Spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber and preparation method of spinning solution

By adding graphene powder to the spinning solution and utilizing its ultrathin sheet structure, the creep problem of ultra-high molecular weight polyethylene fiber was solved, and the dimensional stability of the fiber under long-term load was achieved, making it suitable for applications such as ropes and cables and deep-sea cages.

CN118932520APending Publication Date: 2024-11-12SHANDONG NANSHAN TEXTILE GARMENT +2

Patent Information

Application Number
CN202310538997.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies for preparing ultra-high molecular weight polyethylene fibers exhibit creep, which leads to dimensional instability of the fibers under long-term loads, affecting the reliability of applications, especially in the fields of ropes and cables and deep-sea cages.

Method used

A creep-resistant ultra-high molecular weight polyethylene (UHMWPE) fiber spinning solution is used, which includes UHMWPE powder, graphene powder, wetting and dispersing agent, anti-settling agent, coupling agent and antioxidant. Graphene is uniformly dispersed in the spinning solution through a specific mixing and grinding process. The ultra-thin sheet structure of graphene is used to block the movement of molecular chains and crystalline regions during the spinning process, thereby improving the creep resistance of the fiber.

Benefits of technology

It effectively controls fiber creep, improves fiber creep resistance, and maintains good spinnability, making it suitable for widespread application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932520A_ABST
    Figure CN118932520A_ABST
Patent Text Reader

Abstract

The invention provides a spinning solution for creep-resistant ultra-high molecular weight polyethylene fibers and a preparation method of the spinning solution. The spinning solution comprises ultra-high molecular weight polyethylene powder, graphene powder, a wetting dispersant, an anti-settling agent, a coupling agent and an antioxidant, wherein white oil is taken as a solvent; the preparation method comprises the steps of preparing a graphene powder mixture and preparing a spinning solution. The spinning solution prepared by the method provided by the invention overcomes the defect of creep phenomenon in use of the ultra-high molecular weight polyethylene fiber, and radiation crosslinking treatment is not used in the process, so that the problems of fiber surface crosslinking, surface oxidation, non-uniform chemical structure and poor performance caused by radiation treatment are effectively avoided; and the creep phenomenon of the ultra-high molecular weight polyethylene fiber in use is controlled within a controllable degree. The preparation method is simple, easy to control and suitable for wide popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high molecular weight polyethylene fiber manufacturing, and in particular to a spinning solution for creep resistant ultra-high molecular weight polyethylene fiber and a preparation method thereof. Background Art

[0002] UHMWPE fiber has excellent tensile strength and initial tensile modulus. Compared with carbon fiber and aramid, its specific tensile strength is the highest. As an excellent high-performance fiber, UHMWPE fiber is widely used in gloves, bulletproof vests, cables and other fields.

[0003] Although UHMWPE fiber has the characteristics of high strength and high modulus, since UHMWPE fiber is a non-polar molecule, the intermolecular force is much weaker than that of polymers such as polyester and aramid that can form intermolecular hydrogen bonds. Therefore, the molecular chains of UHMWPE fiber are prone to slip and creep, and under the action of external forces at a certain temperature, UHMWPE fiber will become longer under the action of creep.

[0004] Fiber creep is very disadvantageous in applications with long-term loads, especially in the field of ropes and cables. For example, ropes and cables used for lifting for a long time will become longer due to creep under continuous load, resulting in unstable size of the ropes and cables. In severe cases, it may cause the hoisted objects to slip. For example, in the field of deep-sea aquaculture, high-end cages are basically made of UHMWPE fibers. After a long period of use, the fibers become longer due to creep, causing the mesh of the cages to become larger, resulting in the escape of precious fish.

[0005] In the preparation of creep-resistant ultra-high molecular weight polyethylene fibers, the prior art generally adopts chemical-high energy radiation crosslinking. The invention patent with publication number CN105442100A provides an ultra-high molecular weight polyethylene fiber and a preparation method thereof, wherein the preparation method comprises extracting the primary filaments of the ultra-high molecular weight polyethylene fiber, impregnating the fiber with a radiation-sensitive crosslinking agent, drying, multi-stage hot stretching, and then irradiating the fiber with high energy rays. However, the ultra-high molecular weight polyethylene fiber product obtained by this method has technical defects such as fiber surface crosslinking, surface oxidation, chemical structure heterogeneity, and poor performance.

