Catalyst with C-O-M chlorine corrosion resistance site, preparation method of catalyst and application of catalyst in electrolyzed water and seawater
The C-O-M anti-chlorine corrosion site oxygen-excitation reaction electrocatalyst prepared by hydrothermal reaction uses the coordination of carboxylic organic molecules with transition metals to solve the corrosion problem of Cl-on-in-sea water catalyst, and achieves efficient anti-chlorine corrosion performance and stability, providing an inexpensive and easy-to-access electrocatalyst suitable for electrolyzing water and seawater electrolysis.
Patent Information
- Application Number
- CN202411064210.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
AI Technical Summary
The structure of the high concentration of Cl-corrosive electrolytic water anode catalyst in seawater leads to a decrease in its activity and stability, hindering the efficiency of electrolytic seawater technology. The existing preparation methods for anti-chlorine corrosion catalysts are complex and costly.
The oxygen evolution reaction electrocatalyst with C-O-M anti-chlorine corrosion sites was prepared by hydrothermal reaction, and the C-O-M anti-chlorine corrosion site was coordinated with the transition metal (Ni, Fe, Cu, Co) was used to form a C-O-M anti-chlorine corrosion site, preventing Cl- from approaching catalysis Center, simple preparation method and low cost.
It realizes efficient anti-chlorine corrosion performance in electrolytic water and seawater, reduces the overpotential of the catalyst, improves the stability and activity of the catalyst, provides a cheap and easy-to-get electrocatalyst, and solves the chloride ions in seawater electrolysis. Poisoning problem.
Smart Images

Figure CN118932407A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts, and in particular relates to a catalyst with COM chlorine corrosion resistance sites, a preparation method thereof, and application in electrolysis of water and seawater. Background Art
[0002] Developing clean and renewable energy is an inevitable way to promote sustainable social development. Water electrolysis hydrogen production technology is considered an effective technical means to develop clean energy due to its simple process and high purity of produced hydrogen.
[0003] Compared with scarce freshwater resources, seawater is considered to be an ideal substitute due to its abundant resources and can achieve large-scale production of green hydrogen. Unfortunately, the high concentration of Cl in seawater - (about 0.5M) will corrode the structure of the electrolytic water anode catalyst, causing the activity and stability of the catalyst to drop sharply, seriously hindering the electrolytic water efficiency. Therefore, the key to seawater electrolysis technology is to design and construct an anode electrocatalyst that is resistant to chlorine corrosion.
[0004] The patent with publication number CN 115418667 A published on December 2, 2022 discloses a manganese oxide film-coated hydrotalcite-like nanosheet seawater oxidation electrocatalyst and its preparation method. The NiFe-LDH nanosheet array covered with an ultra-thin MnOx film is directly assembled on nickel foam by hydrothermal and electrodeposition, denoted as MnO x / NiFe-LDH / NF. The catalyst exhibited excellent selective OER activity in alkaline seawater electrolyte. x / NiFe-LDH / NF has better oxygen evolution performance and chlorine corrosion resistance than NiFe-LDH / NF. The good OER selectivity and catalytic performance are attributed to the MnO x The thin film layer selectively blocks Cl - Approaching the catalytic center and electrodeposition of MnO x The oxygen vacancies generated in the MnO layer, good conductivity, fast kinetics and abundant active sites. x The film layer can also effectively inhibit Cl - It can prevent the catalyst from leaking and improve the corrosion resistance and stability of the catalyst. However, its preparation method is complicated and the cost is high. Summary of the invention
[0005] The object of the present invention is to provide a catalyst with COM chlorine corrosion resistant sites and a preparation method thereof. An oxygen evolution reaction electrocatalyst with COM corrosion resistant sites is prepared by a hydrothermal reaction. In the catalyst, COM chlorine corrosion resistant sites are formed due to the coordination of carboxyl functional groups in carboxyl organic molecules with transition metals (Ni, Fe, Cu and Co, etc.); the product has a uniform morphology and a flaky structure, and the preparation method of the present invention is simple and low in cost.
