Polypropylene composition, preparation method of polypropylene material and automobile part

By adding microcapsules and force-discolored compounds to the polypropylene composition, the mechanical damage status monitoring of fiber-reinforced plastic parts is solved, and the problem of untimely monitoring in the prior art is improved, and the material performance and production efficiency are improved.

CN118956056APending Publication Date: 2024-11-15CHONGQING CHANGAN AUTOMOBILE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411034232.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to accurately and timely monitor the mechanical damage status of fiber-reinforced plastic parts, resulting in performance deviations and use effects in actual applications.

Method used

Polypropylene composition is used, in which microcapsules are added as nucleating agents, and the fluorescence color is changed under the action of external forces, significantly differentiating the cracked and non-cracked areas, and monitoring the damage status of materials and parts is achieved.

Benefits of technology

Through the use of microcapsules, the mechanical strength and creep resistance of the polypropylene composition are improved, and the damage status of materials and parts is monitored in a timely manner, solving the problem of monitoring fiber-reinforced plastic parts, and improving material performance and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956056A_ABST
    Figure CN118956056A_ABST
Patent Text Reader

Abstract

The invention relates to a polypropylene composition, a preparation method of a polypropylene material and an automobile part, and relates to the technical field of high polymer materials. The polypropylene composition is prepared from the following components in parts by mass: 100 parts of a component A and 2 to 5 parts of microcapsules, wherein the component A comprises the following components in percentage by mass: 5-40% of reinforced fibers, 3-5% of a first compatilizer and the balance of polypropylene; a core material of the microcapsule comprises a mechanochromic compound. Wherein the microcapsule can be used as a nucleating agent to accelerate the crystallization speed and refine the grain structure, and the mechanical strength and creep resistance of the polypropylene composition can be effectively improved by matching with other component raw materials. Moreover, the microcapsules can enable the crack area to have color difference different from that of a non-crack area when the polypropylene material and the parts made of the polypropylene material generate microcracks due to external force, so that the mechanical damage state of the polypropylene material and the parts made of the polypropylene material can be conveniently, timely and effectively monitored.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, in particular to the technical field of polypropylene composite materials, and specifically to a polypropylene composition, a method for preparing a polypropylene material, and an automobile part. Background Art

[0002] Fiber reinforced plastics have high elastic modulus, low water absorption and good dimensional stability, and are widely used in parts related to the automotive, transportation, construction and other industries. In the automotive field, with the development of new automotive business, some metal parts in automobiles can be replaced by plastic and semi-plastic parts, such as steering support, front frame, back door frame, suspension, etc. Such parts are usually affected by the external environment and their own mechanical state during use. CAE simulation is usually used in industry to predict the risks of parts, and optimize the parts from the material and structure to ensure the integrity and functionality of the parts. However, simulation often causes differences between risk prediction results and actual results due to factors such as model matching and molding process accuracy; in addition, the material cards required for simulation (such as material rheological properties, mechanical properties, etc.) and part force model testing and construction process take too long. When the performance risk of parts deviates, the cause of the problem cannot be determined in a timely and accurate manner, which will have a certain impact on the normal use of parts.

[0003] Therefore, how to more accurately evaluate the performance of fiber-reinforced plastic parts in practical applications and monitor their mechanical damage state in a timely and effective manner has become a technical problem that needs to be solved urgently. Summary of the invention

[0004] The present application provides a polypropylene composition, a method for preparing a polypropylene material, and an automotive part to solve the technical problem of inconvenient and untimely monitoring of the mechanical damage state of fiber reinforced plastic parts in the related art. The technical solution of the present application is as follows:

[0005] According to the first aspect of the present application, a polypropylene composition is provided, wherein the components of the polypropylene composition include, by weight, 100 parts of component A and 2 to 5 parts of microcapsules. Component A includes, by weight percentage, 5% to 40% of reinforcing fibers, 3% to 5% of a first compatibilizer, and the remainder is polypropylene. The core material of the microcapsule includes a mechanochromic compound.

[0006] According to the above technical means, the present application uses polypropylene as a matrix, adds reinforcing fibers for use in combination, and adds a first compatibilizer to improve the compatibility between the component materials. At the same time, microcapsules are used as nucleating agents for the polypropylene composition, so that the nucleation process of the polypropylene composition is transformed from the original homogeneous phase to the heterogeneous phase, the crystallization rate is accelerated, the grain structure is refined, and the mechanical strength and creep resistance of the polypropylene composition can be improved.

[0007] Moreover, the microcapsules can be broken under the action of external force, and the mechanochromic compounds in the core material can undergo changes in structure or electronic state due to the external force, causing them to appear in a color different from that of the microcapsules under fluorescence. This makes the crack area appear different in color from the non-crack area, which can conveniently, timely and effectively monitor the damage status of materials and parts made of polypropylene compositions.

[0008] In one possible embodiment, the mechanochromic compound includes at least one of carbazole and its derivatives, spiropyran and its derivatives, spirothiopyran and its derivatives, coumarin dimer and its derivatives, cyclobutane peroxide and its derivatives, rhodamine and its derivatives, and isothiocyanic acid and its derivatives.

[0009] According to the above technical means, the above-mentioned mechanochromic compound is easy to obtain, and can undergo changes in structure or electronic state under the action of external force, so that it presents another color under fluorescence, which can more accurately monitor the damage status of materials and parts prepared from polypropylene compositions.

[0010] In a possible implementation, the shell material of the microcapsule includes polyurea resin.

[0011] According to the above technical means, the microcapsules can be well compatible with other components in the polypropylene composition, so that the acrylic acid composition can form a stable whole.

[0012] In a possible implementation, the particle size of the microcapsules ranges from 5 μm to 30 μm.

[0013] According to the above technical means, when the particle size of the microcapsules is within the above range, the microcapsules can be dispersed more completely and evenly in the polypropylene composition.

[0014] In a possible implementation, the reinforcing fiber includes carbon fiber and glass fiber; by mass percentage, component A includes: carbon fiber: 5% to 40%, glass fiber: 5% to 40%, first compatibilizer: 3% to 5%, and the balance is polypropylene.

[0015] According to the above technical means, carbon fiber and glass fiber are used as reinforcements, and the first compatibilizer can improve the compatibility of the fiber and polypropylene. The present application can increase the mechanical properties of the polypropylene composition and improve its creep resistance.

[0016] In a possible implementation, the diameter of the glass fiber is 5 μm to 15 μm; and / or the diameter of the carbon fiber is 5 μm to 15 μm.

[0017] According to the above technical means, the diameter of the glass fiber is within the above range, and / or the diameter of the carbon fiber is within the above range, which can improve the reinforcing effect of the reinforcing fiber in the polypropylene composition and reduce the cost of use.

[0018] In a possible implementation, the melt flow rate of polypropylene under preset conditions is 10 g / 10 min to 80 g / 10 min.

[0019] According to the above technical means, when the melt flow rate of polypropylene is within the above range, the polypropylene composition has better fluidity.

[0020] In a possible embodiment, the polypropylene composition further comprises, by weight, at least one of: an antioxidant: 1 to 3 parts; and a lubricant: 0.5 to 3 parts.

[0021] According to the above technical means, the antioxidant can prevent the polypropylene composition from being oxidized, thereby preventing the performance of the polypropylene composition from being degraded due to oxidation; the lubricant can improve the fluidity of the melt; through the above settings, the components cooperate with each other to improve the mechanical strength and creep resistance of the polypropylene composition.

[0022] In one possible embodiment, the first compatibilizer includes a compatible component, or the first compatibilizer includes a polymer and a compatible component grafted to the polymer; wherein the compatible component includes at least one of maleic anhydride and its derivatives, compounds containing epoxy groups, carboxylic acids and their derivatives, and acrylic acid glycidol and its derivatives.

[0023] According to the above technical means, the first compatibilizer can diffuse and graft well between the components of the polypropylene composition, chemically react with other components of the polypropylene composition or form physical crosslinks, so that the different components of the polypropylene composition can be mixed more evenly, thereby enhancing the overall stability of the polypropylene composition.

[0024] In a possible implementation, the lubricant includes at least one of silicone and its derivatives, erucamide and its derivatives, stearic acid and its derivatives, and vinyl bisstearamide and its derivatives.

[0025] In a possible embodiment, the antioxidant includes at least one of hindered phenols and their derivatives, phosphites and their derivatives, and amines and their derivatives.

[0026] In a second aspect, a method for preparing a polypropylene material is provided.

[0027] A method for preparing a polypropylene material comprises: blending and extruding the components in the polypropylene composition of any one of the possible implementation modes described above to obtain the polypropylene material.

