Method for recovering lithium, iron and phosphorus from lithium iron phosphate waste by using molten salt electrolysis and high-purity lithium phosphate
Through molten salt electrolysis technology, the recycling of lithium iron phosphate waste in an inert atmosphere has solved the problem of complex and high energy consumption in the existing process, and the recycling of high-purity lithium phosphate and metal iron is achieved, reducing waste emissions and energy consumption, and promoting resources sustainable use.
Patent Information
- Application Number
- CN202411166454.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing lithium iron phosphate recycling process is complex, has high energy consumption, and produces a large amount of acid and alkali waste, which affects environmental sustainability.
Using molten salt electrolysis technology combined with electrochemical technology, LiCl-MCl molten salt system electrolyzes lithium iron phosphate waste under an inert atmosphere, achieving the recycling of high-purity lithium phosphate and metal iron, avoiding the use of acid and alkali reagents and reducing energy consumption and waste emissions.
It has achieved efficient and environmentally friendly recycling of lithium phosphate and metal iron, improved product purity and economic benefits, reduced resource waste and waste emissions, and promoted the establishment of a recycling model.
Smart Images

Figure CN118932430A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery material technology, and in particular to a method for recovering lithium, iron, and phosphorus from lithium iron phosphate waste using molten salt electrolysis and high-purity lithium phosphate. Background Art
[0002] Lithium-ion batteries (LIBs) play an indispensable role in the rapid growth of electrified transportation and storage of renewable energy. Due to the limited lifespan of lithium-ion batteries, a large number of retired waste batteries will endanger the sustainability of resources and cause environmental pollution. Therefore, recycling of discarded lithium batteries has become an important step in the entire battery supply chain. Lithium iron phosphate (LiFePO4, LFP) is widely used as a battery material due to its low preparation cost, high safety and good cycle performance. Recycling of spent LFP batteries is necessary.
[0003] At present, the main methods for recycling lithium iron phosphate are pyrometallurgy and wet recycling processes. Since the structure of LiFePO4 is very stable, it is difficult to recover the Li element through pyrometallurgy, and pyrometallurgy and wet recycling processes are usually used in combination. The wet recycling process uses inorganic acids (sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid) and oxidants to selectively extract Li or completely dissolve it in an acid solution. The wet recycling process has the advantages of high metal leaching and high recycling efficiency, but the wet recycling process has the disadvantages of large acid and alkali consumption and large wastewater and waste gas treatment volume.
[0004] The existing technology uses hot acid leaching to obtain iron phosphate by oxygen pressure hydrothermal leaching, and then separates lithium salts through alkaline precipitation. Although this process separates lithium salts and iron phosphate, it is complicated and requires a large amount of acid and alkali oxidants and additives, with a large amount of wastewater treatment and high energy consumption. Therefore, it is necessary to develop a green and efficient lithium iron phosphate leaching system to reduce waste emissions and energy consumption. Summary of the invention
[0005] In view of this, the present application provides a method for recovering lithium, iron, and phosphorus from lithium iron phosphate waste using molten salt electrolysis and high-purity lithium phosphate. The present application combines a chloride molten salt system with an electrochemical process to achieve the recovery of high-purity lithium phosphate and metallic iron. The process has high electrolysis efficiency, strong process operability, and does not involve the use of any acid or alkali reagents, and is a green and environmentally friendly innovative process. In particular, during the electrolysis process, the method of the present application can convert low-purity LiCl into high-purity Li3PO4, thereby improving product purity while recycling waste and improving economic benefits.
[0006] In a first aspect, the present application provides a method for recovering lithium, iron and phosphorus from lithium iron phosphate waste by molten salt electrolysis, the method comprising: S100, obtaining LiCl-MCl molten salt, the LiCl-MCl molten salt being in a molten state, adding lithium iron phosphate waste into the LiCl-MCl molten salt, and electrolyzing under an inert atmosphere to obtain a product metallic iron a attached to a cathode plate, an anode product and a molten salt electrolyte, wherein the molten salt electrolyte comprises Li3PO4 and metallic iron b fallen off from the cathode plate; S200, filtering the molten salt electrolyte to obtain a filter residue containing Li3PO4 and metallic iron b, and a filtrate; S300, placing the filter residue in water, magnetically attracting and washing it, to obtain high-purity lithium phosphate and metallic iron b, wherein M is selected from at least one of Na element and K element. The present application uses LiCl-KCl / NaCl molten salt as the reaction system, and utilizes high-temperature molten salt (molten state) to electrolyze and recover lithium iron phosphate. The whole process does not consume acid and alkali, which is more environmentally friendly than traditional wet treatment. At the same time, it can ensure the efficient recovery of Li, Fe, and P elements. It can be seen that the present application can convert waste lithium iron phosphate waste resources into high-purity lithium phosphate and metallic iron that can be recycled resources by combining molten salt with electrolysis, which is helpful to establish a circular recycling model, reduce resource waste and waste emissions, and realize resource conservation and utilization. In addition, during the electrolysis process, the present application can convert low-purity LiCl into high-purity Li3PO4, thereby achieving the purification effect of LiCl and improving economic benefits.