[0006] With the development of spinning technology and the continuous expansion of product application areas, how to control the creep phenomenon of ultra-high molecular weight polyethylene fibers within a controllable range is a problem that needs to be solved. Summary of the invention

[0007] In view of the above-mentioned deficiencies of the prior art, the present invention provides a spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber and a preparation method thereof, wherein the spinning solution comprises ultra-high molecular weight polyethylene powder, graphene powder, wetting dispersant, anti-settling agent, coupling agent, antioxidant, and the solvent is white oil; the spinning solution prepared by the method of the present invention overcomes the disadvantage that ultra-high molecular weight polyethylene fiber has creep phenomenon during use, and no radiation cross-linking treatment is used in the process, which effectively avoids the problems of fiber surface cross-linking, surface oxidation, chemical structure inhomogeneity and poor performance caused by radiation treatment, and controls the creep phenomenon of ultra-high molecular weight polyethylene fiber during use within a controllable degree. The preparation method is simple, easy to control, and suitable for wide promotion and application.

[0008] The technical solution of the present invention is as follows:

[0009] A spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber, the components of which are as follows by weight percentage:

[0010] Ultra-high molecular weight polyethylene powder: 5.0-15.0%, graphene powder: 0.01-0.1%, wetting and dispersing agent: 0.01-0.1%, anti-settling agent: 0.01-0.1%, coupling agent: 0.05-1.0%, antioxidant: 0.05-1.0%, and the balance is white oil solvent.

[0011] The spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber obtained by the present invention is a suspension of a multi-chemical component composite type, wherein the ultra-high molecular weight polyethylene powder material is the main material for forming ultra-high molecular weight polyethylene fiber, and white oil is a good solvent for the ultra-high molecular weight polyethylene powder material to form a high-temperature melt under heating; the wetting dispersant and the anti-settling agent can make the graphene powder material have a good dispersion effect, so that it is dispersed in the spinning solution with a micron size, and the coupling agent can prevent the graphene powder material from migrating in the subsequent spinning process unit. In addition, in the present invention, the ultra-thin sheet structure characteristics of the graphene powder material are utilized, and the graphene with an ultra-thin sheet structure is uniformly dispersed in the spinning solution by mixing and grinding when the spinning solution is configured. During the spinning process, the graphene is fixed between the molecular chains, between the crystalline regions of the molecular chains, and between the non-crystalline regions of the molecular chains. Since the ultra-thin sheet of the graphene has a certain blocking effect on the movement of the molecular chains, the crystalline regions, and the non-crystalline regions, the creep resistance of the ultra-high molecular weight polyethylene fiber is improved macroscopically.

[0012] Preferably, the weight percentage of the ultra-high molecular weight polyethylene powder is 6.0-12.0%; the viscosity average molecular weight of the ultra-high molecular weight polyethylene powder is 300×10 4 -900×10 4 .

[0013] Preferably, the viscosity average molecular weight of the ultra-high molecular weight polyethylene powder is 300×10 4 -600×10 4 .

[0014] Preferably, the weight percentage of the graphene powder is 0.01-0.05%; the number of layers of the graphene powder is 1.0-10.0 layers, and the plane size of the layer is 1-10.0 μm.

[0015] Preferably, the number of layers of the graphene powder is 5.0-8.0 layers, and the plane size of the flakes is 1.0-5.0 μm.

[0016] Preferably, the weight percentage of the wetting and dispersing agent is 0.01-0.05%, the weight percentage of the anti-settling agent is 0.01-0.05%, the weight percentage of the coupling agent is 0.05-0.5%, and the weight percentage of the antioxidant is 0.05-0.5%.

[0017] Preferably, the kinematic viscosity (40°C) of the white oil is 30-100 mm 2 / s, the preferred kinematic viscosity (40°C) is 60-90 mm 2 / s.

[0018] A method for preparing a spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber, the process is as follows:

[0019] (1) Preparation of graphene powder mixture:

[0020] First, add part of the white oil into the mixing barrel, then add the wetting dispersant and anti-settling agent at a low stirring speed of 30-60rpm, continue stirring for 30-60 minutes, and then add the graphene powder material. After the addition is completed, adjust the speed to 1200-1500rpm, stir for 3-6 hours, and let it stand for 3-6 hours to obtain a slurry;

[0021] The slurry is ground using a ball mill. The grinding process is as follows: first, grinding for 4-8 hours, then continuing to grind and monitoring the fineness of the slurry every half an hour. When the fineness of the slurry is 1.0-5.0 μm, the grinding is completed to obtain the ground material.