[0028] According to the above technical means, the polypropylene material can be prepared by blending and extruding the polypropylene composition, and in this process, the microcapsules can be used as nucleating agents to transform the nucleation process of the polypropylene composition from the original homogeneous phase to the heterogeneous phase, accelerate the crystallization rate, refine the grain structure, and improve the mechanical strength and creep resistance of the polypropylene composition; when the obtained polypropylene material forms a crack zone under the action of external force, the crack zone appears different in color from the non-crack zone under fluorescence, which can conveniently, timely and effectively monitor the damage state of the polypropylene material.

[0029] In a possible embodiment, a method for preparing a polypropylene material specifically includes: configuring raw materials according to the components of the polypropylene composition in any of the above possible embodiments; adding the raw materials into a twin-screw extruder through multiple feed ports, and obtaining extrusion raw materials after extrusion; cooling, drying, and pelletizing the extruded raw materials to obtain a polypropylene material.

[0030] In a possible embodiment, the first direction is parallel to the extension direction of the screw assembly and is the direction from the feed port of the twin-screw extruder to the discharge port. Along the first direction, the screw assembly of the twin-screw extruder is divided into a conveying section, a melting section, a plasticizing section and a discharge section arranged in sequence; wherein the conveying section, the melting section and the plasticizing section include a plurality of forward shear blocks; and the melting section and the plasticizing section also include at least one reverse transport block.

[0031] Here, the material can move in a forward direction under the action of the forward shear block, and can move in a reverse direction under the action of the reverse transport block, wherein the forward direction is the same direction as the first direction and the reverse direction is the direction opposite to the first direction.

[0032] According to the above technical means, the present application can ensure the mixing uniformity of the components in the polypropylene composition, reduce the degree of damage to the reinforcing fibers during the blending and extrusion process, and make the retention length of the reinforcing fibers longer, thereby improving the creep resistance of the polypropylene material.

[0033] In a possible implementation manner, the staggered angle of the forward shear blocks ranges from 30° to 60°.

[0034] The forward shear block is staggered by a plurality of shear pieces, and the staggered angle refers to the angle between the symmetry centers of two adjacent shear pieces.

[0035] According to the above technical means, the present application can make the reinforcing fibers retain a longer length in the polypropylene material and achieve a better dispersion effect. Moreover, it can reduce the damage to the microcapsules during the co-extrusion process, thereby improving the performance of the polypropylene material and improving the accuracy of monitoring the mechanical damage state of the polypropylene material parts.

[0036] In a possible implementation, the method for preparing the polypropylene material further includes: preparing microcapsules.

[0037] The preparation of microcapsules includes: adding 0.5-1.5 parts by mass of urea to 1.5-2.5 parts by mass of formaldehyde solution, and adding an alkaline catalyst to the formaldehyde solution to obtain a first mixed solution with a pH value of 7-8.

[0038] The first mixed solution is stirred at a temperature of 60° C. to 70° C. for 1 to 2 hours to obtain a polyurea resin prepolymer.

[0039] 9 to 11 parts by mass of styrene monomer, 2 to 4 parts by mass of a cross-linking agent, and 1 to 3 parts by mass of a second compatibilizer are mixed to obtain a second mixed solution, and an emulsifier is added to the second mixed solution so that the ratio of the mass of the emulsifier to the mass of the second mixed solution is 1 to 3 to obtain a third mixed solution.

[0040] The third mixed solution is stirred at a temperature of 30° C. to 40° C. for 10 to 30 minutes to obtain a first reaction solution. The mechanochromic compound is added to the first reaction solution, and the first reaction solution is stirred for 5 to 15 minutes after the addition to obtain a core material prepolymer.

[0041] The core material prepolymer and the polyurea resin prepolymer are mixed to obtain a fourth mixed solution, and the pH of the fourth mixed solution is adjusted to 3-4.

[0042] The fourth mixed solution is stirred at a temperature of 60° C. to 70° C. for 2 h to 3 h to obtain a suspension containing microcapsules.

[0043] The microcapsule suspension is filtered, purified and dried to obtain microcapsules.

[0044] In a third aspect, an automobile part is provided. The automobile part comprises the polypropylene composition of any one of the possible embodiments described above; or the automobile part comprises the polypropylene material obtained by the preparation method of any one of the possible embodiments described above.

[0045] According to the above technical means, the present application can obtain automobile parts that are easy to monitor damage and have good creep resistance.

[0046] Therefore, the above technical features of the present application have the following beneficial effects:

[0047] (1) The present application includes a microcapsule in the polypropylene composition. On the one hand, the microcapsule can be used as a nucleating agent to transform the nucleation of the polypropylene composition from the original homogeneous phase to the heterogeneous phase, accelerate the crystallization rate, refine the grain structure, and cooperate with other components to effectively improve the mechanical strength and creep resistance of the polypropylene composition, and shorten the molding cycle of polypropylene materials and parts. On the other hand, the microcapsule can make the color difference between the crack area and the non-crack area appear when microcracks are generated in the polypropylene material and its parts due to external force, so that the mechanical damage state of the polypropylene material and parts can be conveniently, timely and effectively monitored.

[0048] (2) The present application improves the compatibility of organic molecules and reinforcing fibers in the polypropylene composition components by using a screw assembly including a reverse transport block in the polypropylene material preparation method, reduces the damage to the reinforcing fibers and microcapsules during the blending extrusion process, and increases the retention length of the fibers on the basis of good dispersion of the reinforcing fibers, thereby improving the mechanical properties and creep resistance of the polypropylene material, and improving the accuracy of monitoring the mechanical damage state of the polypropylene material and parts.

[0049] (3) The polypropylene composition of the present application has low raw material price and simple process requirements, which is conducive to improving production efficiency and cost control and is suitable for large-scale production.

[0050] (4) This application effectively solves the contradiction between fiber retention length and fiber dispersion in the reinforced fiber composite extrusion process by optimizing the polypropylene material preparation equipment and process, and provides a set of practical and effective solutions for the production of polypropylene materials. The solution is not limited to this application, but can also be used for other fiber reinforced material systems.

[0051] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] The drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present application, and together with the specification are used to explain the principles of the present application, and do not constitute an improper limitation on the present application.

[0053] Figure 1 is a schematic diagram of a preparation process of a polypropylene material according to an exemplary embodiment;

[0054] Figure 2 is a structural diagram of a twin-screw extruder unit according to an exemplary embodiment;

[0055] Figure 3 is a partial structural diagram of a screw assembly of a twin-screw extruder according to an exemplary embodiment;

[0056] Figure 4 is an electron microscope image showing a compatibility effect of a reinforcing fiber according to an exemplary embodiment;

[0057] Figure 5A is a schematic diagram of a preparation principle and process of a microcapsule according to an exemplary embodiment;

[0058] Figure 5B is a schematic diagram of a preparation principle and process of a microcapsule according to another exemplary embodiment;

[0059] Figure 6 is an electron microscope image of a microcapsule according to an exemplary embodiment;

[0060] Figure 7 is another electron microscope image of a microcapsule according to an exemplary embodiment. DETAILED DESCRIPTION

[0061] In order to enable ordinary persons in the art to better understand the technical solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the accompanying drawings.

[0062] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present application. On the contrary, they are merely examples of devices and methods consistent with some aspects of the present application as detailed in the attached claims.

[0063] Polypropylene is a common general-purpose plastic with high cost-effectiveness and wide application, and there is a lot of research in the industry. In the related technology, a dimensionally stable and creep-resistant long glass fiber reinforced polypropylene composite material and a preparation method thereof are provided. By adding a nucleating agent or a filler modifier to cooperate with the long glass fiber, the common warping phenomenon of the long glass fiber reinforced polypropylene material is alleviated, and the dimensional stability of the material is improved. The disadvantage is that the strength of the prepared material is insufficient, especially the tensile strength and bending strength representing the strength and rigidity of the material.

[0064] In another related technology, a creep-discoloring glass fiber reinforced polypropylene material and a preparation method are provided. In this scheme, a spiropyran photochromic compound is grafted onto the glass fiber. When the material is subjected to external force, the spiropyran CO bond on the glass fiber undergoes heterolytic cleavage to generate an open-ring cyanine compound. At this time, the conjugated chain of the compound molecule is reformed and emits red fluorescence, and the material itself has a color-changing function. However, during production, the screw exerts a large shear force on the glass fiber, so the grafted spiropyran photochromic compound on the glass fiber is easily damaged by the shear force. When the material is extruded, it will undergo heterolytic cleavage in advance to generate an open-ring cyanine compound, and the color-changing effect will occur in advance. Therefore, this scheme is less effective in monitoring the mechanical damage state of fiber-reinforced parts. In addition, the material mechanical strength of this scheme is weak, and it is easy to creep during use, so its application range is limited.

[0065] In view of the above problems, the object of the present invention is to provide a polypropylene composition, a method for preparing a polypropylene material and an automotive part, so as to realize convenient, timely and effective monitoring of the mechanical damage state of fiber reinforced plastic parts.