[0007] In this process, oxygen must be isolated from the electrolysis process, that is, electrolysis must be carried out in an oxygen-free atmosphere, such as in an inert atmosphere, because during the electrolysis process, the cathode produces metallic iron. When oxygen is present, oxidation reaction will inevitably occur to produce iron oxide, which affects the purity of the product Li3PO4. The reactions involved are as follows:
[0008] i) Cathode reaction Fe 2+ +2e - →Fe;
[0009] ii) Anode reaction 2Cl - -2e - →Cl2;
[0010] iii) Overall reaction LiFePO4+2LiCl→Fe+Li3PO4+Cl2↑.
[0011] In some embodiments, in step S100, obtaining the LiCl-MCl molten salt includes: heating a material containing LiCl and a material containing MCl at 350°C to 800°C to obtain a molten LiCl-MCl molten salt, wherein the molar ratio of LiCl to MCl in the LiCl-MCl molten salt is K, and 0.15≤K≤4.0. Preferably, 1.6≤K≤1.9. The present application heats the molten salt to a molten state by high temperature, and when the molten salt reaches a molten state, lithium iron phosphate waste is added. At this time, the lithium iron phosphate structure is broken to form Li + , Fe 2+ PO4 3- The ions exist in the molten salt and are electrolyzed to make Li + and PO4 3- Combined to generate Li3PO4. Regulating the molar ratio K of LiCl and MCl within a suitable range can not only make lithium iron phosphate waste more soluble, improve the recovery rate of Fe and Li / P, but also reduce the electrolysis temperature.
[0012] In some embodiments, in the material containing LiCl, the purity of LiCl is 80wt% to 95wt%, and the impurities in the material containing LiCl include at least one of NaCl, KCl, MgCl2, CaCl2, and AlCl3. The present application further regulates the purity of LiCl in the material containing LiCl within the above range, which is conducive to improving the electrolysis efficiency during electrolysis and obtaining high-purity Li3PO4 with low energy consumption. If the purity of LiCl in the material containing LiCl is too low (for example, less than 80%), it will lead to excessive impurities in the molten salt, affecting the properties of the molten salt. On the one hand, it is not conducive to the complete breaking of the structure of lithium iron phosphate waste, resulting in a decrease in the recovery rate of Fe and Li / P, and affecting the purity of the product Li3PO4. On the other hand, too many impurities in the molten salt will require a higher melting temperature and electrolysis temperature, affecting the electrolysis efficiency and increasing energy consumption.
[0013] In some embodiments, in step S100, the mass ratio of LiCl-MCl molten salt to lithium iron phosphate waste is (2-30):1. Preferably, the mass ratio of LiCl-MCl molten salt to lithium iron phosphate waste is (8-30):1. LiCl in the LiCl-MCl molten salt participates in the electrolysis reaction as a reactant, i.e., Li + and PO4 3- In the process of combining to form Li3PO4, one Li + From LiFePO4 (lithium iron phosphate waste), two parts of Li + From LiCl. Molten salt plus electrolysis can not only realize the recovery of LiFePO4, but also convert low-purity LiCl into high-purity Li3PO4, which belongs to the process of Li purification and maximizes economic benefits.
[0014] In some embodiments, in step S100, the mass percentage of LiFePO4 in the lithium iron phosphate waste is W%, 95%≤W%≤100%. The lithium iron phosphate waste contains only a small amount of carbon and organic matter, and the LFP content of some wastes after treatment (such as roasting) can be defaulted to 100%.
[0015] In some embodiments, in step S100, the electrolysis conditions include: electrolysis temperature: 350°C to 800°C, electrolysis voltage: 2.0V to 4.0V. The electrolysis temperature is related to the melting temperature of the molten salt. By regulating the molar ratio K of LiCl and MCl in a preferred range (1.6≤K≤1.9), the electrolysis temperature can be further reduced to 350°C to 500°C, thereby achieving low-temperature electrolysis, reducing energy consumption, and taking into account the high recovery rate of Fe and Li / P and obtaining a high-purity Li3PO4 product.
[0016] In some embodiments, in step S100, the anode product includes chlorine gas, which is enriched by a collection device and is an additional economic income.
[0017] In some embodiments, in step S200, the filtrate contains molten LiCl and MCl, and the filtrate is returned to step S100 to continue molten salt electrolysis of the lithium iron phosphate waste. The filtrate contains molten LiCl and MCl, which are circulated to step S100 to continue dissolving lithium iron phosphate, thereby achieving an overall cycle.