[0022] The ground material is filtered through a 400-mesh filter to obtain a graphene powder mixture for later use;

[0023] (2) Preparation of spinning solution:

[0024] Add part of the white oil into the mixing barrel, and then add the coupling agent and antioxidant at a low stirring speed of 30-60rpm; continue stirring for 30 minutes, and then add the ultra-high molecular weight polyethylene powder. After the addition is completed, adjust the speed of the mixer to 100-300rpm and stir for 1-2 hours; then add the graphene powder mixture, use a stirring speed of 100-300rpm, and stir for 1-2 hours; after the stirring is completed, add the remaining white oil, adjust the viscosity of the spinning solution to 80-120mPa.s, and the preparation of the spinning solution is completed.

[0025] Compared with the prior art, the beneficial effects of the present invention are:

[0026] 1. The ultra-high molecular weight polyethylene fiber obtained by the spinning solution used has good anti-creep performance and good spinnability, and can release ultra-high molecular weight polyethylene fibers with good anti-creep function.

[0027] 2. The preparation method provided by the invention is simple, easy to control, and suitable for wide promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0029] Figure 1 This is the flow chart of spinning solution preparation. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0031] In the following embodiments and comparative examples of the present invention, the raw material information is as follows: 4 million molecular weight PE powder: Asahi Kasei UH951 of Japan; 7 million molecular weight PE powder: Korea Petrochemical U070; white oil: Zhejiang Zhengxin F-04-009; graphene powder (commercially available); wetting dispersant: acrylic acid (commercially available); anti-settling agent: hydrophobic fumed silica (commercially available); coupling agent: titanate (commercially available); antioxidant: phosphite (commercially available).

[0032] Example 1

[0033] A spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber, the preparation method is as follows:

[0034] (1) Preparation of graphene powder mixture:

[0035] First, add 400g of white oil into a 2000ml glass beaker, then add 0.3g of wetting dispersant and 0.2g of anti-settling agent at a low stirring speed of 50rpm; continue stirring for 30 minutes, then add 0.5g of graphene powder material, after adding, adjust the speed to 1200rpm, stir for 3.5 hours, and let stand for 6 hours to obtain slurry;

[0036] The slurry was ground using a ball mill. The grinding process was as follows: first, grinding for 5 hours, then continuing to grind and monitoring the fineness of the slurry every half an hour. When the fineness of the slurry was 2.0 μm, the grinding was completed to obtain the grind material. The grinding time was recorded as 6 hours.

[0037] The ground material is filtered through a 400-mesh filter to obtain a graphene powder mixture for later use;

[0038] (2) Preparation of spinning solution:

[0039] Add 450g of white oil into a 2000ml glass beaker, then add 1.0g of coupling agent and 1.0g of antioxidant at a low stirring speed of 50rpm; continue stirring for 30 minutes, then add 100g of ultra-high molecular weight polyethylene powder with a viscosity-average molecular weight of 4 million, after the addition is completed, adjust the speed of the stirrer to 200rpm, and stir for 2 hours; then add the graphene powder mixture, adjust the stirring speed to 500rpm, and stir for 1.5 hours; after the stirring is completed, add 50g of white oil, adjust the viscosity of the spinning solution, and the viscosity of the spinning solution is detected to be 105mPa.s, and the preparation of the spinning solution is completed.

[0040] After the preparation, a spinning solution sample 1 for creep-resistant ultra-high molecular weight polyethylene fiber with a solid content of 10.0% was obtained.

[0041] Example 2

[0042] A spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber, the preparation method is as follows:

[0043] (1) Preparation of graphene powder mixture:

[0044] First, add 1000g of white oil into a 2000ml glass beaker, then add 0.6g of wetting dispersant and 0.4g of anti-settling agent at a low stirring speed of 50rpm; continue stirring for 30 minutes, then add 1.0g of graphene powder material, after adding, adjust the speed to 1200rpm, stir for 3.0 hours, and let it stand for 6 hours to obtain slurry;

[0045] The slurry was ground using a ball mill. The grinding process was as follows: first, grinding for 4 hours, then continuing to grind and monitoring the fineness of the slurry every half an hour. When the fineness of the slurry was 2.0 μm, the grinding was completed to obtain the grind material. The grinding time was recorded as 5 hours.

