the shell and the Co / Fe-N4 groups in the metal core can successfully prevent further Cl - corrosion, and continue to play a strong role as active sites ( Fig.14 D region), thus enabling CoFe55@NC to maintain its high catalytic activity over 2000 hours of operation. - The diffusion barrier effect may also partially contribute to the higher apparent OER selectivity of CoFe55@NC over other catalysts.

[0074] In order to fully reveal the key role of the Co / Fe-N4-C coordination structure in its excellent oxygen evolution reaction (OER) performance, four representative models representing CoFe@NC, CoCo@NC, FeFe@NC and CoFe2O4 were constructed based on the experimental characterization results. A series of density functional theory (DFT) calculations on OER and chlorine evolution reaction (CER) in alkaline seawater were carried out based on these models. Fig.16 ). The simulation calculation process is:

[0075] Using a three-layer graphitized carbon ( The pores are created by removing carbon atoms in the top layer, and the 8 carbon atoms at the edge are exchanged with nitrogen. The CoFe2O4(311) surface with a (1×2) superlattice is used to represent the flat plate model of the metal oxide without a carbon shell. The vacuum at the bottom of the plate prevents unintended interactions between the periodically repeated images in each model. The atoms were fixed at their optimized bulk positions, while the others were allowed to relax. All density functional theory (DFT) calculations were performed using the Vienna Ab Initio Simulation Package (VASP). The electron interactions were described with the generalized gradient approximation (GGA) projected augmented wave (PAW) method parameterized by Perdew, Burke, and Ernzerhof (PBE), and the van der Waals interactions were described with Grimme’s dispersion correction (DFT-D3), using a kinetic cutoff energy of 450 eV and 2 × 2 × 1 gamma-centered k-points. In addition, all atoms were fully relaxed until the energy and residual forces on each atom converged to 1 × 10 -5 eV and

[0076] The OER process can generally be described as four electron transfer steps

[0077]

[0078]

[0079] Where * represents the active site on the catalyst surface, *OH, *O, *OOH represent three different catalytic intermediates. The Gibbs free energy can be obtained by the following expression:

[0080] G(T) = E DFT + G correct (T) = E DFT + ZPE - TS + △U 0→T (5)

[0081] Where G(T) is the Gibbs free energy at temperature T, E DFT is the DFT energy, G correct (T) is the thermal correction of Gibbs free energy, ZPE, S, U 0→T They are zero-point energy, entropy, and the change in internal energy due to temperature. Based on these four steps, the Gibbs free energy change can be defined as

[0082] △G1=G(*OH) + 1 / 2G(H2) - G(*) - G(H2O) + G U + G pH (6)

[0083] △G2 = G(*O) + 1 / 2G(H2) - G(*OH) + G U + G pH (7)

[0084] △G3= G(*OOH) + 1 / 2G(H2) - G(*O) - G(H2O) + G U + G pH (8)

[0085] △G4=4.92+G(*)+2G(H2O)-3 / 2G(H2)-G(*OOH)+G U +GpH. (9)

[0088] Where GU = -eU, U is the electrode potential, GpH = -k B Tln10×pH=-0.0592pH (pH=13 in this work). The standard electrode potential of OER at pH=13 is 0.4604V (1.23-0.059213, SHE). Therefore, the theoretical overpotential OER can be easily expressed as

[0089] η OER = max(△G1, △G2, △G3, △G4) / e - 0.4604 V. (10)

[0090] like Fig.17 As shown in Figure 2, the adsorption intensity of the intermediates (OH and Cl) on CoFe2O4 is much greater than that on CoFe@NC and CoCo@NC, which will hinder the desorption of the intermediates and block the Co active sites, resulting in the deactivation of CoFe2O4. The standard free energy curves of OER and CER of the four models at zero potential were also calculated and shown in Fig.18 and Table 1. OER overpotential (η) of CoFe@NC OER ) as low as 0.282V( Fig.14 The E region), which is very close to the experimental value (0.285 V), verifies its excellent OER activity. These OER calculation results confirm that the Co / Fe-N4-C coordination is essential for the excellent OER activity of CoFe@NC. Then, using the descriptor △U (V, △U = △U0 + η CER -η OER ) to clearly illustrate the OER selectivity (η CER like Fig.19 △U is defined as the electrode potential difference between the chlorine evolution reaction (CER) and the oxygen evolution reaction (OER), and a larger value of △U indicates a higher OER selectivity. Fig.14As shown in the middle F region, CoFe@NC has the largest △U of 1.09V, which is much higher than the standard △U0 value (0.49V) and other models, indicating its best OER selectivity. The order of △U of these materials is: CoFe@NC (1.09V)>CoCo@NC (0.94V)>FeFe@NC (0.88V)>CoFe2O4 (0.40V). The excellent intrinsic OER selectivity of CoFe@NC and the Cl- screening effect of the carbon shell of the CoFe@NC catalyst can minimize the generation of corrosive ClO-, which is conducive to long-term electrocatalytic operation in seawater electrolyte.