[0006] Another object of the present invention is to provide a catalyst having COM chlorine corrosion resistant sites for use in electrolysis of water or seawater. The product has COM chlorine corrosion resistant sites and the COM sites hinder the poisoning of metal sites by chloride ions due to the mutual repulsion of electronegativity, and can be used for seawater electrolysis.
[0007] The specific technical solutions of the present invention are as follows:
[0008] A method for preparing a catalyst having COM chlorine corrosion resistant sites, specifically comprising:
[0009] The oxygen evolution reaction electrocatalyst and the organic matter containing carboxyl group are mixed in a solvent, and heated to react to obtain a catalyst having COM chlorine corrosion resistance site.
[0010] The oxygen evolution reaction electrocatalyst is an oxygen evolution reaction electrocatalyst containing one or more of metal nickel, iron, cobalt or copper; preferably, the oxygen evolution reaction electrocatalyst is a nickel foam-supported NiFe LDH catalyst, a nickel foam-supported NiFeCo LTH catalyst or an iron foam-supported NiFeCu LTH catalyst.
[0011] The oxygen evolution reaction electrocatalyst and the solvent are used in a ratio of 0.1-100 mg / mL;
[0012] The solvent is a mixed solvent of water and alcohol in any proportion; the alcohol is selected from any one or more of methanol, ethanol or ethylene glycol; and the water is preferably pure water.
[0013] The carboxyl-containing organic matter is selected from one or more of sodium tartrate, sodium malate, sodium citrate or sodium salicylate;
[0014] The mass ratio of the carboxyl-containing organic matter to the oxygen evolution reaction electrocatalyst is 1:1-45:1;
[0015] The heating reaction refers to reacting at 80-160°C for 4-48 hours;
[0016] Furthermore, after the hydrothermal reaction is completed, the precipitate is cooled and separated, the precipitate is first washed with water, then washed with alcohol, and vacuum dried at 30-60° C. to constant weight, thereby obtaining a catalyst having COM chlorine corrosion resistance sites.
[0017] The present invention provides a catalyst with COM chlorine corrosion resistant sites, which is prepared by the above method. The catalyst with COM chlorine corrosion resistant sites is mutually stacked nanosheets with a width of 300nm-700nm. M is one or more of Ni, Fe, Cu or Co;
[0018] The present invention provides a catalyst with COM sites that are resistant to chlorine corrosion and is used in electrolysis of water or seawater. In a 1.0M KOH solution, the catalyst with COM sites that are resistant to chlorine corrosion reaches 300 mA·cm -2 The overpotential is between 200-330 mV vs. RHE; in 1.0 M KOH + seawater medium, it reaches 300 mA cm -2 The overpotential of the catalyst is between 260-450 mV vs. RHE. In addition, due to the effect of the COM bond, the overpotential of the catalyst with chlorine-resistant COM sites is reduced by 10-100 mV in 1.0 M KOH and 1.0 M KOH + seawater, respectively, compared with the catalyst without chlorine corrosion resistance.
[0019] The present invention uses carboxyl organic molecules as structural units, and couples carboxyl organic molecules with Ni, Fe, Cu or Co through hydrothermal reaction to obtain carboxyl anchored metal (COM, C is carbon element, O is oxygen element, M represents metal, specifically Ni, Fe, Cu or Co) catalysts. Due to the regulatory effect of carboxyl groups on the electronic structure of active sites, the material exhibits excellent oxygen evolution activity and excellent corrosion resistance. Carboxyl organic molecules are cheap and easy to obtain. Under hydrothermal conditions, the carboxyl functional groups in carboxyl organic molecules are easy to coordinate with metal ions (iron, nickel, cobalt and copper, etc.), so that the electronic structure of the metal active sites in the target material changes, which is conducive to the adsorption and desorption of oxygen active species, and the organic electrostatic repulsion of COM bonds in the corrosion-resistant sites can effectively hinder the poisoning effect of chloride ions. The present invention uses carboxyl organic molecules as structural units to modify transition metal-based electrocatalysts, replacing traditional noble metal catalysts, and provides a cheap, easy-to-obtain electrocatalyst with outstanding electrocatalytic activity for the electrolysis of water and oxygen evolution reaction.