[0046] The ground material is filtered through a 400-mesh filter to obtain a graphene powder mixture for later use;

[0047] (2) Preparation of spinning solution:

[0048] Add 800g of white oil into a 3000ml stainless steel bucket, then add 1.5g of coupling agent and 1.5g of antioxidant at a low stirring speed of 50rpm; continue stirring for 30 minutes, then add 150g of ultra-high molecular weight polyethylene powder with a viscosity-average molecular weight of 7 million, after the addition is completed, adjust the speed of the stirrer to 200rpm, and stir for 2 hours; then add the graphene powder mixture, adjust the stirring speed to 500rpm, and stir for 1.5 hours; after the stirring is completed, add 50g of white oil to adjust the viscosity of the spinning solution, and the viscosity of the spinning solution is detected to be 97.0mPa.s, and the preparation of the spinning solution is completed.

[0049] After the preparation, a spinning solution sample 2 for creep-resistant ultra-high molecular weight polyethylene fiber with a solid content of 7.5% was obtained.

[0050] Example 3

[0051] Preparation of a comparative spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber:

[0052] Add 900g of white oil into a 2000ml glass beaker, then add 0.3g of dispersant, 0.2g of anti-settling agent, 1.0g of coupling agent and 1.0g of antioxidant at a low stirring speed of 50rpm, and continue stirring for 30 minutes; then add 100g of ultra-high molecular weight polyethylene powder with a viscosity-average molecular weight of 4 million, after the addition is completed, adjust the speed of the stirrer to 200rpm, and stir for 2 hours; after the stirring is completed, add 50g of white oil to adjust the viscosity of the spinning solution, and the viscosity of the spinning solution is detected to be 95mPa.s, and the preparation of the spinning solution is completed.

[0053] After the preparation, a comparative spinning solution sample 3 of a spinning solution sample for creep resistant ultra-high molecular weight polyethylene fiber with a solid content of 10.0% was obtained.

[0054] Example 4

[0055] Preparation of a comparative spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber:

[0056] Add 1800g of white oil into a 3000ml stainless steel bucket, then add 0.6g of wetting dispersant, 0.4g of anti-settling agent, 1.5g of coupling agent and 1.5g of antioxidant at a low stirring speed of 50rpm; continue stirring for 30 minutes, then add 150g of ultra-high molecular weight polyethylene powder with a viscosity-average molecular weight of 7 million. After the addition is completed, adjust the speed of the stirrer to 200rpm and stir for 2 hours; after the stirring is completed, add 50g of white oil to adjust the viscosity of the spinning solution. The viscosity of the spinning solution is detected to be 98.0mPa.s, and the preparation of the spinning solution is completed.

[0057] After the preparation, a comparative spinning solution sample 4 of a spinning solution sample for creep-resistant ultra-high molecular weight polyethylene fiber with a solid content of 7.5% was obtained.

[0058] Example 5

[0059] Preparation of spinning solution: Sample 1, Sample 2, Sample 3, and Sample 4 prepared in Examples 1-4 were used for laboratory spinning experiments, wherein Sample 1 and Sample 2 have anti-creep functions, and Sample 3 and Sample 4 are their corresponding blank control samples; Examples 1-4 are all in the laboratory stage;

[0060] Laboratory spinning process: The spinning solution dissolution extrusion equipment used in the laboratory is a TSH-high torque co-rotating parallel twin-screw compounding extruder with a screw diameter of 26 mm and a twin-screw aspect ratio of 52:1. There are eight heating zones in total. Samples 1, 2, 3, and 4 were tested for their spinning performance under the same subsequent experimental process conditions.

[0061] The spinning process is as follows:

[0062] First, set the temperature of the heating zone of the twin screw to 100℃, 120℃, 170℃, 225℃, 235℃, 200℃, 190℃, and 190℃ respectively. When the temperature of each heating zone of the screw reaches the set value, start the water pump and oil pump of the twin screw. After running for 10 minutes, the twin screw is started and the speed is set to 80rpm. At this time, slowly pour the spinning solution sample into the feeding port; when the spinning solution passes through the twin screw, the spinning solution is heated, and the ultra-high molecular weight polyethylene powder is dissolved in the white oil to form a spinning solution, which is extruded from the spinning die at the head of the twin screw and enters the water tank; at this time, the head pressure of the twin screw is 0.32MPa, and the melt temperature of the spinning solution is measured by a temperature measuring gun to be 190℃;

[0063] The spinning solution passes through the spinning die to form a tow that enters the water bath. The temperature of the water bath is controlled at 25±2°C. The tow forms a gel state in the water bath. At this time, the spinning speed is 1.5 m / min. After the water bath, the gel tow enters the extraction tank filled with an extractant for extraction. The white oil solvent in the tow is replaced by the extractant. The speed of the tow in the extraction tank is 1.5 m / min, and the extraction time is 10 min.