[0091] Table 1

[0092]

[0093] In order to further reveal the role of the subsurface carbon layer in protecting the interface Co / Fe-N4-C and the core from OH - / Cl - In order to improve the corrosion resistance, CoFe was directly deposited on the surface of N-doped graphene (CoFe / NG) by argon plasma treatment. CoFe exists in the form of exposed nanoclusters with a diameter of about 1 nm ( Fig. 20 The Co / Fe-N4 moiety can be identified from its Co 2p spectrum. However, in 0.1 M KOH + 0.6 M NaCl solution, CoFe / NG requires an overpotential of 540 mV to reach 10.0 mA cm -2 The current density ( Fig. 20 B region), which is significantly greater than the overpotential required for CoFe55@NC (285mV). In addition, the activity of CoFe / NG dropped sharply after 1 hour of catalysis. After 10 hours of catalysis, almost all the CoFe nanoclusters on its surface were removed, indicating that its structure and activity were unstable during alkaline seawater oxidation. In addition to Co / Fe-NG, the stability of bare CoFe2O4 and metal foams (such as nickel foam, nickel-iron foam and cobalt foam) in seawater decomposition was also studied. Cl 2p depth profiling XPS at 0nm and 3nm confirmed that after running in 0.1M KOH+0.6M NaCl for 10 hours, the surface of the non-porous CoFe2O4 was significantly damaged, forming an amorphous layer (2~3nm) ( Fig.21 ), while its OER activity decreased by 60% ( Fig.13). In 0.1M KOH+0.6M NaCl, the metal foam also showed poor stability. In contrast, the crystal structure and core-shell morphology of CoFe55@NC were well maintained after 2000 h of catalytic testing. These results all prove that the shell subsurface layer plays a crucial role in protecting the active sites from Cl- corrosion.

[0094] To reveal the key role of the conductive core, CoFe55@NC was washed with dilute hydrochloric acid solution to obtain CoFe55@NC-AW. From the transmission electron microscopy (TEM) image of CoFe55@NC-AW ( Fig. 22 ) it can be seen that during the acid treatment, the CoFe core can be partially removed and separated from the N-doped carbon shell to form a yolk-shell structure. However, the N1s spectrum of CoFe55@NC-AW proves that a large amount of Co / Fe-N4-C is still present after acid treatment. Even though the X-ray diffraction (XRD) pattern of CoFe55@NC-AW still shows two characteristic peaks at 2θ of 26.4° and 44.9° similar to those of CoFe55@NC, the charge transfer resistance increases significantly to 40.5Ω, indicating that the charge transfer rate in CoFe55@NC-AW is slower ( Fig. 20 Therefore, in 0.1M KOH + 0.6M NaCl, CoFe55@NC-AW requires a larger overpotential (369 mV) than CoFe55@NC (285 mV) to reach 10.0 mA cm -2 The current density ( Fig. 20 Density functional theory (DFT) calculations further demonstrate that the density of states (DOS) of the Co 3d orbital near the Fermi level of Co / Fe-Nx-C in direct contact with the metal alloy is much higher than that of the Co 3d orbital not in contact with the metal alloy, which can promote the adsorption of adsorbates and thus improve the OER activity ( Fig.23 ).

[0095] Furthermore, by adjusting the mass ratio of metal and melamine, a CoFe55@NC sample with a thinner carbon shell (4 nm) (CoFe55@NC-thin) was prepared. Fig.24 ) and a large Raman intensity ratio of the D band to the G band (ID / IG) (~1.03, Fig.25 ) shows that there are a lot of defects on the graphitized carbon shell. The pore size distribution of CoFe55@NC and CoFe55@NC-thin was analyzed by carbon dioxide adsorption isotherm ( Fig.26 Middle A area and Fig. 27). The results show that the carbon shells of CoFe55@NC and CoFe55@NC-thin both have ultramicropores with diameters of approximately 0.34 nm and 0.57 nm, which are caused by defects on the graphitized carbon or the spaces between the graphitized carbon layers.

[0096] In order to better understand the role of ultramicropores in ion screening, classical molecular dynamics (MD) simulations were performed based on a two-dimensional slit model consisting of two graphitized carbon layers, with the distance (ds) set to 0.34nm and 0.57nm to correspond to the results of the pore size. The MD calculation results show that it is the two-dimensional slit with a ds value of 0.34nm that has the greatest effect on OH - Shows significant size screening effect, exceeding Cl - , and protect the catalyst from Cl - corrosion( Fig.26 Region B), rather than a 0.57 nm two-dimensional slit ( Fig.28 ). This result is consistent with the excellent stability of CoFe55@NC in alkaline simulated seawater oxidation. In addition, the pore size test ( Fig.29 ) showed that after long-term stability testing, ultra-micropores with a diameter of about 0.34 nm in CoFe55@NC-A still existed. However, although CoFe55@NC-thin also has ultra-micropores with size screening, the overly thin carbon shell can hardly completely protect the metal alloy core from long-term Cl- intrusion and corrosion.