[0018] In some embodiments, in step S200, the filtration is high temperature filtration, and the temperature of the high temperature filtration is 350° C. to 550° C. The high temperature filtration is to prevent the molten salt from cooling, and after the high temperature filtration, a filtrate containing molten LiCl and MCl and a filter residue containing Li3PO4 and metallic iron b are obtained, which ensures a high recovery rate of Fe and Li / P and a high purity of Li3PO4.
[0019] In some embodiments, the yield of metallic iron a is greater than the yield of metallic iron b. In the present application, the product metallic Fe is recovered by two parts, most of which is metallic iron a of the cathode product, and a small part is metallic iron b in the electrolyte. The mass of metallic iron a and the mass of metallic iron b are combined and then calculated to obtain the recovery rate of Fe, wherein the metallic iron b in the electrolyte is detached from the cathode.
[0020] In some embodiments, the high purity lithium phosphate has a purity greater than or equal to 99%.
[0021] In a second aspect, the present application provides high-purity lithium phosphate prepared by any one of the methods in the first aspect, wherein the purity of the high-purity lithium phosphate is greater than or equal to 99%.
[0022] This patent proposes a method for recovering lithium, iron and phosphorus from lithium iron phosphate waste by molten salt electrolysis, involving LiCl-KCl / NaCl molten salt, which has the following advantages over the traditional wet process:
[0023] 1. This application combines the technical advantages of molten salt and electrochemistry to melt lithium iron phosphate waste and then electrolyze and recycle it. The process uses a chloride molten salt system, has strong process operability, and is a green and environmentally friendly innovative process;
[0024] 2. The process does not involve any acid or alkali, reduces the use of chemical reagents, reduces energy consumption, does not generate any waste, and does not cause environmental pollution. At the same time, the electrolysis efficiency in the molten salt system can be greatly improved, achieving low energy consumption, and can realize the recycling of lithium iron phosphate;
[0025] 3. This process converts low-purity LiCl into high-purity Li3PO4 during the electrolysis process, thereby improving product purity while recycling waste and improving economic benefits;
[0026] 4. The technology of recycling lithium iron phosphate by LiCl-KCl / NaCl molten salt electrolysis has many advantages, including efficient recycling, environmental protection, resource conservation, economic benefits, technical maturity, versatility, sustainable development and wide applicability. It provides a feasible solution for waste battery treatment and resource recycling, and helps promote the development of the clean energy industry and the realization of sustainable development goals. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0028] Figure 1 This is a schematic diagram of the process flow of the method for recovering lithium iron phosphorus from lithium iron phosphate waste by molten salt electrolysis in this application;
[0029] Figure 2 This is the XRD test diagram of the lithium phosphate product in Example 1 of the present application. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0031] Method for recovering lithium iron phosphorus from lithium iron phosphate waste by molten salt electrolysis
[0032] See also Figure 1 The method for recovering lithium iron phosphorus from lithium iron phosphate waste by molten salt electrolysis includes:
[0033] Step S100, obtaining LiCl-MCl molten salt, the LiCl-MCl molten salt is in a molten state, adding lithium iron phosphate waste to the LiCl-MCl molten salt, and electrolyzing it under an inert atmosphere to obtain a product metallic iron a attached to the cathode plate, an anode product and a molten salt electrolyte, wherein the molten salt electrolyte includes Li3PO4 and metallic iron b detached from the cathode plate; M is selected from at least one of Na element and K element.
[0034] The molten salt used in the present application is LiCl-KCl / NaCl. LiCl and KCl / NaCl are mixed evenly in a certain proportion, and the molten salt is heated at a high temperature to reach a molten state. When the molten salt reaches a molten state, lithium iron phosphate waste (waste lithium iron phosphate positive electrode material) is added. After the lithium iron phosphate waste is added, the lithium iron phosphate structure is broken to form Li + , Fe 2+ PO4 3- The ions exist in LiCl-MCl molten salt, and then electrolysis is carried out. The electrolysis electrode is selected from one of graphite plate, stainless steel plate and titanium plate.
[0035] Step S200, filtering the molten salt electrolyte to obtain a filter residue containing Li3PO4 and metallic iron b, and a filtrate, wherein the filtrate contains molten LiCl and MCl. The filtration is preferably high-temperature filtration, and the temperature of the high-temperature filtration is 350° C. to 550° C. The high-temperature filtration is beneficial to prevent the purity of the product Li3PO4 from being reduced due to the cooling of the molten salt, and is more conducive to the efficient recovery of Li and Fe / P. The filtrate can be optionally returned to step S100 to continue the molten salt electrolysis of lithium iron phosphate waste.
[0036] Step S300, placing the filter residue in water, magnetically attracting and washing, to obtain high-purity lithium phosphate and metallic iron b. The magnetic attraction and washing can refer to conventional technical means in the prior art, as long as the magnetic Fe powder and non-magnetic Li3PO4 can be separated, and this application does not limit it.