[0064] Then it enters the drying box for drying. In the drying box, hot air drying is adopted. The temperature of the hot air is 55℃. The speed of the tow in the drying box is 1.5m / min and the drying time is 6min. When passing through the drying box, the extractant in the tow is completely volatilized from the tow. The tow out of the drying box is an undrawn tow of ultra-high molecular weight polyethylene.

[0065] The undrawn tow is subjected to three heat drawing in the heating box, and passes through four four-roller drawing machines and three heating boxes. The four-roller drawing machines and the heating boxes are arranged at intervals, and the drawing is completed by using the speed difference of the four-roller drawing machines; the speed of the first four-roller drawing machine is 1.5m / min, the temperature of the first drawing heating box is 135℃, and the speed of the second four-roller drawing machine is 9.0m / min. The tow is drawn in the first drawing hot box, and the first drawing ratio is 6.0; then the tow The fiber bundle enters the second stretching and heating box for stretching, the temperature of the second stretching and heating box is 140°C, the speed of the third four-roller stretching machine is 13.5m / min, and the second stretching ratio is 1.5; finally, it enters the third stretching and heating box for stretching, the temperature of the third stretching and heating box is 140°C, and the fiber bundle exits the third stretching and heating box and enters the winder for winding, the speed of the winder is 16.2m / min, and the third stretching ratio is 1.2, and a fiber sample is obtained on the winder.

[0066] The spinning experiments described above were carried out using the spinning solution samples 1, 2, 3 and 4 prepared in Examples 1-4, respectively, to obtain corresponding fiber samples.

[0067] Example 6

[0068] A spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber, the preparation method is as follows:

[0069] (1) Preparation of graphene powder mixture:

[0070] First, add 500 kg of white oil into a 2000 liter stirring kettle, then add 0.4 kg of wetting dispersant and 0.4 kg of anti-settling agent at a low stirring speed of 50 rpm; continue stirring for 30 minutes, then add 1.0 kg of graphene powder material, after adding, adjust the speed to 1200 rpm, stir for 3.0 hours, and let it stand for 6 hours to obtain slurry;

[0071] The slurry was ground using a ball mill. The grinding process was as follows: first, grinding for 4 hours, then continuing to grind and monitoring the fineness of the slurry every half an hour. When the fineness of the slurry was 2.0 μm, the grinding was completed to obtain the grind material. The grinding time was recorded as 5 hours.

[0072] The ground material is filtered through a 400-mesh filter to obtain a graphene powder mixture for later use;

[0073] (2) Preparation of spinning solution:

[0074] Add 1300kg of white oil into a 3000-liter stirring kettle, then add 1.5kg of coupling agent and 1.5kg of antioxidant at a low stirring speed of 50rpm; continue stirring for 30 minutes, then add 150kg of ultra-high molecular weight polyethylene powder with a viscosity-average molecular weight of 7 million, after the addition is completed, adjust the speed of the stirrer to 200rpm, and stir for 2 hours; then add the graphene powder mixture, use a stirring speed of 300rpm, and stir for 1.5 hours; after the stirring is completed, add 50kg of white oil to adjust the viscosity of the spinning solution, and the viscosity of the spinning solution is detected to be 105.0mPa.s, and the preparation of the spinning solution is completed.

[0075] After the preparation, a spinning solution sample 5 for creep-resistant ultra-high molecular weight polyethylene fiber with a solid content of 7.5% was obtained.

[0076] Example 7

[0077] Preparation of a comparative spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber:

[0078] Add 1800kg of white oil into a 3000-liter stirring kettle, then add 0.4kg of wetting dispersant, 0.4kg of anti-settling agent, 1.5kg of coupling agent and 1.5kg of antioxidant at a low stirring speed of 50rpm; after stirring for 30 minutes, add 150kg of ultra-high molecular weight polyethylene powder with a viscosity-average molecular weight of 7 million. After the addition is completed, adjust the speed of the stirrer to 200rpm and stir for 2 hours; after the stirring is completed, add 50kg of white oil to adjust the viscosity of the spinning solution. The viscosity of the spinning solution is detected to be 96.0mPa.s, and the preparation of the spinning solution is completed.