[0020] Compared with the prior art, the present invention is prepared under hydrothermal conditions, and the carboxyl organic molecules are easy to react with transition metals (Ni, Fe, Cu and Co, etc.) to improve the electronic structure of the metal site, which is beneficial to the adsorption and desorption of oxygen active species. The anti-corrosion site COM can effectively hinder the poisoning effect of chloride ions on the active site due to the electrostatic repulsion. The preparation method is simple, the morphology is uniform, and it has excellent electrocatalytic activity for oxygen evolution reaction. The application of the present invention in the field of water electrolysis and seawater electrolysis can provide a practical idea for solving the increasingly serious energy crisis and environmental pollution problems. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the X-ray powder diffraction XRD pattern of the catalyst having COM (M = Ni and Fe) sites obtained in Example 1;
[0022] Figure 2 This is a scanning electron microscope photograph of the catalyst having COM (M = Ni and Fe) sites obtained in Example 1;
[0023] Figure 3 The Ni L-edge absorption spectra of the catalysts with COM (M = Ni and Fe) sites and without COM (M = Ni and Fe) sites obtained in Example 1;
[0024] Figure 4 Fe L-edge absorption spectra of the catalysts with COM (M = Ni and Fe) sites and without COM (M = Ni and Fe) sites obtained in Example 1;
[0025] Figure 5 The LSV curve of the oxygen evolution reaction of the catalyst having COM (M = Ni and Fe) sites in 1.0 M KOH obtained in Example 1;
[0026] Figure 6 This is the LSV curve of the oxygen evolution reaction of the catalyst with COM (M = Ni and Fe) sites obtained in Example 1 in 1.0 M KOH + seawater.
[0027] Figure 7 The LSV curve of the oxygen evolution reaction of the catalyst without COM (M = Ni and Fe) sites obtained in Example 1;
[0028] Figure 8 This is the LSV curve of the oxygen evolution reaction of the catalyst without COM (M = Ni and Fe) sites obtained in Example 1 in 1.0 M KOH + seawater. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0031] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0032] Example 1
[0033] A method for preparing a NiFe LDH oxygen evolution reaction electrocatalyst having COM (M=Fe, Ni) chlorine corrosion resistant sites, comprising the following steps:
[0034] A. Preparation of NiFe LDH catalyst: 0.6 mmol NiCl2·6H2O, 0.2 mmol FeCl3·6H2O, 200 mg urea and 2.5×0.5 cm nickel foam were added to a mixed solution of 15 mL ethylene glycol and water in a volume ratio of 1:1 and stirred for 20 min; the mixed solution was transferred to a hydrothermal reactor and reacted at 120°C for 12 h to obtain a NiFe LDH catalyst supported on nickel foam.
[0035] B. Dispersion: Add 2 mg NiFe LDH catalyst supported by nickel foam and 0.15 mmol sodium tartrate into 15 mL pure water and stir for 10 min, then transfer all to a hydrothermal reactor and react at 120 °C for 10 h;
[0036] C. Drying: The system after the reaction is cooled and separated, the precipitate is first washed with water, then with alcohol, and then vacuum dried at 40°C to constant weight, thus obtaining an oxygen evolution reaction catalyst with COM resistance to chlorine corrosion, the XRD pattern of which is as follows: Figure 1 As shown, its diffraction peak corresponds to the standard card JCPDS No.51-0463 of NiFeLDH, and the catalyst is a 300nm-700nm flake structure ( Figure 2 ), labeled as CO-NiFe. The raw materials used in this experimental method are simple and easy to obtain, and the reaction temperature is low and the procedure is simple. At the same time, synchrotron radiation tests showed that sodium tartrate improved the electrochemical behavior of oxygen active species ( Figure 3 and Figure 4 ), thereby improving the electrochemical behavior of *OH, *O, and *OOH oxygen active species.