[0037] The present application uses LiCl-KCl / NaCl molten salt as the reaction system and performs high-temperature molten salt electrolysis to recover lithium iron phosphate waste, thereby preparing high-purity metallic Fe and high-purity Li3PO4 (purity greater than or equal to 99%), which not only realizes the green recycling of lithium iron phosphate waste, but also realizes the purification effect of LiCl, that is, preparing high-purity Li3PO4 from low-purity LiCl.
[0038] In some embodiments, in step S100, obtaining a LiCl-MCl molten salt includes: heating a material containing LiCl and a material containing MCl at 350°C to 800°C to obtain a molten LiCl-MCl molten salt, wherein the molar ratio of LiCl to MCl in the LiCl-MCl molten salt is K, and 0.15≤K≤4.0. The present application regulates the molar ratio K of LiCl and MCl in the LiCl-MCl molten salt within the above range, thereby reducing the electrolysis temperature, and the recovery rates of Li and Fe / P are higher, and the purity of the product Li3PO4 is also better.
[0039] Exemplarily, the value of K is 0.15, 0.18, 0.2, 0.3, 0.37, 0.5, 0.6, 0.66, 0.8, 1.2, 1.3, 1.6, 1.8, 1.87, 1.9, 2.1, 2.5, 2.8, 3.0, 3.5, 4.0 or a value within the range formed by any two of these values.
[0040] In some embodiments, the purity of LiCl in the material containing LiCl is 80wt% to 95wt%, and the impurities in the material containing LiCl include at least one of NaCl, KCl, MgCl2, CaCl2, and AlCl3. When the purity of LiCl in the material containing LiCl is within the above range and the types of its impurities are also appropriate, it is more conducive to dissolving lithium iron phosphate waste in molten salt to obtain Li + , Fe 2+ PO4 3- , and the efficiency of obtaining high-purity Li3PO4 by electrolysis is also better.
[0041] Exemplarily, the purity of LiCl in the LiCl-containing material is 80wt%, 82wt%, 84wt%, 85wt%, 88wt%, 90wt%, 92wt%, 93wt%, 95wt% or a value within the range consisting of any two of these values.
[0042] In some embodiments, the mass ratio of LiCl-MCl molten salt to lithium iron phosphate waste is (2-30):1, and the mass percentage of LiFePO4 in the lithium iron phosphate waste is W%, 95%≤W%≤100%. Regulating the mass ratio of LiCl-MCl molten salt to lithium iron phosphate waste within the above range is more conducive to improving Li + and PO4 3- Combined with the generation rate of Li3PO4, it is beneficial to the purification of Li while reducing energy consumption.
[0043] Exemplarily, the mass ratio of LiCl-MCl molten salt to lithium iron phosphate waste is 2:1, 4:1, 6:1, 8:1, 9:1, 10:1, 15:1, 18:1, 20:1, 25:1, 28:1, 30:1 or a value within the range consisting of any two of these values.
[0044] In some embodiments, the electrolysis conditions include: electrolysis temperature: 350°C to 800°C, electrolysis voltage: 2.0 V to 4.0 V. Further, the electrolysis temperature: 350°C to 500°C.
[0045] Illustratively, the electrolysis temperature is 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, or a value within the range consisting of any two of these values.
[0046] Illustratively, the electrolysis voltage is 2.0 V, 2.2 V, 2.3 V, 2.5 V, 2.8 V, 3.0 V, 3.5 V, 3.8 V, 4.0 V, or a value within a range consisting of any two of these values.
[0047] The following are possible implementations
[0048] This patent uses molten salt plus electrolysis to recover lithium iron phosphate. The molten salt used is LiCl and MCl (NaCl and / or KCl). LiCl and MCl are evenly mixed in a certain proportion. The molar ratio of LiCl: KCl is 0.25 to 4.0, and the molar ratio of LiCl: NaCl is 0.15 to 4.0. The molten salt is heated at high temperature to reach a molten state. The high temperature heating temperature is 350°C to 800°C. When the molten salt reaches a molten state, lithium iron phosphate material is added. The lithium iron phosphate material is added according to the mass of the molten salt. Among them, the mass ratio of molten salt: lithium iron phosphate is 2:1 to 30:1. After the lithium iron phosphate material is added, the lithium iron phosphate structure is broken. + , Fe 2+ PO4 3- It exists in the molten salt in the form of ions, and then undergoes electrolysis. Here, the electrolysis electrode is selected from one of graphite plates, stainless steel plates, and titanium plates. The electrolysis voltage is 2.0 to 4.5 V. High-temperature molten salt is used to improve the electrolysis efficiency. The entire electrolysis process must be isolated from oxygen (it must be carried out under an inert atmosphere) to ensure the efficient output of the electrolysis product. The electrolysis cathode produces high-purity Fe metal, and the anode produces chlorine gas. The chlorine gas is enriched by a collection device and is an additional economic income. Li + and PO4 3-Combined into Li3PO4, one part of Li comes from LiFePO4, and two parts of Li come from LiCl. The LiCl used here is low-purity, and high-purity Li3PO4 is generated during the electrolysis process, which belongs to the process of Li purification. In this process, the molten salt composed of LiCl and MCl is not only the medium of the electrolysis process, but also LiCl acts as a reactant. In this way, electrolysis can not only realize the recovery of LiFePO4, but also convert low-purity LiCl into high-purity Li3PO4, thereby maximizing economic benefits. The electrolysis product is filtered at high temperature to obtain filter residue and filtrate. The high-temperature filtration is to prevent the molten salt from cooling. The filter residue product is a mixture of metal Fe powder and Li3PO4. The filter residue mixture is placed in deionized water for magnetic attraction. The magnetic Fe powder and non-magnetic Li3PO4 are separated by magnetic attraction to obtain high-purity Fe powder and high-purity Li3PO4. The filtrate is a molten salt containing LiCl and KCl, which continues to dissolve lithium iron phosphate after circulating to high-temperature melting to achieve overall circulation.