[0079] After the preparation, a comparative spinning solution sample 6 of a spinning solution sample for creep-resistant ultra-high molecular weight polyethylene fiber with a solid content of 7.5% was obtained.

[0080] Example 8

[0081] Preparation of spinning solution: Spinning solution samples 5 and 6 prepared in Examples 6 and 7 were used to carry out spinning experiments on the production line, wherein sample 5 has an anti-creep function and sample 6 is its corresponding blank control sample; Examples 6 and 7 are the production stage;

[0082] Spinning process: The spinning solution dissolution extrusion equipment used is a TSB-125 high-torque co-rotating parallel twin-screw compounding extruder with a screw diameter of 125 mm and a twin-screw aspect ratio of 68:1. There are 16 heating zones in total. Samples 5 and 6 were tested for their spinning performance under the same subsequent production process conditions.

[0083] The production process consists of two parts, the pre-spinning part and the post-spinning part. The main function of the pre-spinning part is to dissolve the ultra-high molecular weight polyethylene powder in white oil, and form a good gel tow in a water bath after metering by a metering pump and forming by a spinning assembly; the main function of the post-spinning part is to obtain the finished ultra-high molecular weight polyethylene fiber through pre-stretching, extraction, drying, hot stretching and other processes. They are described as follows:

[0084] Pre-spinning part: first set the temperature of the heating zone of the twin screw to 135℃, 220℃, 235℃, 240℃, 245℃, 255℃, 255℃, 255℃, 265℃, 270℃, 270℃, 280℃, 295℃, 295℃, 280℃, 280℃, and wait until the temperature of each heating zone of the screw reaches the set value, start the water pump and oil pump of the twin screw, and after running for 10 minutes, the twin screw is started, and the speed is set to 175rpm. At this time, slowly pour the spinning solution sample into the feeding port; when the spinning solution passes through the twin screw, the spinning solution is heated, and the ultra-high molecular weight polyethylene powder is dissolved in the white oil to form a spinning solution, which is extruded from the spinning die at the head of the twin screw and enters the water tank; at this time, the head pressure of the twin screw is 4.5Mpa, and the melt temperature of the spinning solution is measured by a temperature measuring gun to be 280℃;

[0085] The spinning solution passes through the filter and enters the melt metering pump, the speed of the metering pump is 36.0rpm, and the temperature of the box where the metering pump is located is 245°C; after being metered by the metering pump, the spinning solution enters the spinning assembly and is sprayed out to form a tow, wherein the specifications of the spinneret in the spinning assembly are: 480 spinnerets, divided into two zones, the diameter of each spinneret is 0.7mm, and the aspect ratio (L / D) of the spinneret is 10; the tow sprayed out from the spinning assembly forms a gel yarn after entering the water bath, wherein the temperature of the water bath is controlled at 25±2°C, the tow forms a gel state in the water bath, and the spinning speed is 4.5m / min at this time; the spun tow is placed in the corresponding wire barrel for standby use;

[0086] Post-spinning part: After three days of natural equilibrium, the gel tow is first subjected to preliminary drawing before extraction, wherein the speeds of the four-roller drawing machines 1 and 2 are 0.8m / min and 4.00m / min respectively; the gel tow after preliminary drawing enters the extraction tank filled with the extractant for extraction, and the white oil solvent in the tow is replaced by the extractant, the speed of the tow in the extraction tank is 4.5m / min, and the extraction time is 15min; then it enters the drying oven for drying, in which hot air drying is adopted, the temperature of the hot air is 50℃, the speed of the tow in the drying oven is 4.5m / min, and the drying time is 6min; when passing through the drying oven, the extractant in the tow is completely volatilized from the tow, and the tow out of the drying oven is an undrawn tow containing ultra-high molecular weight polyethylene;

[0087] The undrawn tow is drawn in the post-drawing process, and a total of three drawing processes are carried out under the heating state. The drawing heating is completed in the heating box. There is a drawing machine on both sides of the heating box, and the speed difference is used for stretching; the speed of the first four-roll drawing machine is 5.5m / min, the temperature of the first drawing heating box is 135℃, and the speed of the second four-roll drawing machine is 21.5m / min. The tow is drawn in the first drawing hot box, and the first drawing ratio is 3.9; then the tow enters the second drawing heating box for drawing, the temperature of the second drawing heating box is 138℃, the speed of the third four-roll drawing machine is 32.0m / min, and the second drawing ratio is 1.5; finally, it enters the third drawing heating box for drawing, the temperature of the third drawing heating box is 140℃, the tow comes out of the third drawing hot box, enters the winder for winding, the speed of the winder is 38.5m / min, the third drawing ratio is 1.2, and the fiber sample is obtained on the winder;

[0088] The spinning experiments described above were carried out using the spinning solution samples 5 and 6 prepared in Example 6 and Example 7, respectively, to obtain corresponding fiber samples.