[0066] Based on this, the embodiment of the present application provides a polypropylene composition, whose mechanical damage can be monitored quickly, effectively and easily. A polypropylene composition, in terms of mass percentage, the components of the polypropylene composition include: component A: 100 parts, and microcapsules: 2 to 5 parts. Among them, in terms of mass percentage, component A includes: reinforcing fiber: 5% to 40%, first compatibilizer: 3% to 5%, and the balance is polypropylene. The core material of the microcapsule includes a mechanochromic compound.

[0067] For example, the polypropylene composition may include microcapsules in an amount of 2 parts, 3 parts, 4 parts, 5 parts by weight, etc.

[0068] For example, the mass percentage of the reinforcing fibers included in component A may be 5%, 10%, 15%, 25%, 30%, 35% or 40%, etc.

[0069] For example, the mass fraction of the first compatibilizer included in component A may be 3%, 4% or 5%, etc.

[0070] Based on this scheme, the polypropylene used in this application as a matrix material component can provide support and protection, and the use of reinforcing fibers can improve the overall performance of the material. The use of 3% to 5% of the first compatibilizer can improve the compatibility between the component materials, thereby enhancing the overall strength of the polypropylene composition, ensuring the close combination between the component materials and the polypropylene resin, and avoiding stress concentration and creep deformation. The use of 2 to 5 parts of microcapsules can play at least two roles. On the one hand, the microcapsules can be used as nucleating agents in the molten state of the material during the preparation of polypropylene materials, so that the nucleation process is transformed from the original homogeneous phase to the heterogeneous phase, which accelerates the crystallization rate, refines the grain structure, can shorten the preparation cycle, and improve the mechanical strength and creep resistance of the material. On the other hand, as a component of the polypropylene composition, when the polypropylene composition is subjected to external force and produces microcracks, the microcracks tear the microcapsules, and the mechanochromic compound in the core material present in the microcapsules can undergo changes in structure or electronic state due to the external force, resulting in a larger conjugated structure, which makes it present a different color from the microcapsules under fluorescence, so that the crack area has a color difference different from the non-crack area, so that the materials and parts prepared by the polypropylene composition can conveniently, timely and effectively monitor the mechanical damage state. For example, the mechanochromic compound included in the core material can be 2-anthryl-4,5-diphenylimidazole, the structure of which is shown in (a), and the molecular formula C 29 H 20 N2, whose structure contains a carbazole ring, two benzene rings, and an anthracene group connected to the carbazole, has a molecular weight of 396.48. When subjected to external force, the compound can be transformed into a compound with a structure as shown in (b), which can be green under fluorescence and can be easily detected.

[0071]

[0072] In some embodiments, the mechanochromic compound includes at least one of carbazole and its derivatives, spiropyran and its derivatives, spirothiopyran and its derivatives, coumarin dimer and its derivatives, cyclobutane peroxide and its derivatives, rhodamine and its derivatives, and isothiocyanic acid and its derivatives.

[0073] Here, carbazole and its derivatives can also be understood as carbazole compounds, including carbazole and compounds containing carbazole groups. For the understanding of spiropyran and its derivatives, spirothiopyran and its derivatives, coumarin dimer and its derivatives, cyclobutane peroxide and its derivatives, rhodamine and its derivatives, isothiocyanic acid and its derivatives, please refer to the description of carbazole and its derivatives, which will not be repeated here.

[0074] In some embodiments, the shell material of the microcapsules includes polyurea resin.

[0075] Urea-formaldehyde resin has good compatibility, which makes the microcapsules more universal and can be used to prepare various types of mechanochromic fiber-reinforced nylon, mechanochromic fiber-reinforced acrylonitrile-butadiene-styrene copolymer resin (ABS resin), mechanochromic fiber-reinforced polypropylene, etc.

[0076] In some embodiments, Figure 6 As shown, the particle size of the microcapsules ranges from 5 μm to 30 μm.

[0077] For example, the particle size of the microcapsule may be 2 μm, 10 μm, 16 μm, 23 μm, 30 μm, or the like.

[0078] In some embodiments, the reinforcing fiber includes carbon fiber and glass fiber; by mass percentage, component A includes: carbon fiber: 5% to 40%, glass fiber: 5% to 40%, first compatibilizer: 3% to 5%, and the balance is polypropylene.

[0079] For example, the mass percentage of carbon fibers included in component A may be 5%, 15%, 20%, 30% or 40%, etc.

[0080] For example, the mass percentage of glass fiber included in component A may be 5%, 15%, 20%, 30% or 40%, etc.

[0081] For example, the mass percentage of the first compatibilizer included in component A may be 3%, 3.5%, 4%, 4.5% or 5%, etc.

[0082] Based on this scheme, when the mass percentage of carbon fiber included in component A is 5% to 40%, carbon fiber can be used as a reinforcement of the polypropylene composition, increase the strength and rigidity of the polypropylene material, and can also effectively disperse stress and reduce the creep deformation of the material under high temperature or high stress. When the mass percentage of glass fiber included in component A is 5% to 40%, glass fiber, as a reinforcement of the polypropylene composition, can improve the comprehensive performance of the polypropylene material, including strength and hardness, and can reduce the thermal expansion coefficient of the polypropylene material, reduce thermal stress, thereby helping to improve the heat resistance and creep resistance of the polypropylene material. When the mass percentage of the first compatibilizer included in component A is 3% to 5%, the compatibility between the component materials can be improved, so that the close combination between the component materials and the polypropylene resin can be achieved, and the overall strength of the polypropylene composition can be further improved to avoid stress concentration and creep deformation.

[0083] In some embodiments, the diameter of the glass fiber is 5 μm to 15 μm.

[0084] In some embodiments, the diameter of the carbon fibers is 5 μm to 15 μm.

[0085] When the diameter of glass fiber or carbon fiber is large (for example, greater than 15 μm), the interaction between reinforcing fiber and polypropylene is weakened, and the reinforcing effect of the polypropylene composition is reduced; when the diameter of glass fiber or carbon fiber is too small (<5 μm), the cost may increase.

[0086] For example, the diameter of the glass fiber may be 5 μm, 8 μm, 10 μm, 13 μm, 15 μm, etc.

[0087] For example, the glass fiber can be a surface-treated continuous alkali-free glass fiber, such as 2400TEX series glass fiber from China Jushi Group, Chongqing International Composite Glass Co., Ltd., OC Company, and Taishan Fiberglass Group.

[0088] For example, the diameter of the carbon fiber may be 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, etc.

[0089] For example, the carbon fiber can be a surface-treated continuous carbon fiber, such as Japan Toray and Shanghai Petrochemical T700 series carbon fiber.

[0090] In some embodiments, the melt flow rate of the polypropylene under preset conditions is 10 g / 10 min to 80 g / 10 min.

[0091] Exemplarily, the preset conditions may be 230° C. and 2.16 kg.

[0092] For example, the melt flow rate of polypropylene under preset conditions may be 10 g / 10 min, 25 g / 10 min, 40 g / 10 min, 55 g / 10 min, 80 g / 10 min, or the like.

[0093] Based on this scheme, the melt flow rate is an important indicator reflecting the fluidity and processing performance of the polymer in the molten state. When the melt flow rate of polypropylene under preset conditions is within the range of 10g / 10min to 80g / 10min, the polypropylene composition has good fluidity, so that during the processing of the polypropylene material, the mold can be filled more evenly, and the generation of bubbles and defects can be reduced, thereby obtaining parts with smooth surface and stable dimensions.

[0094] In some embodiments, the polypropylene composition further comprises, by weight, at least one of: an antioxidant: 1 to 3 parts; and a lubricant: 0.5 to 3 parts.

[0095] For example, the polypropylene composition may include 1 part, 2 parts, 3 parts by weight of the antioxidant, etc.

[0096] For example, the polypropylene composition may include 0.5 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts by weight of the lubricant, etc.

[0097] Based on this scheme, the polypropylene composition uses 1 to 3 parts of antioxidants to delay and inhibit the degradation process of the polypropylene composition by stopping the chain oxidation reaction, inhibiting the autocatalytic effect of free radicals, and inhibiting the activity of metal ions, thereby alleviating the performance degradation of the polypropylene composition. The use of 0.5 to 3 parts of lubricants can reduce the friction between raw materials and between materials and processing equipment surfaces, improve the fluidity of the melt, and enhance the processability of the polypropylene composition.

[0098] In some embodiments, the first compatibilizer includes a compatible component, or the first compatibilizer includes a polymer and a compatible component grafted to the polymer; wherein the compatible component includes at least one of maleic anhydride and its derivatives, compounds containing epoxy groups, carboxylic acids and their derivatives, and acrylic acid glycidol and its derivatives.

[0099] Here, for the understanding of maleic anhydride and its derivatives, carboxylic acid and its derivatives, glycidyl acrylate and its derivatives, reference may be made to the aforementioned description of carbazole and its derivatives, which will not be repeated here.