[0049] The reactions involved are as follows:
[0050] Cathode reaction: Fe 2+ +2e - →Fe
[0051] Anode reaction: 2Cl - -2e - →Cl2
[0052] Overall reaction: LiFePO4+2LiCl→Fe+Li3PO4+Cl2↑
[0053] KCl can be replaced by NaCl;
[0054] The process of electrolysis in this process needs to be isolated from oxygen throughout the process, because during the electrolysis process, the cathode produces metallic iron. When oxygen is present, an oxidation reaction will inevitably occur, resulting in the production of iron oxide, which affects the purity of the product Li3PO4. The effects of this process: 1) High-purity metallic Fe and high-purity Li3PO4 can be prepared; 2) The purification effect of LiCl is achieved, that is, low-purity LiCl is prepared into high-purity Li3PO4.
[0055] Hereinafter, examples and comparative examples are given to more specifically illustrate the embodiments of the present application. Unless otherwise stated, the parts, percentages and ratios listed are all based on mass.
[0056] In the following examples and comparative examples, the lithium iron phosphate waste includes unqualified lithium iron phosphate and obsolete lithium iron phosphate batteries. The unqualified lithium iron phosphate and / or lithium iron phosphate obtained by dismantling obsolete lithium iron phosphate batteries are simply roasted in an inert atmosphere to obtain lithium iron phosphate waste with carbon and organic matter removed.
[0057] Example 1
[0058] LiCl-KCl molten salt was prepared with a LiCl:KCl molar ratio of 0.66, that is, 29.1g of lithium chloride with a purity of 90% and 71.9g of potassium chloride with a purity of 98% were weighed, mixed evenly and placed in a high-temperature furnace, heated to 650°C to make the molten salt reach a molten state, and then 10g of lithium iron phosphate waste was added to perform high-temperature (550°C) molten salt electrolysis. The electrolysis was carried out in a nitrogen atmosphere throughout the process. Graphite plates were used for both the positive and negative electrodes, and the electrode area was 4cm 2 , the electrolysis voltage was 4.0 V, and the current density was 200 mA / cm 2 , electrolysis time 2h, during the electrolysis process, the cathode plate produces metallic Fe, and the anode plate produces Cl2. A set of negative pressure devices is added to the anode plate to enrich the generated chlorine. Most of the metallic Fe (i.e. metallic iron a) is attached to the cathode plate, and metallic Fe powder is obtained by mechanical separation. At the same time, there is still a small amount of metallic Fe (i.e. metallic iron b) in the molten salt. After the electrolysis is completed, the molten salt is filtered at high temperature to obtain a solid mixed product of metallic Fe and Li3PO4, which is then placed in deionized water, and the Fe powder is separated from Li3PO4 by magnetic attraction, and the filtered molten salt is returned to the high-temperature molten salt for subsequent lithium iron phosphate electrolysis. Finally, 3.5g of ultrafine metallic Fe powder and 4.62g of Li3PO4 are obtained by LiCl-KCl molten salt electrolysis. The recovery rate of Fe element reaches 97.8%, and the recovery rate of Li and P elements reaches 98.9%. At the same time, the obtained Li3PO4 is subjected to XRD test, see the attached for details. Figure 2 , and the purity of Li3PO4 was tested, and the purity of Li3PO4 reached 99.0%. See Table 1.