[0089] Example 9

[0090] The tensile creep elongation of the fiber samples obtained in the laboratory was determined as follows:

[0091] Sampling method:

[0092] The fiber samples were obtained by laboratory spinning with the spinning solution sample 1 in Example 1. One meter was taken every 50 meters as the test sample, and the test was repeated three times. The samples were labeled as S11, S12, and S13 (see Example 5 for the specific spinning experiment);

[0093] The fiber samples were obtained by laboratory spinning with the spinning solution sample 2 in Example 2. One meter was taken every 50 meters as the test sample, and the test was repeated three times. The samples were labeled as S21, S22, and S23 (see Example 5 for the specific spinning experiment);

[0094] The fiber samples were obtained by laboratory spinning with the spinning solution sample 3 in Example 3. One meter was taken every 50 meters as the test sample, and the test was repeated three times. The samples were labeled as S31, S32, and S33 (see Example 5 for the specific spinning experiment);

[0095] The fiber samples were obtained by laboratory spinning with the spinning solution sample 4 in Example 4. One meter was taken every 50 meters as the test sample, and the test was repeated three times. The samples were labeled as S41, S42, and S43 (see Example 5 for the specific spinning experiment);

[0096] Test method: Test method for tensile properties of high-strength fiber filaments (GB / T 19975-2005);

[0097] The test results are shown in Table 1 below.

[0098] Table 1 Test results of spinning samples in laboratory stage

[0099] Serial number 1 2 3 4 5 6 7 8 9 10 11 12 sample S11 S12 S13 S21 S22 S23 S31 S32 S33 S41 S42 S43 G 0.80 0.81 0.82 0.90 0.92 0.92 1.62 1.62 1.64 1.90 1.92 1.90

[0100] Note: G is tensile creep elongation, %.

[0101] Example 10

[0102] The tensile creep elongation of the fiber samples obtained during production was measured:

[0103] Sampling method:

[0104] The spinning solution sample 5 in Example 6 was used to spin the fiber sample in the production stage. Five silk cakes were randomly selected from the full roll fiber products obtained as test samples, and the samples were marked as S51, S52, S53, S54, and S55 (see Example 8 for the specific spinning experiment);

[0105] The spinning solution sample 6 in Example 7 was used to spin the fiber sample in the production stage. Five silk cakes were randomly selected from the full roll fiber products obtained as test samples. The samples were identified as S61, S62, S63, S64, and S65 (see Example 8 for the specific spinning experiment);

[0106] Test method: Test method for tensile properties of high-strength fiber filaments (GB / T 19975-2005);

[0107] The test results are shown in Table 2 below.

[0108] Table 2 Test results of spinning samples in the production stage

[0109] Serial number 1 2 3 4 5 6 7 8 9 10 sample S51 S52 S53 S54 S55 S61 S62 S63 S64 S65 G 0.86 0.86 0.85 0.85 0.86 1.72 1.70 1.70 1.72 1.70

[0110] Note: G is tensile creep elongation, %.

[0111] From Table 1, we can see that:

[0112] ① In the laboratory stage, a PE raw material with the same molecular weight of 4 million was used to prepare a spinning solution with a solid content of 10%. The spinning solution prepared by the method of the present invention (see Example 1) had an average tensile creep elongation G (corresponding to the test results S11, S12, and S13) of 0.86 after spinning. The spinning solution prepared by the conventional method (without adding graphene) (see Example 3) had an average tensile creep elongation G (corresponding to the test results S31, S32, and S33) of 1.71 after spinning. This shows that the spinning solution prepared by the method of the present invention has a good anti-creep effect;