[0097] In order to further reveal the function of the carbon shell, finite element method (FEM) simulations were also performed to study the effect of carbon shell thickness on the ion mass transfer process. A simulation channel model for FEM calculation was constructed based on the pore size distribution and transmission electron microscopy (TEM) images of CoFe55@NC and CoFe55@NC-thin. Fig.26 The C and D regions in the middle). It can be seen from the model that the width of some channels is smaller than the size of hydrated chloride ions, which can effectively hinder the penetration of chloride ions. Considering the size difference between chloride ions and hydroxide ions, the modified Poisson-Nernst-Planck (MPNP) equation is used as the governing equation for ion migration in the FEM simulation to explain the ion screening mechanism of the carbon shell. Fig.26As shown in the D area in the middle, the entire simulation process of CoFe55@NC almost reaches equilibrium after nearly 20000ps, and the further diffusion of ions becomes insignificant. Therefore, the state of the system at 20000ps is selected for analysis. It is found that the hydroxide ions can be dispersed throughout the carbon shell, while the mass transfer of chloride ions is hindered and confined to the outside of the carbon shell, thereby preventing the chlorine species from accelerating the oxygen corrosion of the metal alloy core. For CoFe55@NC-thin, the diffusion process can reach equilibrium after 3500ps, and at this stage, both hydroxide ions and chloride ions can be dispersed throughout the carbon shell and reach the core ( Fig.26 Therefore, a too thin carbon shell will not be able to completely block the mass transfer of chloride ions.

[0098] In the oxygen evolution reaction (OER) catalytic process, if chloride ions are not involved in the reaction, the CoFe metal core in CoFe55@NC will only react with hydroxide ions (OH-) (Eq. 1) and be oxidized to form Co / FeO x H y The passivation shell (low conductivity) is beneficial to reduce the oxygen corrosion rate. It can effectively protect the CoFe core from further corrosion, which can be well demonstrated by the almost unchanged charge transfer resistance of CoFe55@NC-A. However, if chloride ions are involved in the reaction, the Co / FeO x H y The passive area will be destroyed, generating soluble Co / Fe(OH) x . Therefore, chloride ions will greatly accelerate the corrosion of the CoFe metal core in the catalyst. Unlike CoFe55@NC, which can form a limited chloride-corrosion-resistant Co / Fe-leached carbon layer during long-term catalysis, the Co / Fe-N4-C part of CoFe55@NC-thin will be completely removed, while its core-shell structure may be corroded and destroyed after 100 h of catalysis. As a result, its OER current density dropped sharply by 99.5%.

[0099] Passivation reaction: 2Co / Fe+O2+H2O→2Co / FeO x H y (1)

[0100] Cl - Depassivation reaction of Co / FeO x H y +Cl - +H2O→Co / Fe(OH) x +Cl - (2)

[0101] Subsequently, by adjusting the mass ratio of metal to melamine, other CoFe@NC samples with carbon shell thickness of 7nm, 26nm and 32nm were prepared. It was found that when the carbon shell thickness was greater than 7nm, it could effectively protect the metal alloy core from corrosion during long-term catalysis ( Fig.30 ). A thicker carbon shell may provide more anchoring sites for Co / Fe-N4-C coordination, resulting in higher OER activity. However, when the thickness is too large, the shuttling of electrons between carbon layers will be restricted, resulting in a decrease in the intrinsic activity of active sites at the shell interface. At the same time, an overly thick carbon shell will also hinder the penetration of hydroxide ions, which together lead to a decrease in OER activity. Both experimental and computational results indicate that the efficient chloride ion screening ability of N-doped graphitized carbon shell can endow CoFe@NC with ultra-stable activity in direct seawater decomposition.

[0102] For practical applications, a facile and scalable synthesis of the catalyst is equally important. Here, we further carried out a large-scale (hundred-gram scale) synthesis of this CoFe55@NC catalyst following the same procedure as the previous small-batch synthesis, but using a larger volume of mixture and a tube furnace. According to the XRD patterns and TEM images ( Fig.31 ), the bulk-prepared CoFe55@NC has the same crystal structure and core-shell morphology as the small-batch-prepared CoFe55@NC. Similarly, in 0.1 M KOH + 0.6 M NaCl, it achieved 76.5 mA cm at a potential of 1.6 V relative to the reversible hydrogen electrode (RHE). -2 This is similar to the current density of the catalyst prepared on a small scale.