[0059] Example 2
[0060] LiCl-KCl molten salt was prepared with a LiCl:KCl molar ratio of 1.87, that is, 53.8g of lithium chloride with a purity of 90% and 46.2g of potassium chloride with a purity of 98% were weighed, mixed evenly, and placed in a high-temperature furnace, heated to 450°C to make the molten salt reach a molten state, and then 10g of lithium iron phosphate waste was added to perform high-temperature (400°C) molten salt electrolysis. The electrolysis was carried out in an argon atmosphere. Stainless steel plates were used for both the positive and negative electrodes, and the electrode area was 4cm 2 , the electrolysis voltage was 4.0 V, and the current density was 240 mA / cm 2, electrolysis time 1.8h, during the electrolysis process, the cathode plate produces metallic Fe, and the anode plate produces Cl2. A set of negative pressure devices is added to the anode plate to enrich the generated chlorine. Most of the metallic Fe (i.e. metallic iron a) is attached to the cathode plate, and metallic Fe powder is obtained by mechanical separation. At the same time, there is still a small amount of metallic Fe (i.e. metallic iron b) in the molten salt. After the electrolysis is completed, the molten salt is filtered at high temperature to obtain a mixed product of metallic Fe and Li3PO4, and then placed in deionized water. The Fe powder is separated from Li3PO4 by magnetic attraction, and the filtered molten salt is returned to the high-temperature molten salt for subsequent lithium iron phosphate electrolysis. Finally, 3.48g of ultrafine metallic Fe powder and 4.63g of Li3PO4 are obtained by LiCl-KCl molten salt electrolysis. The recovery rate of Fe element reaches 97.5%, the recovery rate of Li and P elements reaches 99.0%, and the purity of Li3PO4 reaches 99.0%. See Table 1.
[0061] Example 3
[0062] LiCl-NaCl molten salt was prepared with a LiCl:NaCl molar ratio of 0.37, that is, 22.5g of 90% pure lithium chloride and 77.5g of 98% pure sodium chloride were weighed, mixed evenly and placed in a high-temperature furnace, heated to 700°C to make the molten salt reach a molten state, and then 10g of lithium iron phosphate waste was added to perform high-temperature (600°C) molten salt electrolysis. The electrolysis was carried out in a nitrogen atmosphere. Titanium plates were used for both positive and negative electrodes, and the electrode area was 4cm 2 , the electrolysis voltage is 2.0V, and the current density is 250mA / cm 2 , electrolysis time 0.7h, during the electrolysis process, the cathode plate produces metallic Fe, and the anode plate produces Cl2. A set of negative pressure devices is added to the anode plate to enrich the generated chlorine. Most of the metallic Fe (i.e. metallic iron a) is attached to the cathode plate, and metallic Fe powder is obtained by mechanical separation. At the same time, there is still a small amount of metallic Fe (i.e. metallic iron b) in the molten salt. After the electrolysis is completed, the molten salt is filtered at high temperature to obtain a mixed product of metallic Fe and Li3PO4, and then placed in deionized water. The Fe powder is separated from Li3PO4 by magnetic attraction, and the filtered molten salt is returned to the high-temperature molten salt for subsequent lithium iron phosphate electrolysis. Finally, 1.4g of ultrafine metallic Fe powder and 1.85g of Li3PO4 are obtained by LiCl-KCl molten salt electrolysis. The recovery rate of Fe element reaches 97.2%, the recovery rate of Li and P elements reaches 99.0%, and the purity of Li3PO4 reaches 99.0%. See Table 1.
[0063] Example 4
[0064] LiCl-KCl molten salt was prepared with a molar ratio of LiCl:KCl of 4, that is, 114.6g of lithium chloride with a purity of 90% and 46.2g of potassium chloride with a purity of 98% were weighed, mixed evenly and placed in a high-temperature furnace, heated to 650°C to make the molten salt reach a molten state, and then 16.7g of lithium iron phosphate waste was added to perform high-temperature (540°C) molten salt electrolysis. The electrolysis was carried out in a nitrogen atmosphere throughout the process. Graphite plates were used for both the positive and negative electrodes, and the electrode area was 4cm 2 , the electrolysis voltage was 4.0 V, and the current density was 200 mA / cm 2 , electrolysis time 2.2h, during the electrolysis process, the cathode plate produces metallic Fe, and the anode plate produces Cl2. A set of negative pressure devices is added to the anode plate to enrich the generated chlorine. Most of the metallic Fe (i.e. metallic iron a) is attached to the cathode plate, and metallic Fe powder is obtained by mechanical separation. At the same time, there is still a small amount of metallic Fe (i.e. metallic iron b) in the molten salt. After the electrolysis is completed, the molten salt is filtered at high temperature to obtain a solid mixed product of metallic Fe and Li3PO4, which is then placed in deionized water, and the Fe powder is separated from Li3PO4 by magnetic attraction, and the filtered molten salt is returned to the high-temperature molten salt for subsequent lithium iron phosphate electrolysis. The recovery rate of Fe element reaches 97.1%, the recovery rate of Li and P elements reaches 98.7%, and the purity of Li3PO4 is 99.1%. See Table 1.