[0113] ② In the laboratory stage, a PE raw material with the same molecular weight of 7 million was used to prepare a spinning solution with a solid content of 7.5%. The spinning solution prepared by the method of the present invention (see Example 2) had an average tensile creep elongation G (corresponding to the test results S21, S22, and S23) of 0.91 after spinning. The spinning solution prepared by the conventional method (without adding graphene) (see Example 4) had an average tensile creep elongation G (corresponding to the test results S41, S42, and S43) of 1.91 after spinning. This shows that the spinning solution prepared by the method of the present invention has a good anti-creep effect;

[0114] From Table 2, we can see that:

[0115] ③ In the production stage, a PE raw material with the same molecular weight of 7 million was used to prepare a spinning solution with a solid content of 7.5%. The spinning solution prepared by the method of the present invention (see Example 6) had an average tensile creep elongation G (corresponding to the test results S51, S52, S53, S54, and S55) of 0.86 after spinning. The spinning solution prepared by the conventional method (without adding graphene) (see Example 7) had an average tensile creep elongation G (corresponding to the test results S61, S62, S63, S64, and S65) of 1.71 after spinning. This shows that the spinning solution prepared by the method of the present invention has a good anti-creep effect;

[0116] Although the present invention has been described in detail by reference to the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.

Claims

1. A spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber, characterized in that: The components by weight percentage are as follows: Ultra-high molecular weight polyethylene powder: 5.0-15.0%, graphene powder: 0.01-0.1%, wetting and dispersing agent: 0.01-0.1%, anti-settling agent: 0.01-0.1%, coupling agent: 0.05-1.0%, antioxidant: 0.05-1.0%, and the balance is white oil solvent.

2. The spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: The weight percentage of the ultra-high molecular weight polyethylene powder is 6.0-12.0%; the viscosity average molecular weight of the ultra-high molecular weight polyethylene powder is 300×10 4 -900×10 4 .

3. The spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber according to claim 2, characterized in that: The viscosity average molecular weight of ultra-high molecular weight polyethylene powder is 300×10 4 -600×10 4 .

4. The spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: The weight percentage of the graphene powder is 0.01-0.05%; the number of layers of the graphene powder is 1.0-10.0 layers, and the plane size of the layer is 1-10.0 μm.

5. The spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber according to claim 4, characterized in that: The number of layers of the graphene powder is 5.0-8.0 layers, and the plane size of the flakes is 1.0-5.0 μm.

6. The spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: The weight percentage of the wetting and dispersing agent is 0.01-0.05%, the weight percentage of the anti-settling agent is 0.01-0.05%, the weight percentage of the coupling agent is 0.05-0.5%, and the weight percentage of the antioxidant is 0.05-0.5%.

7. The spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: The kinematic viscosity (40°C) of the white oil is 30-100 mm 2 / s.

8. The spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber according to claim 7, characterized in that: The kinematic viscosity of white oil (40℃) is 60-90mm 2 / s.

9. The method for preparing a spinning solution for creep-resistant ultra-high molecular weight polyethylene fiber according to any one of claims 1 to 8, characterized in that: The process is as follows: (1) Preparation of graphene powder mixture: First, add part of the white oil into the mixing barrel, then add the wetting dispersant and anti-settling agent at a low stirring speed of 30-60rpm, continue stirring for 30-60 minutes, and then add the graphene powder material. After the addition is completed, adjust the speed to 1200-1500rpm, stir for 3-6 hours, and let it stand for 3-6 hours to obtain a slurry; The slurry is ground using a ball mill. The grinding process is as follows: first, grinding for 4-8 hours, then continuing to grind and monitoring the fineness of the slurry every half an hour. When the fineness of the slurry is 1.0-5.0 μm, the grinding is completed to obtain the ground material. The ground material is filtered through a 400-mesh filter to obtain a graphene powder mixture for later use; (2) Preparation of spinning solution: Add part of the white oil into the mixing barrel, then add the coupling agent and antioxidant at a low stirring speed of 30-60rpm; continue stirring for 30 minutes, then add the ultra-high molecular weight polyethylene powder, after the addition is completed, adjust the speed of the mixer to 100-300rpm, and stir for 1-2 hours; then add the graphene powder mixture, use a stirring speed of 300-600rpm, and stir for 1-2 hours; after the stirring is completed, add the remaining white oil, adjust the viscosity of the spinning solution to 80-120mPa.s, and the preparation of the spinning solution is completed.

Citation Information

Patent Citations

  • Ultra-high molecular weight polyethylene fiber and preparation method thereof

    CN105442100A

Cited By

  • Creep-resistant ultra-high molecular weight polyethylene fiber as well as preparation method and application thereof