[0037] The application of the NiFe LDH oxygen evolution reaction electrocatalyst having COM (M=Fe, Ni) chlorine corrosion resistant sites prepared in Example 1 is specifically as follows:
[0038] First, the prepared CO-NiFe was inserted into a 1.0 M KOH solution with an area of 1.0 cm × 1.0 cm, and the electrocatalytic process of the oxygen evolution reaction was recorded using an electrochemical workstation in a potential window of 1.2 to 1.55 V vs. RHE. It can be seen that when the current density reaches 300 mA cm -2When the overpotential is only 270mV vs.RHE, see Figure 5 ;
[0039] Secondly, the prepared CO-NiFe was inserted into a 1.0M KOH + seawater solution with an area of 1.0cm×1.0cm, and an electrochemical workstation was used to record the electrocatalytic process of oxygen evolution reaction in the potential window of 1.2-1.55V vs.RHE. It can be seen that when the current density reaches 300mA·cm -2 When the overpotential is only 285mV vs.RHE, see Figure 6 .
[0040] The above-mentioned nickel foam-supported NiFe LDH catalyst is used as a catalyst for the electrocatalytic reaction of oxygen evolution reaction:
[0041] First, the prepared NiFe LDH was inserted into a 1.0 M KOH solution with an area of 1.0 cm × 1.0 cm, and an electrochemical workstation was used to record the electrocatalytic process of oxygen evolution reaction in the potential window of 1.2 to 1.70 V vs. RHE. It can be seen that when the current density reaches 300 mA cm -2 When the overpotential is only 425mV vs.RHE, see Figure 7 ;
[0042] Next, NiFe LDH was inserted into 1.0 M KOH + seawater (1.0 cm × 1.0 cm), and an electrochemical workstation was used to record the electrocatalytic process of oxygen evolution reaction in the potential window of 1.2 to 1.73 V vs. RHE. It can be seen that when the current density reaches 300 mA cm -2 When the overpotential is only 474mV vs.RHE, see Figure 8 .
[0043] Example 2
[0044] A method for preparing a NiFeCo LTH oxygen evolution reaction electrocatalyst having COM (M = Ni, Fe, Co) chlorine corrosion resistant sites, comprising the following steps:
[0045] A. Preparation of NiFeCo LTH catalyst: 0.6 mmol NiCl2·6H2O, 0.2 mmol FeCl3·6H2O, 0.05 mmol CoCl3·6H2O, 200 mg urea and 2.5×0.5 cm2 nickel foam were added to a mixed solution of 15 mL ethylene glycol and water in a volume ratio of 1:1 and stirred for 20 min; the mixed solution was transferred to a hydrothermal reactor and reacted at 120°C for 12 h to obtain a NiFeCo LTH catalyst supported on nickel foam.
[0046] B. Dispersion: Add 3.0 mg NiFeCo LTH catalyst supported by nickel foam and 0.05 mmol sodium malate to a mixed solution of 7 mL pure water and 8 mL ethylene glycol and stir for 10 min. Then transfer all of the mixture to a hydrothermal reactor and react at 120 °C for 12 h.
[0047] C. Drying: The system after the reaction is cooled and separated, and the precipitate is first washed with water and then with alcohol, and then vacuum dried at 40°C to constant weight to obtain NiFeCo LTH with corrosion-resistant sites, and the NiFeCo double metal hydroxide is a flaky structure, marked as CO-NiFeCo.
[0048] Example 2: Electrocatalytic reaction of CO-NiFeCo LTH as catalyst for oxygen evolution reaction:
[0049] First, the prepared CO-NiFeCo was inserted into a 1.0M KOH solution with an area of 1cm×1cm, and the electrocatalytic process of the oxygen evolution reaction was recorded using an electrochemical workstation in a potential window of 1.2 to 1.55V vs. RHE. It can be seen that when the current density reaches 300mA·cm -2 Its overpotential is only 280mV vs.RHE;
[0050] The prepared CO-NiFeCo was inserted into 1.0M KOH + seawater 1cm×1cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2~1.55V vs.RHE. It can be seen that when the current density reaches 300mA·cm -2 Its overpotential is only 295mV vs.RHE.