[0065] Example 5
[0066] LiCl-KCl molten salt was prepared with a LiCl:KCl molar ratio of 0.1, that is, 2.8g of 90% pure lithium chloride and 46.2g of 98% pure potassium chloride were weighed, mixed evenly and placed in a high-temperature furnace, heated to 650°C to make the molten salt reach a molten state, and then 4.9g of lithium iron phosphate waste was added to perform high-temperature (700°C) molten salt electrolysis. The electrolysis was carried out in a nitrogen atmosphere. Graphite plates were used for both positive and negative electrodes, and the electrode area was 4cm 2 , the electrolysis voltage was 4.0 V, and the current density was 200 mA / cm 2 , electrolysis time 1.2h, during the electrolysis process, the cathode plate produces metallic Fe, and the anode plate produces Cl2. A set of negative pressure devices is added to the anode plate to enrich the generated chlorine. Most of the metallic Fe (i.e. metallic iron a) is attached to the cathode plate, and metallic Fe powder is obtained by mechanical separation. At the same time, there is still a small amount of metallic Fe (i.e. metallic iron b) in the molten salt. After the electrolysis is completed, the molten salt is filtered at high temperature to obtain a solid mixed product of metallic Fe and Li3PO4, which is then placed in deionized water, and the Fe powder is separated from Li3PO4 by magnetic attraction, and the filtered molten salt is returned to the high-temperature molten salt for subsequent lithium iron phosphate electrolysis. The recovery rate of Fe element reaches 96.1%, the recovery rate of Li and P elements reaches 97.3%, and the purity of Li3PO4 is 98.5%. See Table 1.
[0067] Example 6
[0068] LiCl-KCl molten salt was prepared with a LiCl:KCl molar ratio of 4.5, that is, 125.8g of lithium chloride with a purity of 90% and 46.2g of potassium chloride with a purity of 98% were weighed, mixed evenly and placed in a high-temperature furnace, heated to 650°C to make the molten salt reach a molten state, and then 17.2g of lithium iron phosphate waste was added to perform high-temperature (550°C) molten salt electrolysis. The electrolysis was carried out in a nitrogen atmosphere throughout the process. Graphite plates were used for both the positive and negative electrodes, and the electrode area was 4cm 2 , the electrolysis voltage was 4.0 V, and the current density was 200 mA / cm 2 , electrolysis time 2.4h, during the electrolysis process, the cathode plate produces metallic Fe, and the anode plate produces Cl2. A set of negative pressure devices is added to the anode plate to enrich the generated chlorine. Most of the metallic Fe (i.e. metallic iron a) is attached to the cathode plate, and metallic Fe powder is obtained by mechanical separation. At the same time, there is still a small amount of metallic Fe (i.e. metallic iron b) in the molten salt. After the electrolysis is completed, the molten salt is filtered at high temperature to obtain a solid mixed product of metallic Fe and Li3PO4, which is then placed in deionized water, and the Fe powder is separated from Li3PO4 by magnetic attraction, and the filtered molten salt is returned to the high-temperature molten salt for subsequent lithium iron phosphate electrolysis. The recovery rate of Fe element reaches 96.3%, the recovery rate of Li and P elements reaches 97.6%, and the purity of Li3PO4 is 98.3%. See Table 1.
[0069] Example 7
[0070] LiCl-KCl molten salt was prepared with a LiCl:KCl molar ratio of 1.87, that is, 53.8g of lithium chloride with a purity of 90% and 46.2g of potassium chloride with a purity of 98% were weighed, mixed evenly, and placed in a high-temperature furnace, heated to 650°C to make the molten salt reach a molten state, and then 3.33g of lithium iron phosphate waste was added to perform high-temperature (410°C) molten salt electrolysis. The electrolysis was carried out in a nitrogen atmosphere throughout the process. Graphite plates were used for both the positive and negative electrodes, and the electrode area was 4cm 2 , the electrolysis voltage is 2.5V, and the current density is 200mA / cm 2, electrolysis time 1.3h, during the electrolysis process, the cathode plate produces metallic Fe, and the anode plate produces Cl2. A set of negative pressure devices is added to the anode plate to enrich the generated chlorine. Most of the metallic Fe (i.e. metallic iron a) is attached to the cathode plate, and metallic Fe powder is obtained by mechanical separation. At the same time, there is still a small amount of metallic Fe (i.e. metallic iron b) in the molten salt. After the electrolysis is completed, the molten salt is filtered at high temperature to obtain a solid mixed product of metallic Fe and Li3PO4, which is then placed in deionized water, and the Fe powder is separated from Li3PO4 by magnetic attraction, and the filtered molten salt is returned to the high-temperature molten salt for subsequent lithium iron phosphate electrolysis. The recovery rate of Fe element reaches 97.3%, the recovery rate of Li and P elements reaches 98.8%, and the purity of Li3PO4 is 99.0%. See Table 1.
[0071] Comparative Example 1 (Oxygen is present during the entire electrolysis process)
[0072] Compared with Example 2, the only difference in Comparative Example 1 is that the entire electrolysis process is carried out in an air atmosphere. After the electrolysis is completed, the molten salt is magnetically separated to obtain magnetic material Fe and non-magnetic material. The non-magnetic material is tested and it is determined that the composition contains Fe2O3, which leads to a decrease in the purity of Li3PO4 after electrolysis, indicating that Fe2O3 will be produced in an oxygen environment.