[0100] The melt flow rate of the first compatibilizer is 0.05-1000 g / 10 min, and the grafting rate is 0.05-3%. Preferably, the first compatibilizer is a compatible component grafted polypropylene (PP-g-MAH), and the melt flow rate is 100-800 g / 10 min.

[0101] Based on this scheme, the compatibilizer reduces the interfacial tension between different polymer components, increases the thickness of the interfacial layer, and prevents the dispersed phase from condensing, so that the components of the polypropylene composition can be mixed more evenly, thereby improving the overall performance of the polypropylene composition. In addition, active substances such as maleic anhydride and its derivatives, epoxies, carboxylic acids, and acrylic acid glycidol can cross-link with polypropylene molecular chains, thereby enhancing the interaction between polypropylene molecular chains, helping to improve the compatibility of the components of the polypropylene composition, allowing different components to be mixed more evenly, and making the component materials of the polypropylene composition closely combined with the polypropylene, avoiding the occurrence of stress concentration and creep deformation.

[0102] In some embodiments, the lubricant includes at least one of silicone and its derivatives, erucamide and its derivatives, stearic acid and its derivatives, and vinyl bisstearamide and its derivatives.

[0103] In some embodiments, the antioxidant includes at least one of hindered phenols and their derivatives, phosphites and their derivatives, and amines and their derivatives.

[0104] In order to further enhance the mechanical properties and creep resistance of long glass fiber creep-resistant reinforced polypropylene materials, a long glass fiber and long carbon fiber composite reinforced polypropylene material and a preparation method thereof are provided in the related art. The creep-resistant fiber reinforced polypropylene material is mainly prepared by an impregnation method. However, it is not clearly disclosed how the long carbon fiber and the long glass fiber are pulled out from an impregnation grinding mouth, and how to ensure the mixing uniformity between the glass fiber and the carbon fiber, which becomes the main obstacle to subsequent large-scale applications.

[0105] In another related technology, a carbon / glass fiber composite reinforced polypropylene material and a preparation method thereof are provided. In this scheme, glass fiber, carbon fiber and other filler components are directly fed into an extruder to produce the material by conventional extrusion granulation. During the process, the fiber, filler and resin are surface treated to improve the compatibility between the components in the formula and improve the material properties. However, the effect of the fiber retention length on the material properties is not considered, and the improvement of the material properties is limited. In addition, this scheme does not describe the creep of the material.

[0106] In another related technology, a long glass fiber and long carbon fiber composite reinforced polypropylene material and a preparation method thereof are provided. This method uses a conventional extrusion granulation processing method to directly feed glass / carbon fiber longer short fibers and some other filler components into the extrusion granulation process, and does not optimize and improve the fiber retention length and the compatibility of carbon / glass fiber / polypropylene resin, resulting in the prepared material having low strength, failing to achieve the true enhancement and modification expectations, and failing to meet the use requirements of related high-strength and creep components.

[0107] In a second aspect, a method for preparing the polypropylene material in the above embodiment is provided.

[0108] The method for preparing the polypropylene material comprises: blending and extruding the components in the polypropylene composition according to any one of the above embodiments to obtain the polypropylene material.

[0109] Illustratively, the extrusion temperature may be 200° C. to 250° C., such as 200° C., 210° C., 220° C., 230° C., 240° C., or 250° C., etc.

[0110] Illustratively, the vacuum degree may be -0.1 MPa to 0 MPa, for example, -0.1 MPa, -0.08 MPa, -0.06 MPa, -0.04 MPa, -0.02 MPa or 0 MPa.

[0111] Illustratively, the rotation speed of the twin-screw extruder may be 300 rpm to 400 rpm, such as 300 rpm, 325 rpm, 350 rpm, 375 rpm or 400 rpm.

[0112] In some embodiments, Figure 2 and Figure 3As shown, the first direction X is parallel to the extension direction of the screw assembly and is the direction from the feed port of the twin-screw extruder to the discharge port. Figure 3 As shown, the screw assembly 6 of the twin-screw extruder along the first direction X is divided into a conveying section Q1, a melting section Q2, a plasticizing section Q3 and a discharge section Q4 which are arranged in sequence, wherein the conveying section Q1, the melting section Q2 and the plasticizing section Q3 include a plurality of forward shear blocks; the melting section Q2 and the plasticizing section Q3 also include at least one reverse transport block.

[0113] It should be noted that Figure 2 It is a structural diagram of a twin-screw extruder unit, wherein 1 is the main hopper, 2 is the gearbox, 3 is the extruder frame, 4 is the main motor, 5 is the main feed port, 6 is the extruder screw, 7 is the machine cover, 8 is the glass fiber, 9 is the carbon fiber, 10 is the first side feed port, 11 is the temperature control system, 12 is the transmission shaft, 13 is the barrel, 14 is the main feed motor, and 15 is the second side feed port. Figure 3 It is a partial diagram of the screw assembly structure of a twin-screw extruder, wherein 6-1 is the vacuum port, 6-2 is the exhaust zone of the side feeding port, 6-3 is the exhaust zone of the side feeding port, 6-4 is the first exhaust zone of the melting section, 6-5 is the second exhaust zone of the melting section, and 6-6 is the main feeding port.

[0114] After the raw materials of the polypropylene composition are mixed, during the extrusion process of the material, multiple forward shear blocks and at least one reverse transport are used in combination, so that the dispersion of the carbon fiber and the glass fiber in the material is enhanced, the dispersion of the reinforcing fiber in the polypropylene composition can be improved, and the contact surface between the reinforcing fiber and the functional group of the polypropylene graft is increased, thereby improving the compatibility of the reinforcing fiber and the polypropylene. Figure 4 As shown, Figure 4 (a) is a polypropylene material prepared by a screw assembly without a reverse transport block, Figure 4 (b) is a polypropylene material prepared by a screw assembly including a reverse transport block. It can be seen that Figure 4 The fibers in the polypropylene material obtained in (b) have good compatibility with polypropylene.

[0115] In some embodiments, the stagger angle of the forward shear blocks ranges from 30° to 60°.

[0116] For example, the stagger angle of the positive shear block may be 30°, 40°, 45°, 60°, etc.

[0117] Table 1 below shows the different positions of at least one reverse transport block in the melting section Q2 and the plasticizing section Q3 under different screw lengths, as well as the different staggered angles of multiple forward shear blocks. After combination, there are the following 6 combinations, but it is not limited to this. The properties of the polypropylene materials obtained under these 6 combinations are tested below, and the details are shown in Table 2.

[0118] Table 1 Screw specific combination

[0119]

[0120]

[0121]

[0122]

[0123] Here, L is a reverse transport block, 32 / 16L means a reverse transport block with a lead (the axial distance generated by rotating a point on the screw edge 360° along the spiral line with the core axis as the axis) of 32mm and a length of 16mm; A means the top, 32 / 32A means the top thread block with a lead of 32mm and a length of 32mm; K means a shear block, K45° / 5 / 48 means a forward shear block composed of 5 shear pieces with a staggered angle of 45° and a total length of 48mm.

[0124] Table 2 Characterization of fiber and microcapsule dispersion and shearing effect

[0125]

[0126] Here, the fiber retention length is tested by an optical fiber scope on the glass fiber remaining after the modified extruded particles are burned; the notched impact strength is prepared and tested in accordance with the requirements of ISO179-1; the number of fiber agglomerates is measured by injection molding the prepared material into a 150*100*3.2mm sample and counting the number of undispersed fiber clusters on the sample; the sample fluorescent color effect is measured by injection molding the prepared material into a 150*100*3.2mm sample and observing the fluorescent color of the sample under ultraviolet light; the sample mechanical damage monitoring effect is measured by injection molding the prepared material into a 150*100*3.2mm sample, using external force to create cracks, and then observing the fluorescent color of the sample cracks under ultraviolet light.

[0127] As shown in Table 1 and Table 2 above, it can be seen from the data of combination 1 and combination 2 that the addition of the reverse transport block can reduce the shear force and increase the retention length of the reinforcing fiber; it can be seen from the data of combination 3 and combination 4 that when the staggered angle of the forward shear block is large, the retention length and the material notch impact strength are small, indicating that when the staggered angle of the forward shear block is large, it will affect the material retention length, and then affect the material performance. Therefore, by optimizing and adjusting the screw combination of the twin-screw extruder, such as combination 4 to combination 6 in Table 1, the staggered angle of the forward shear block is appropriately reduced. The test results are shown in Table 2. The fiber retention length of combination 4 to combination 6 is longer than that of combination 1 and combination 3, and the number of fiber agglomerations is significantly reduced, indicating that the combination of the appropriate staggered angle of the forward shear block and the reverse transport block can not only increase the fiber retention length, but also ensure the dispersion of the fiber. This is because the adjustment of the screw combination weakens the shear strength in the preparation process of the polypropylene material, increases the fiber retention length in the polypropylene composition, and can improve the creep resistance of the polypropylene material.