[0051] The NiFeCo LTH used in Example 2 was used as a catalyst for the electrocatalytic reaction of water oxidation:
[0052] First, the prepared NiFeCo LTH was inserted into 1.0M KOH 1.0cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2~1.75V vs.RHE. It can be seen that when the current density reaches 300mA·cm -2 Its overpotential is only 420mV vs.RHE;
[0053] The prepared NiFeCo LTH was inserted into a 1.0M KOH + seawater solution with an area of 1cm×1cm, and an electrochemical workstation was used to record the electrocatalytic process of oxygen evolution reaction in the potential window of 1.2-1.75V vs. RHE. It can be seen that when the current density reaches 300mA·cm -2Its overpotential is only 460mVvs.RHE.
[0054] Example 3
[0055] A method for preparing a NiFeCu LTH oxygen evolution reaction electrocatalyst having COM (M = Ni, Fe, Cu) chlorine corrosion resistant sites, comprising the following steps:
[0056] A. Preparation of NiFeCu LTH catalyst: 0.6 mmol NiCl2·6H2O, 0.2 mmol FeCl3·6H2O, 0.05 mmol CuCl2·6H2O, 200 mg urea and 2.5×0.5 cm nickel foam were added to a mixed solution of 15 mL ethylene glycol and water in a volume ratio of 1:1 and stirred for 20 min; the mixed solution was transferred to a hydrothermal reactor and reacted at 120°C for 12 h to obtain a NiFeCu LTH catalyst supported on nickel foam.
[0057] B. Dispersion: Add 2 mg NiFeCu LTH catalyst supported by foam iron and 0.3 mmol sodium salicylate to a mixed solution of 8 mL pure water and 7 mL ethylene glycol and stir for 10 min, then transfer all to a hydrothermal reactor and react at 100 °C for 18 h;
[0058] C. Drying: The system after the reaction is cooled and separated, and the precipitate is first washed with water and then with alcohol, and then dried in vacuum at 40°C to constant weight, i.e., NiFeCu LTH modified with sodium salicylate, marked as CO-NiFeCu LTH.
[0059] The CO-NiFeCu LTH obtained in Example 3 was used as a catalyst for the electrocatalytic reaction of oxygen evolution reaction:
[0060] First, the prepared CO-NiFeCu LTH was inserted into 1.0M KOH with an area of 1.0cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2-1.55V vs.RHE. It can be seen that when the current density reaches 300mA·cm -2 Its overpotential is only 300mV vs.RHE;
[0061] The prepared CO-NiFe LTH was inserted into a 1.0M KOH + seawater solution with an area of 1cm×1cm, and an electrochemical workstation was used to record the electrocatalytic process of oxygen evolution reaction in the potential window of 1.2-1.54V vs.RHE. It can be seen that when the current density reaches 300mA·cm -2 Its overpotential is only 315mV vs.RHE.
[0062] The NiFeCu LTH used in Example 3 was used as a catalyst for the electrocatalytic reaction of oxygen evolution reaction:
[0063] First, the prepared NiFeCu LTH was inserted into 1.0M KOH 1.0cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2~1.75V vs.RHE. It can be seen that when the current density reaches 300mA·cm -2 Its overpotential is only 410mV vs.RHE;
[0064] The prepared NiFeCu LTH LDH was inserted into 1.0M KOH + seawater 1.0cm×1.0cm, and the electrocatalytic process of oxygen evolution reaction was recorded by an electrochemical workstation in the potential window of 1.2-1.75V vs. RHE. It can be seen that when the current density reaches 300mA·cm -2 Its overpotential is only 450mV vs.RHE.
[0065] Comparative Example 1
[0066] A method for preparing a NiFe LDH oxygen evolution reaction electrocatalyst having excessive COM (M=Fe, Ni) chlorine corrosion resistant sites, comprising the following steps:
[0067] A. Preparation of NiFe LDH catalyst: 0.6 mmol NiCl2·6H2O, 0.2 mmol FeCl3·6H2O, 200 mg urea and 2.5×0.5 cm nickel foam were added to a mixed solution of 15 mL ethylene glycol and water in a volume ratio of 1:1 and stirred for 20 min; the mixed solution was transferred to a hydrothermal reactor and reacted at 120°C for 12 h to obtain a NiFe LDH catalyst supported on nickel foam.