[0073] In Table 1, the lithium chloride, potassium chloride, and sodium chloride in each embodiment can be obtained commercially, and the calculation of the mass of pure LiCl and pure MCl is based on the purity of lithium chloride and potassium chloride / sodium chloride in each embodiment. For example, in Example 1, the mass of pure LiCl = 29.1g x 90% = 26.19g, and the mass of pure KCl = 71.9g x 98% = 70.46g. Pure LiCl and pure MCl in other embodiments can be obtained by referring to the above calculation.
[0074] Table 1
[0075]
[0076]
[0077] From the comparison of Examples 1-4 and 7 with Examples 5-6 in Table 1, it can be seen that when the ratio of LiCl to MCl in the molten salt is greater than 0.1 and less than 4.5 (e.g., 0.15 to 4), the Fe recovery rate, the Li / P recovery rate, and the Li3PO4 purity are all improved, the Fe recovery rate is increased from about 96% to 97%-98%, the Li / P recovery rate is increased from about 97% to about 99%, and the Li3PO4 purity is increased from about 98% to more than 99%, and the temperature during electrolysis is relatively reduced to a certain extent, from 550 to 700°C to 400 to 600°C;
[0078] Furthermore, when the ratio continues to narrow the range (1.6 to 1.9), for example, to 1.87 in Example 2 and Example 7, while maintaining a good Fe recovery rate, Li / P recovery rate and Li3PO4 purity, the electrolysis temperature is significantly reduced (about 350 to 450°C), for example, the electrolysis temperature in Example 2 is 400°C, and the electrolysis temperature in Example 7 is 410°C.
[0079] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for recovering lithium, iron and phosphorus from lithium iron phosphate waste by molten salt electrolysis, characterized in that: The method comprises: S100, obtaining a LiCl-MCl molten salt, wherein the LiCl-MCl molten salt is in a molten state, adding lithium iron phosphate waste to the LiCl-MCl molten salt, and performing electrolysis under an inert atmosphere to obtain a product metallic iron a attached to a cathode plate, an anode product, and a molten salt electrolyte; The molten salt electrolyte includes Li3PO4 and metal iron b detached from the cathode plate; S200, filtering the molten salt electrolyte to obtain a filter residue containing Li3PO4 and metallic iron b, and a filtrate; S300, placing the filter residue in water, magnetically absorbing and washing it, to obtain high-purity lithium phosphate and metallic iron b; Wherein, M is selected from at least one of Na element and K element.
2. The method according to claim 1, characterized in that In step S100, obtaining LiCl-MCl molten salt includes: The material containing LiCl and the material containing MCl are placed under the condition of 350° C. to 800° C. and heated to obtain the LiCl-MCl molten salt in a molten state; In the LiCl-MCl molten salt, the molar ratio of LiCl to MCl is K, 0.15≤K≤4.0; Preferably, 1.6≤K≤1.9; Preferably, in the LiCl-containing material, the purity of LiCl is 80wt% to 95wt%; More preferably, the impurities in the LiCl-containing material include at least one of NaCl, KCl, MgCl2, CaCl2, and AlCl3.
3. The method according to claim 1, characterized in that In step S100, the mass ratio of the LiCl-MCl molten salt to the lithium iron phosphate waste is (2-30):1; Preferably, the mass ratio of the LiCl-MCl molten salt to the lithium iron phosphate waste is (8-30):1; Preferably, in step S100, the mass percentage of LiFePO4 in the lithium iron phosphate waste is W%, 95%≤W%≤100%.
4. The method according to claim 2, characterized in that: In step S100, LiCl in the LiCl-MCI molten salt participates in the electrolysis reaction as a reactant.
5. The method according to claim 1, characterized in that: In step S100, the anode product includes chlorine gas.
6. The method according to any one of claims 1 to 5, characterized in that: In step S100, the electrolysis conditions include: Electrolysis temperature: 350℃ to 800℃; Electrolysis voltage: 2.0V to 4.0V.
7. The method according to claim 6, characterized in that Electrolysis temperature: 350℃ to 500℃.
8. The method according to claim 1, characterized in that In step S200, at least one of the following conditions is met: Condition I: the filtrate contains molten LiCl and MCl, and the filtrate is returned to step S100 to continue molten salt electrolysis of the lithium iron phosphate waste; Condition II: the filtration is high temperature filtration, and the temperature of the high temperature filtration is 350°C to 550°C.
9. The method according to claim 1, characterized in that: The yield of the metallic iron a is greater than the yield of the metallic iron b.
10. High-purity lithium phosphate obtained by the method according to any one of claims 1 to 9, characterized in that: The purity of the high-purity lithium phosphate is greater than or equal to 99%.
Citation Information
Cited By
Waste battery recycling method and device
CN121215955A