[0128] Moreover, the fluorescent color effects of the samples of combination 4 to combination 6 are all blue fluorescence, indicating that the microcapsules in the polypropylene materials corresponding to combination 4 to combination 6 are more complete before being subjected to force. After being mechanically damaged, the microcapsules rupture, and there is a large amount of green fluorescence at the cracks, making the damage detection more obvious, further improving the accuracy of monitoring the mechanical damage state of fiber reinforced plastic parts.

[0129] Based on this scheme, by adjusting and optimizing the extruder screw combination, the shear arrangement of the screw thread group can be reduced to reduce the destructive force of the screw on the fiber and microcapsule, promote the compatibility between the fiber and the raw materials in the polypropylene composition, ensure the dispersion of the fiber, increase the fiber retention length, and thus improve the creep resistance of the polypropylene composition; the integrity of the microcapsule can be improved, and the damage of the microcapsule during the preparation process can be avoided, so that the microcapsule has good integrity in the polypropylene material and the parts prepared therefrom. On this basis, when the polypropylene composition and its products are subjected to external force, the damage state of the material and the parts prepared therefrom can be accurately judged.

[0130] In some embodiments, Figure 5A As shown, the method for preparing the polypropylene material further includes preparing microcapsules. The preparation of microcapsules includes S1 to S8.

[0131] S1: adding 0.5-1.5 parts by mass of urea to 1.5-2.5 parts by mass of formaldehyde solution, and adding an alkaline catalyst to the formaldehyde solution to obtain a first mixed solution with a pH value of 7-8.

[0132] For example, the mass fraction of urea may be 0.5, 1 or 1.5, etc.

[0133] For example, the mass fraction of the formaldehyde solution may be 1.5, 2 or 2.5, etc.

[0134] Illustratively, the pH value may be 7, 7.5, or 8, etc.

[0135] S2: Stir the first mixed solution at a temperature of 60° C. to 70° C. for 1 h to 2 h to obtain a polyurea resin prepolymer.

[0136] Illustratively, the temperature may be 60°C, 65°C, or 60°C, etc.

[0137] For example, the stirring time may be 1 h, 1.5 h or 2 h, etc.

[0138] S3: 9 to 11 parts by mass of styrene monomer, 2 to 4 parts by mass of a cross-linking agent, and 1 to 3 parts by mass of a second compatibilizer are mixed to obtain a second mixed solution, and an emulsifier is added to the second mixed solution so that the ratio of the mass of the emulsifier to the mass of the second mixed solution is 1 to 3 to obtain a third mixed solution.

[0139] For example, the mass fraction of styrene monomer may be 9, 10 or 11, etc.

[0140] Illustratively, the styrene monomer is, for example, a styrene standard solution, a 100 μg / ml styrene methanol solution.

[0141] For example, the mass fraction of the second compatibilizer may be 1, 2, or 3, etc.

[0142] Exemplarily, the second compatibilizer is, for example, polyethylene glycol.

[0143] For example, the mass fraction of the cross-linking agent may be 2, 3 or 4, etc.

[0144] Exemplarily, the cross-linking agent is, for example, epoxy resin.

[0145] S4: stirring the third mixed solution at a temperature of 30° C. to 40° C. for 10 min to 30 min to obtain a first reaction solution.

[0146] Illustratively, the temperature may be 30°C, 35°C, 40°C, or the like.

[0147] For example, the stirring time may be 10 min, 20 min, 30 min, etc.

[0148] S5: adding the mechanochromic compound to the first reaction solution, and stirring the first reaction solution for 5 minutes to 15 minutes after the addition to obtain a core material prepolymer.

[0149] For example, the stirring time may be 5 min, 10 min, or 15 min, etc.

[0150] S6: Mix the core material prepolymer and the polyurea resin prepolymer to obtain a fourth mixed solution, and adjust the pH of the fourth mixed solution to 3-4.

[0151] Illustratively, the pH value may be 3, 3.5 or 4, etc.

[0152] S7: stirring the fourth mixed solution at a temperature of 60° C. to 70° C. for 2 h to 3 h to obtain a suspension containing microcapsules.

[0153] Illustratively, the temperature may be 60°C, 65°C, or 60°C, etc.

[0154] For example, the stirring time may be 2 h, 2.5 h or 3 h, etc.

[0155] S8: filtering, purifying and drying the microcapsule suspension to obtain microcapsules.

[0156] Based on this scheme, the first step is to form a prepolymer of polyurea resin. After mixing urea and formaldehyde solutions, under the action of a catalyst, the pH value is adjusted to 7-8 to maintain the stability of the reaction system, and the reaction rate is controlled. The reaction is carried out at a temperature of 60-70°C for 1-2 hours to allow urea and formaldehyde to form a prepolymer of polyurea resin through a condensation reaction; then a first reaction solution is formed, styrene monomer, a crosslinking agent, and a compatibilizer are mixed to obtain a third mixed solution, an emulsifier is added to form a stable emulsion system, and the mixture is stirred at a temperature of 30-40°C for 10-30 minutes to provide a basis for the core material for the subsequent formation of microcapsules; then a core material prepolymer is formed, The mechanochromic compound is added to the first reaction solution, and is evenly dispersed in the core material by stirring to obtain a core prepolymer; then a microcapsule suspension is formed to mix the core prepolymer with the polyurea resin prepolymer. At this time, the core material is wrapped by the polyurea resin prepolymer to form a shell layer of the microcapsule, and the pH value of the system is adjusted to 3-4, which is conducive to further condensation and curing of the polyurea resin to form a stable shell structure. The reaction is carried out at 60°C to 70°C for 2-3h, and the polyurea resin is completely cured to form a complete microcapsule structure; finally, filtration is performed to remove unreacted impurities and larger particles, and purification can further remove impurities. After drying, microcapsules are obtained.

[0157] In a third aspect, the present application provides an automobile part, wherein the automobile part comprises the polypropylene composition of any one of the above embodiments; or the automobile part comprises the polypropylene material obtained by the preparation method of any one of the above embodiments.

[0158] Exemplarily, automotive parts are, for example, plastic front-end modules, gas / electric pedals, fiber-reinforced polypropylene brackets in the fields of body / interior and exterior trim, battery trays, lamp brackets, etc.

[0159] In the following, the preparation process of the polypropylene composition is specifically and exemplarily described in combination with the above preparation method.

[0160] The raw materials used in the examples and preparation examples of the present application are as follows: polypropylene, produced by Zhenhai Petrochemical, brand M60T, the material melt index is about 60g / min at 230°C and 2.16Kg. Glass fiber, produced by Jushi Group, model 2400tex, brand ER13-2000-988A alkali-free continuous glass fiber. Carbon fiber, produced by Shanghai Petrochemical, model T700 1650tex continuous carbon fiber. Lubricant, composed of erucamide, EBS, and stearic acid, the ratio of the three is 1:1:1, wherein erucamide is purchased from Xipuheda, and EBS and stearic acid are purchased from Nanjing Pasteur. Compatibilizer, PP-g-MAH, Shanghai Rizhisheng, brand CMG9801. The standard solution of styrene is a 100μg / ml methanol solution. Mechanochromic compound, produced by Xi'an Qiyue Biotechnology Co., Ltd., CAS 6931-28-8, molecular weight 396.48, λem 477nm, λem about 500nm after grinding, the chemical structure of the compound is All raw materials in this application are commercially available products, which are intended to fully disclose the raw materials in this application and should not be construed as limiting the sources of the raw materials.

[0161] The following is an example of the preparation of microcapsules.

[0162] Preparation Example 1

[0163] like Figure 5B As shown, the microcapsules of Preparation Example 1 are prepared by the following steps:

[0164] S1: Add urea to a three-necked flask containing formaldehyde solution in a mass ratio of 1:2, start the electromagnetic stirrer, stir the mixture for 10 minutes at a stirring speed of 200-300rpm; then slowly add hexamethylenetetramine (alkaline catalyst), adjust the pH value of the mixture to 7-8, then move the mixed solution to a constant temperature water bath at 60℃-70℃, start the electromagnetic stirrer again, stir at a speed of 400rpm-500rpm, and continue to stir the mixed solution for 1-2h;

[0165] S2: Stir and mix the styrene standard solution (styrene monomer), epoxy resin (cross-linking agent), and polyethylene glycol (compatibilizer) in a mass ratio of 10:3:2 to form a mixed solution, and then add a 1% sodium dodecylbenzene sulfonate aqueous solution (emulsifier) ​​to make the mass ratio of the sodium dodecylbenzene sulfonate aqueous solution to the above mixed solution 1:2 to form a first reaction solution, and then move it to a constant temperature water bath at 30°C to 40°C, start the electromagnetic stirrer and continue stirring for 20 minutes at a stirring speed of 600rpm to 700rpm; then add the mechanochromic compound and react for 10 minutes at a stirring speed of 100rpm to 200rpm;

[0166] S3: slowly adding the mixed solution obtained in step S2 to the mixed solution obtained in step S1, slowly adjusting the pH value of the system to 3-4 using phosphoric acid or dilute hydrochloric acid, and then continuing to stir the mixture in a constant temperature water bath at 60°C-70°C for 2-3 hours to obtain a microcapsule suspension; then filtering with filter paper, dissolving with distilled water and ethanol, rinsing, and drying to obtain microcapsules such as Figure 6 and Figure 7 shown.