[0068] B. Dispersion: Add 2 mg NiFe LDH catalyst supported by nickel foam and 0.6 mmol sodium tartrate into 15 mL pure water and stir for 10 min, then transfer all to a hydrothermal reactor and react at 120 °C for 10 h;
[0069] C. Drying: Cool and separate the system after the reaction, wash the precipitate with water first, then with alcohol, and dry it in vacuum at 40°C to constant weight, thereby obtaining an oxygen evolution reaction catalyst having transition COM chlorine corrosion resistant sites.
[0070] The application of the NiFe LDH oxygen evolution reaction electrocatalyst having COM (M = Fe, Ni) chlorine corrosion resistant sites prepared in Comparative Example 1 is specifically as follows:
[0071] First, the prepared CO-NiFe was inserted into a 1.0 M KOH solution with an area of 1.0 cm × 1.0 cm, and the electrocatalytic process of the oxygen evolution reaction was recorded using an electrochemical workstation in a potential window of 1.2 to 1.75 V vs. RHE. It can be seen that when the current density reaches 300 mA cm -2 Its overpotential is as high as 460mVvs.RHE. The main reason is that too many carboxyl molecules will cause the activity to deteriorate, and too many COM sites will repel the adsorption of oxygen active species on the sites, resulting in a decrease in catalyst activity.
[0072] The carboxyl organic molecules in the present invention can optimize the electronic structure of the metal site of the active site, and the COM site formed by the coordination of the carboxyl organic molecules and the metal blocks the damage of chloride ions to the structure of the nanomaterial due to the electrostatic repulsion effect; by controlling the amount of the carboxyl organic molecules, the regulating effect and electrostatic repulsion effect on the electronic structure of the active site are optimized, the adsorption of oxygen active species is optimized, the reaction barrier of the rate-determining step of the oxygen evolution reaction is reduced, and the poisoning of the active site by chloride ions is hindered.
[0073] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a catalyst having COM chlorine corrosion resistant sites, characterized in that: The preparation method is specifically: The oxygen evolution reaction electrocatalyst and the organic matter containing carboxyl group are mixed in a solvent, and heated to react to obtain a catalyst having COM chlorine corrosion resistance site.
2. The preparation method according to claim 1, characterized in that: The oxygen evolution reaction electrocatalyst is an oxygen evolution reaction electrocatalyst containing one or more of metal nickel, iron, cobalt or copper.
3. The preparation method according to claim 1 or 2, characterized in that: The oxygen evolution reaction electrocatalyst is a NiFe LDH catalyst supported by nickel foam, a NiFeCo LTH catalyst supported by nickel foam, or a NiFeCu LTH catalyst supported by iron foam.
4. The preparation method according to claim 1 or 2, characterized in that: The amount ratio of the oxygen evolution reaction electrocatalyst to the solvent is 0.1-100 mg / mL.
5. The preparation method according to claim 1 or 4, characterized in that: The solvent is a mixed solvent of water and alcohol in any proportion.
6. The preparation method according to claim 1, characterized in that: The carboxyl-containing organic matter is selected from one or more of sodium tartrate, sodium malate, sodium citrate or sodium salicylate.
7. The preparation method according to claim 1 or 6, characterized in that: The mass ratio of the organic matter containing carboxyl groups to the oxygen evolution reaction electrocatalyst is 1:1-45:
1.
8. The preparation method according to claim 1, characterized in that: The heating reaction refers to reacting at 80-160° C. for 4-48 hours.
9. A catalyst having COM chlorine corrosion resistant sites prepared by the preparation method according to any one of claims 1 to 8.
10. An application of a catalyst having COM chlorine corrosion resistant sites according to claim 9, characterized in that: Application in electrolysis of water or seawater.
Citation Information
Patent Citations
Manganese oxide film coated hydrotalcite-like nanosheet seawater oxidation electrocatalyst and preparation method thereof
CN115418667A