[0103] Following the same procedure (keeping the total metal content at 4 mmol and melamine at 30 g), samples including Ni@NC, NF@NC (Ni:Fe=9:1), NFW@NC (Ni:Fe:W=1.8:0.2:0.7) and CFW@NC (Co:Fe:W=1:1:0.7) were also successfully prepared. In alkaline simulated seawater, they all showed superior OER activity and corrosion resistance to RuO2 ( Fig.32 ). Therefore, this preparation strategy is a general approach to synthesize ion-selective catalysts for efficient and stable seawater decomposition catalysis.

[0104] In summary, the present invention proposes to combine efficient chloride ion screening and selective oxygen evolution reaction (OER) catalysis to design an efficient CoFe@NC catalyst that can operate stably in direct seawater electrolysis. This robust ion-selective OER catalyst consists of a conductive metal core, an ion-screening metal, and a nitrogen-doped catalytic carbon shell. The electrons of the conductive metal core can pass through the carbon layer, adjust the electronic structure of the interfacial active sites, and enhance its OER catalytic activity. At the same time, the nitrogen-doped carbon outer layer rich in ultra-micropores of about 0.34 nm is very sensitive to OH - It has a significant size screening effect, thus hindering the Cl - to the interfacial carbon layer and the metal alloy core, and further prevent Cl - The species accelerates oxygen corrosion through depassivation reactions. In addition, the CoFe-N4-C group can optimize the adsorption strength of the intermediates, giving the catalyst excellent activity and selectivity (99.5%) for OER. -2 At a current density of 1.5 Å (three-electrode configuration), the CoFe55@NC catalyst drove the OER for 2000 h without structural damage, and the assembled monolithic seawater electrolyzer (Φ18 cm) stably outputted 3000 A m at a low voltage of about 1.85 V. -2 The high current density of CoFe@NC was over 330 h. In addition, the preparation of CoFe@NC can be easily scaled up to 100 g level. The easy scalability and excellent long-term stability of this ion-selective catalyst make it promising for a wide range of applications and may promote the industrialization of seawater electrolysis.

[0105] The above is only a preferred implementation of the patent of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the patent of the present invention. These improvements and modifications should also be regarded as the scope of protection of the patent of the present invention.

Claims

1. A CoFe@NC core-shell structure catalyst, comprising a core and an outer shell, characterized in that: The core is CoFe alloy, and the shell is a carbon material co-doped with N, Co, and Fe elements. x -C coordination structure and Fe-N x -C coordination structure.

2. The CoFe@NC core-shell structure catalyst according to claim 1, characterized in that The shell has a thickness of 5-50 nm and has a microporous structure with a microporous diameter ranging from 0.1-0.7 nm.

3. The CoFe@NC core-shell structure catalyst according to claim 1, characterized in that In the catalyst, the molar ratio of Co to Fe is 1:(0.5-2.5).

4. The method for preparing the CoFe@NC core-shell structure catalyst according to any one of claims 1 to 3, characterized in that: The steps include: S1, dissolving a cobalt source, an iron source, and a nitrogen-containing carbon source in a solvent, stirring evenly, and evaporating the solvent to obtain a precursor; S2. calcining the precursor to obtain a catalyst.

5. The method for preparing the CoFe@NC core-shell structure catalyst according to claim 4, characterized in that: The cobalt source is one or a mixture of cobalt nitrate, cobalt chloride, cobalt sulfate, and cobalt citrate; The iron source is one or a mixture of ferric nitrate, ferric oxide, ferric sulfate, and ferric citrate; The nitrogen-containing carbon source is selected from melamine.

6. The method for preparing the CoFe@NC core-shell structure catalyst according to claim 4, characterized in that: The molar ratio of Co in the cobalt source to Fe in the iron source is 1:(0.5-2.5); The added amounts of the cobalt source, iron source, and nitrogen-containing carbon source are calculated based on the total added molar amount of Co and Fe and the added amount of the nitrogen-containing carbon source: (2-5)mmol:(10-50)g.

7. The method for preparing the CoFe@NC core-shell structure catalyst according to claim 4, characterized in that: The calcination conditions are: in nitrogen or inert atmosphere, heating to 700-950°C at 3-8°C / min and keeping warm for 1.5-3h.

8. Use of the CoFe@NC core-shell structure catalyst according to any one of claims 1 to 3 in hydrogen production by seawater electrolysis.

9. The use according to claim 8, characterized in that: The loading amount of CoFe@NC core-shell catalyst on the electrode surface is 3-12 mg cm -2 .

10. A method for predicting the OER selectivity of a core-shell catalyst, characterized in that: The process includes the following steps: constructing the catalyst chemical structure and then calculating the electrode potential difference between the chlorine evolution reaction (CER) and the oxygen evolution reaction (OER) by DFT. The catalyst with the highest electrode potential difference △U is taken as the catalyst with the best OER selectivity.