[0167] The following are examples of polypropylene compositions and corresponding polypropylene materials.

[0168] Example 1-1

[0169] The raw materials of the polypropylene composition of Example 1-1 are calculated by mass as follows: 57 parts of polypropylene, 35 parts of glass fiber, 5 parts of carbon fiber, 3 parts of compatibilizer (PP-g-MAH), 1 part of antioxidant (including 0.3 parts and 0.2 parts of antioxidants 1010 and 168 respectively), 1.5 parts of lubricant (including 0.5 parts of erucamide, 0.5 parts of stearic acid, and 0.5 parts of EBS), and 5 parts of microcapsules; wherein, the microcapsules are selected from the microcapsules prepared in Preparation Example 1.

[0170] The polypropylene material of Example 1-1 is prepared by the following preparation method: Figure 1 and Figure 2 As shown, polypropylene, antioxidant, lubricant and compatibilizer are mixed evenly and then added to the twin-screw extruder from the main feed port 5, glass fiber and carbon fiber are fed from the first side feed port 10 at a speed of 100 rpm, and microcapsules are fed from the second side feed port 15. The extruder screw combination is combination 1 in Table 1 for extrusion granulation and injection molding to prepare standard specimens. Among them, the extrusion melt blending temperature is 230°C, and the extrusion vacuum is turned on and the vacuum degree is maintained at -0.08MPa.

[0171] Example 1-2

[0172] The components and amounts of the polypropylene composition of Example 1-2 are the same as those of Example 1-1.

[0173] The preparation method of the polypropylene material of Example 1-2 is the same as that of Example 1-1, except that the screw combination of the twin-screw extruder is combination 2 in Table 1.

[0174] Examples 1-3

[0175] The components and amounts of the polypropylene composition of Example 1-3 are the same as those of Example 1-1.

[0176] The preparation method of the polypropylene material of Example 1-3 is the same as that of Example 1-1, except that the screw combination of the twin-screw extruder is combination 3 in Table 1.

[0177] Examples 1-4

[0178] The components and amounts of the polypropylene composition of Example 1-4 are the same as those of Example 1-1.

[0179] The preparation method of the polypropylene material of Example 1-4 is the same as that of Example 1-1, except that the screw combination of the twin-screw extruder is combination 4 in Table 1.

[0180] Examples 1-5

[0181] The components and amounts of the polypropylene composition of Example 1-5 are the same as those of Example 1-1.

[0182] The preparation method of the polypropylene material of Example 1-5 is the same as that of Example 1-1, except that the screw combination of the twin-screw extruder is combination 5 in Table 1.

[0183] Examples 1-6

[0184] The components and amounts of the polypropylene composition of Example 1-6 are the same as those of Example 1-1.

[0185] The preparation method of the polypropylene material of Example 1-6 is the same as that of Example 1-1, except that the screw combination of the twin-screw extruder is combination 6 in Table 1.

[0186] Example 2-1

[0187] The components of the polypropylene composition of Example 2-1 are the same as those of Example 1-1, except that the amount of glass fiber is 30 parts and the amount of carbon fiber is 10 parts.

[0188] The preparation method of the polypropylene material of Example 2-1 is the same as that of Example 1-1.

[0189] Example 2-2

[0190] The components and amounts of the polypropylene composition of Example 2-2 are the same as those of Example 2-1.

[0191] The preparation method of the polypropylene material of Example 2-2 is the same, except that the screw combination of the twin-screw extruder is combination 2 in Table 1.

[0192] Example 2-3

[0193] The components and amounts of the polypropylene composition of Example 2-3 are the same as those of Example 2-1.

[0194] The preparation method of the polypropylene material of Example 2-3 is the same as that of Example 2-1, except that the screw combination of the twin-screw extruder is combination 3 in Table 1.

[0195] Embodiment 2-4

[0196] The components and amounts of the polypropylene composition of Example 2-4 are the same as those of Example 2-1.

[0197] The preparation method of the polypropylene material of Example 2-4 is the same as that of Example 2-1, except that the screw combination of the twin-screw extruder is combination 4 in Table 1.

[0198] Embodiment 2-5

[0199] The components and amounts of the polypropylene composition of Example 2-5 are the same as those of Example 2-1.

[0200] The preparation method of the polypropylene material of Example 2-5 is the same as that of Example 2-1, except that the screw combination of the twin-screw extruder is combination 5 in Table 1.

[0201] Embodiment 2-6

[0202] The components and amounts of the polypropylene composition of Example 2-6 are the same as those of Example 2-1.

[0203] The preparation method of the polypropylene material of Example 2-6 is the same as that of Example 2-1, except that the screw combination of the twin-screw extruder is combination 6 in Table 1.

[0204] Example 3-1

[0205] The components of the polypropylene composition of Example 3-1 are the same as those of Example 1-1, except that the amount of glass fiber is 20 parts and the amount of carbon fiber is 20 parts.

[0206] The preparation method of the polypropylene material of Example 3-1 is the same as that of Example 1-1.

[0207] Example 3-2

[0208] The components and amounts of the polypropylene composition of Example 3-2 are the same as those of Example 3-1.

[0209] The preparation method of the polypropylene material of Example 3-2 is the same as that of Example 3-1, except that the screw combination of the twin-screw extruder is combination 2 in Table 1.

[0210] Example 3-3

[0211] The components and amounts of the polypropylene composition of Example 3-3 are the same as those of Example 3-1.

[0212] The preparation method of the polypropylene material of Example 3-3 is the same as that of Example 3-1, except that the screw combination of the twin-screw extruder is combination 3 in Table 1.

[0213] Embodiment 3-4

[0214] The components and amounts of the polypropylene composition of Example 3-4 are the same as those of Example 3-1.

[0215] The preparation method of the polypropylene material of Example 3-4 is the same as that of Example 3-1, except that the screw combination of the twin-screw extruder is combination 4 in Table 1.

[0216] Embodiment 3-5

[0217] The components and amounts of the polypropylene composition of Example 3-5 are the same as those of Example 3-1.

[0218] The preparation method of the polypropylene material of Example 3-5 is the same as that of Example 3-1, except that the screw combination of the twin-screw extruder is combination 5 in Table 1.

[0219] Embodiment 3-6

[0220] The components and amounts of the polypropylene composition of Example 3-6 are the same as those of Example 3-1.

[0221] The preparation method of the polypropylene material of Example 3-6 is the same as that of Example 3-1, except that the screw combination of the twin-screw extruder is combination 6 in Table 1.

[0222] Example 4-1

[0223] The components of the polypropylene composition of Example 4-1 are the same as those of Example 1-1, except that the amount of glass fiber used is 10 parts and the amount of carbon fiber used is 30 parts.

[0224] The preparation method of the polypropylene material of Example 4-1 is the same as that of Example 1-1.

[0225] Example 4-2

[0226] The components and amounts of the polypropylene composition of Example 4-2 are the same as those of Example 4-1.

[0227] The preparation method of the polypropylene material of Example 4-2 is the same as that of Example 4-1, except that the screw combination of the twin-screw extruder is combination 2 in Table 1.

[0228] Example 4-3

[0229] The components and amounts of the polypropylene composition of Example 4-3 are the same as those of Example 4-1.

[0230] The preparation method of the polypropylene material of Example 4-3 is the same as that of Example 4-1, except that the screw combination of the twin-screw extruder is combination 3 in Table 1.

[0231] Example 4-4

[0232] The components and amounts of the polypropylene composition of Example 4-4 are the same as those of Example 4-1.

[0233] The preparation method of the polypropylene material of Example 4-4 is the same as that of Example 4-1, except that the screw combination of the twin-screw extruder is combination 4 in Table 1.

[0234] Embodiment 4-5

[0235] The components and amounts of the polypropylene composition of Example 4-5 are the same as those of Example 4-1.

[0236] The preparation method of the polypropylene material of Example 4-5 is the same as that of Example 4-1, except that the screw combination of the twin-screw extruder is combination 5 in Table 1.

[0237] Embodiment 4-6

[0238] The components and amounts of the polypropylene composition of Example 4-6 are the same as those of Example 4-1.

[0239] The preparation method of the polypropylene material of Example 4-6 is the same as that of Example 4-1, except that the screw combination of the twin-screw extruder is combination 6 in Table 1.

[0240] Example 5-1

[0241] The components of the polypropylene composition of Example 5-1 are the same as those of Example 1-1, except that the amount of glass fiber used is 5 parts and the amount of carbon fiber used is 35 parts.

[0242] The preparation method of the polypropylene material of Example 5-1 is the same as that of Example 1-1.

[0243] Example 5-2

[0244] The components and amounts of the polypropylene composition of Example 5-2 are the same as those of Example 5-1.

[0245] The preparation method of the polypropylene material of Example 5-2 is the same as that of Example 5-1, except that the screw combination of the twin-screw extruder is combination 2 in Table 1.

[0246] Example 5-3

[0247] The components and amounts of the polypropylene composition of Example 5-3 are the same as those of Example 5-1.

[0248] The preparation method of the polypropylene material of Example 5-3 is the same as that of Example 5-1, except that the screw combination of the twin-screw extruder is combination 3 in Table 1.

[0249] Example 5-4

[0250] The components and amounts of the polypropylene composition of Example 5-4 are the same as those of Example 5-1.

[0251] The preparation method of the polypropylene material of Example 5-4 is the same as that of Example 5-1, except that the screw combination of the twin-screw extruder is combination 4 in Table 1.

[0252] Example 5-5

[0253] The components and amounts of the polypropylene composition of Example 5-5 are the same as those of Example 5-1.

[0254] The preparation method of the polypropylene material of Example 5-5 is the same as that of Example 5-1, except that the screw combination of the twin-screw extruder is combination 5 in Table 1.

[0255] Embodiment 5-6

[0256] The components and amounts of the polypropylene composition of Example 5-6 are the same as those of Example 5-1.

[0257] The preparation method of the polypropylene material of Example 5-6 is the same as that of Example 5-1, except that the screw combination of the twin-screw extruder is combination 6 in Table 1.

[0258] Example 6-1

[0259] The components of the polypropylene composition of Example 6-1 are the same as those of Example 1-1, except that the amount of glass fiber used is 0 parts and the amount of carbon fiber used is 40 parts.

[0260] The preparation method of the polypropylene material of Example 6-1 is the same as that of Example 1-1.

[0261] Example 6-2

[0262] The components and amounts of the polypropylene composition of Example 6-2 are the same as those of Example 6-1.

[0263] The preparation method and component dosage of the polypropylene material of Example 6-2 are the same as those of Example 6-1, except that the screw combination of the twin-screw extruder is combination 2 in Table 1.

[0264] Example 6-3

[0265] The components and amounts of the polypropylene composition of Example 6-3 are the same as those of Example 6-1.

[0266] The preparation method of the polypropylene material of Example 6-3 is the same as that of Example 6-1, except that the screw combination of the twin-screw extruder is combination 3 in Table 1.

[0267] Example 6-4

[0268] The components and amounts of the polypropylene composition of Example 6-4 are the same as those of Example 6-1.

[0269] The preparation method of the polypropylene material of Example 6-4 is the same as that of Example 6-1, except that the screw combination of the twin-screw extruder is combination 4 in Table 1.

[0270] Example 6-5

[0271] The components and amounts of the polypropylene composition of Example 6-5 are the same as those of Example 6-1.

[0272] The preparation method of the polypropylene material of Example 6-5 is the same as that of Example 6-1, except that the screw combination of the twin-screw extruder is combination 5 in Table 1.

[0273] Example 6-6

[0274] The components and amounts of the polypropylene composition of Example 6-6 are the same as those of Example 6-1.

[0275] The preparation method of the polypropylene material of Example 6-6 is the same as that of Example 6-1, except that the screw combination of the twin-screw extruder is combination 6 in Table 1.

[0276] Example 7-1

[0277] The components of the polypropylene composition of Example 7-1 are the same as those of Example 1-1, except that the amount of glass fiber used is 40 parts and the amount of carbon fiber used is 0 parts.

[0278] The preparation method of the polypropylene material of Example 7-1 is the same as that of Example 1-1.

[0279] Example 7-2

[0280] The components and amounts of the polypropylene composition of Example 7-2 are the same as those of Example 7-1.

[0281] The preparation method of the polypropylene material of Example 7-2 is the same as that of Example 7-1, except that the screw combination of the twin-screw extruder is combination 2 in Table 1.

[0282] Example 7-3

[0283] The components and amounts of the polypropylene composition of Example 7-3 are the same as those of Example 7-1.

[0284] The preparation method of the polypropylene material of Example 7-3 is the same as that of Example 7-1, except that the screw combination of the twin-screw extruder is combination 3 in Table 1.

[0285] Example 7-4

[0286] The components and amounts of the polypropylene composition of Example 7-4 are the same as those of Example 7-1.

[0287] The preparation method of the polypropylene material of Example 7-4 is the same as that of Example 7-1, except that the screw combination of the twin-screw extruder is combination 4 in Table 1.

[0288] Example 7-5

[0289] The components and amounts of the polypropylene composition of Example 7-5 are the same as those of Example 7-1.

[0290] The preparation method of the polypropylene material of Example 7-5 is the same as that of Example 7-1, except that the screw combination of the twin-screw extruder is combination 5 in Table 1.

[0291] Example 7-6

[0292] The components and amounts of the polypropylene composition of Example 7-6 are the same as those of Example 7-1.

[0293] The preparation method of the polypropylene material of Example 7-6 is the same as that of Example 7-1, except that the screw combination of the twin-screw extruder is combination 6 in Table 1.

[0294] Example 8-1

[0295] The components and amounts of the polypropylene composition of Example 8-1 are the same as those of Example 7-1.

[0296] The polypropylene material of Example 8-1 was prepared by the following preparation method: Figure 1 and Figure 2As shown, polypropylene resin, antioxidant, lubricant, compatibilizer and microcapsule are mixed evenly and added to the twin-screw extruder from the main feeding port 5, glass fiber and carbon fiber are fed from the side feeding port 10 at a speed of 100 rpm, and the extruder screw combination is selected from the combination 1 in Table 1 for extrusion granulation and injection molding to prepare standard specimens. Among them, the extrusion melt blending temperature is 230°C, and the extrusion vacuum is opened and the vacuum degree is maintained at -0.08MPa.

[0297] Example 8-2

[0298] The components and amounts of the polypropylene composition of Example 8-2 are the same as those of Example 8-1.

[0299] The preparation method of the polypropylene material of Example 8-2 is the same as that of Example 8-1, except that the screw combination of the twin-screw extruder is combination 2 in Table 1.

[0300] Example 9-1

[0301] The components and amounts of the polypropylene composition of Example 9-1 are the same as those of Example 6-1.

[0302] The polypropylene material of Example 9-1 was prepared by the following preparation method: Figure 1 and Figure 2 As shown, polypropylene resin, antioxidant, lubricant, compatibilizer and microcapsule are mixed evenly and added to the twin-screw extruder from the main feeding port 5, glass fiber and carbon fiber are fed from the side feeding port 10 at a speed of 100 rpm, and the extruder screw combination is selected from the combination 1 in Table 1 for extrusion granulation and injection molding to prepare standard specimens. Among them, the extrusion melt blending temperature is 230°C, and the extrusion vacuum is opened and the vacuum degree is maintained at -0.08MPa.

[0303] Example 9-2

[0304] The components and amounts of the polypropylene composition of Example 9-2 are the same as those of Example 9-1.

[0305] The preparation method of the polypropylene material of Example 9-2 is the same as that of Example 9-1, except that the screw combination of the twin-screw extruder is combination 2 in Table 1.

[0306] Performance Testing

[0307] Test 1: Mechanical damage monitoring effect of the sample. The fiber-reinforced polypropylene material prepared in each embodiment was injection molded into a 150*100*3.2 mm sample. An external force was used to generate cracks. The fluorescent color of the sample was observed under ultraviolet light. The specific results are shown in Table 3 below.

[0308] Table 3 Mechanical damage monitoring effect of polypropylene material samples in different embodiments

[0309]

[0310]

[0311]

[0312] It can be concluded from Table 3 above that by adding microcapsules to the polypropylene composition, a large amount of green fluorescence is present at the cracks of the polypropylene material when it is subjected to external force, so that the polypropylene composition material and parts have the function of monitoring the mechanical damage state.

[0313] Test 2: Sample color change effect. The prepared polypropylene material was injection molded into a 150*100*3.2 mm sample. The fluorescent color of the sample was observed under ultraviolet light. The specific results are shown in Table 4 below.

[0314] Table 4 Color change effect of polypropylene material samples in different embodiments

[0315]

[0316]

[0317] It can be concluded from Table 4 that the sample fluorescent color effect of Examples 1-4 to 1-6, 2-4, 2-6, 3-4, 3-6, 4-4, 4-6, 5-4, 5-6, 6-4, 6-6 and 7-4 to 7-6 is a single blue fluorescence, compared with other Examples 1-1 to 1-3, 2-1 to 2-3, 3-1 to 3-3, 4-1 to 4-3, 5-1 to 7-6. The sample fluorescent color effect of Example 5-3, Example 6-1 to Example 6-3, Example 7-1 to Example 7-3, Example 8-1 to Example 8-2 and Example 9-1 to Example 9-2 is the coexistence of green fluorescence and blue fluorescence, so that when the polypropylene material is subjected to external force, the microcapsules are broken by the force, and a large amount of green fluorescence appears at the cracks, which can more accurately monitor the mechanical damage state. This may be related to that when the staggered angle range of multiple forward shear blocks of the screw assembly is 30° to 60° and a reverse transport block is used, the destructive force on the mechanochromic microcapsules can be reduced.

[0318] Test 3: (1) Fiber retention length: An optical fiber microscope was used to test and count the length of the glass fibers remaining after the modified extruded particles were burned. The specific results are shown in Table 5 below.

[0319] (2) Number of fiber agglomerates: The fiber-reinforced polypropylene materials prepared in the embodiments and comparative examples were injection molded into 150*100*3.2 mm samples, and the number of undispersed fiber agglomerates on the samples was counted; the specific results are shown in Table 5 below.

[0320] (3) The tensile creep properties are in accordance with GB / T 41061-2021: Test method for creep properties of fiber reinforced plastics. The results are shown in Table 5.

[0321] (4) Notched impact strength was tested according to GB / T 1043.1-2008, V-notch, 23°C. The results are shown in Table 5.

[0322] (5) The tensile strength was tested according to GB / T 1040.1-2006 at a speed of 5 mm / min. The results are shown in Table 5.

[0323] (6) The flexural modulus was tested according to GB / T 9341-2008 at a speed of 2 mm / min and a span of 64 mm. The results are shown in Table 5.

[0324] Table 5 Test results of polypropylene material samples of different embodiments

[0325]

[0326]

[0327]

[0328] It can be concluded from Table 5 above that the mechanical properties of Examples 1-1 to 9-2 are good, and the tensile creep strain rates of the polypropylene materials of Examples 1-4 to 1-6, Examples 2-4 to 2-6, Examples 3-4 to 3-6, Examples 4-4 to 4-6, Examples 5-4 to 5-6, Examples 6-4 to 6-6 and Examples 7-4 to 7-6 are small, which shows that the tensile creep strain rates of the polypropylene materials of Examples 1-4 to 1-6, Examples 2-4 to 2-6, Examples 3-4 to 3-6, Examples 4-4 to 4-6, Examples 5-4 to 5-6, Examples 6-4 to 6-6 and Examples 7-4 to 7-6 are small. The creep resistance of the polypropylene material in Example 7-6 is improved, which may be related to the relatively small number of fiber agglomerations and the relatively long fiber retention length of the polypropylene materials in Examples 1-4 to 1-6, 2-4 to 2-6, 3-4 to 3-6, 4-4 to 4-6, 5-4 to 5-6, 6-4 to 6-6 and 7-4 to 7-6. This is because when the staggered angles of the multiple forward shear blocks of the screw assembly range from 30° to 60° and a reverse transport block is used, the fiber retention length can be increased while ensuring the fiber dispersion, and the interface compatibility between the raw materials in the polypropylene composition can be improved.

[0329] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto, and any changes or substitutions within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A polypropylene composition, characterized in that The components of the polypropylene composition include, by mass: Component A: 100 parts, and microcapsules: 2 to 5 parts; Wherein, by mass percentage, component A comprises: reinforcing fiber: 5% to 40%, first compatibilizer: 3% to 5%, and the balance is polypropylene; the core material of the microcapsule comprises a mechanochromic compound.

2. The polypropylene composition according to claim 1, characterized in that The mechanochromic compound includes at least one of carbazole and its derivatives, spiropyran and its derivatives, spirothiopyran and its derivatives, coumarin dimer and its derivatives, cyclobutane peroxide and its derivatives, rhodamine and its derivatives, and isothiocyanic acid and its derivatives.

3. The polypropylene composition according to claim 1, characterized in that The shell material of the microcapsule includes polyurea resin.

4. The polypropylene composition according to claim 1, characterized in that The particle size of the microcapsule is in the range of 5 μm to 30 μm.

5. The polypropylene composition according to claim 1, characterized in that The reinforcing fibers include carbon fibers and glass fibers; Calculated by mass percentage, the component A includes: carbon fiber: 5% to 40%, glass fiber: 5% to 40%, first compatibilizer: 3% to 5%, and the balance is polypropylene.

6. The polypropylene composition according to claim 5, characterized in that The diameter of the glass fiber is 5 μm to 15 μm; and / or the diameter of the carbon fiber is 5 μm to 15 μm.

7. The polypropylene composition according to claim 1, characterized in that The melt flow rate of the polypropylene under preset conditions is 10 g / 10 min to 80 g / 10 min.

8. The polypropylene composition according to claim 1, characterized in that The first compatibilizer includes a compatibilizing component, or, The first compatibilizer includes a polymer and a compatible component grafted to the polymer; The compatible components include at least one of maleic anhydride and its derivatives, compounds containing epoxy groups, carboxylic acids and its derivatives, and glycidyl acrylate and its derivatives.

9. The polypropylene composition according to claim 1, characterized in that Also includes: At least one of an antioxidant: 1 to 3 parts and a lubricant: 0.5 to 3 parts.

10. The polypropylene composition according to claim 9, characterized in that The lubricant includes at least one of silicone and its derivatives, erucic acid amide and its derivatives, stearic acid and its derivatives, and vinyl bisstearamide and its derivatives.

11. The polypropylene composition according to claim 9, characterized in that The antioxidant includes at least one of hindered phenols and their derivatives, phosphites and their derivatives, and amines and their derivatives.

12. A method for preparing a polypropylene material, characterized in that: The method comprises: The components in the polypropylene composition according to any one of claims 1 to 11 are blended and extruded to obtain the polypropylene material.

13. The method for preparing a polypropylene material according to claim 12, characterized in that: The method specifically comprises: The raw materials are configured according to the components of the polypropylene composition according to any one of claims 1 to 11; The raw materials are fed into a twin-screw extruder through multiple feed ports, and extruded to obtain extruded materials; The extrudate is cooled, dried and pelletized to obtain the polypropylene material.

14. The method for preparing a polypropylene material according to claim 13, characterized in that: Along the first direction, the screw assembly of the twin-screw extruder is divided into a conveying section, a melting section, a plasticizing section and a discharge section which are arranged in sequence; the first direction is parallel to the extension direction of the screw assembly and is the direction from the feed port of the twin-screw extruder to the discharge port; Wherein, the conveying section, the melting section and the plasticizing section include a plurality of forward shear blocks; the melting section and the plasticizing section also include at least one reverse conveying block.

15. The method for preparing a polypropylene material according to claim 14, characterized in that: The staggered angle of the forward shear block ranges from 30° to 60°.

16. The method for preparing a polypropylene material according to claim 12, characterized in that: The method further comprises: preparing microcapsules; The method for preparing microcapsules comprises: Adding 0.5 to 1.5 parts by mass of urea to 1.5 to 2.5 parts by mass of a formaldehyde solution, and adding an alkaline catalyst to the formaldehyde solution to obtain a first mixed solution having a pH value of 7 to 8; Stirring the first mixed solution at a temperature of 60° C. to 70° C. for 1 h to 2 h to obtain a polyurea resin prepolymer; Mixing 9 to 11 parts by mass of styrene monomer, 2 to 4 parts by mass of a cross-linking agent, and 1 to 3 parts by mass of a second compatibilizer to obtain a second mixed solution, and adding an emulsifier to the second mixed solution so that the ratio of the mass of the emulsifier to the mass of the second mixed solution is 1 to 3 to obtain a third mixed solution; Stirring the third mixed solution at a temperature of 30° C. to 40° C. for 10 min to 30 min to obtain a first reaction solution; Adding the mechanochromic compound to the first reaction solution, and stirring the first reaction solution for 5 minutes to 15 minutes after the addition, to obtain a core material prepolymer; Mixing the core material prepolymer with the polyurea resin prepolymer to obtain a fourth mixed solution, and adjusting the pH of the fourth mixed solution to 3-4; Stirring the fourth mixed solution at a temperature of 60° C. to 70° C. for 2 h to 3 h to obtain a microcapsule suspension; The microcapsule suspension is filtered, purified and dried to obtain the microcapsules.

17. An automobile part, characterized in that: The automotive part comprises the polypropylene composition according to any one of claims 1 to 11; or The automobile part comprises the polypropylene material obtained by the preparation method according to any one of claims 12 to 16.

Citation Information

Cited By

  • High-strength creep-resistant long fiber reinforced polypropylene composite material for automobile and preparation method of high-strength creep-resistant long fiber reinforced polypropylene composite material

    CN119899456A