Single-layer diamond embedded metal-based super-lyophilic micro-nano structure composite board, manufacturing process, application and flat heat pipe
By using a single layer of diamond in the heat pipe to embed the metal-based superliquid micro-nano structure composite plate, the diamond particles and groove array are regulated, and the problem of insufficient thermal conductivity and phase-to-phase core density of traditional heat pipe materials is solved, achieving efficient Phase change heat transfer meets the heat dissipation needs of high-heat flow density electronic devices and promotes ultra-thin structural processing for industrial applications.
Patent Information
- Application Number
- CN202411189762.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional single-phase heat exchange methods are difficult to meet the heat dissipation needs of electronic devices with high heat flow density. Especially in the context of miniaturization and lightweighting of electronic devices, the thermal conductivity and phase-to-phase nuclear density of traditional heat pipe materials are insufficient, making it difficult to cope with the high future. Development of heat flow density systems.
A single-layer diamond embedded in metal-based super-liquid micro-nano structure composite plate is used to regulate the diamond particles and groove array structure to form a high-density phase-turning core and capillary transmission structure, and combine it with the surface micro-nano porous structure to enhance phase change heat transfer. efficiency.
It significantly improves thermal conductivity and phase change heat transfer efficiency, achieves efficient heat dissipation, meets the needs of high-heat flow density electronic devices, and promotes ultra-thin structure processing for industrial applications.
Smart Images

Figure CN118936172A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of heat transfer technology and relates to a heat transfer structure, in particular to a single-layer diamond embedded in a metal-based super-liquid-philic micro-nano structure composite plate and a manufacturing process, application and flat heat pipe. Background Art
[0002] With the rapid development of microelectronics technology, the performance and integration of electronic devices have reached unprecedented heights. However, this progress has also brought significant thermal management challenges. The heat flux density of electronic devices continues to rise, reaching an unprecedented level, making controlling the temperature of devices and ensuring their operation in an efficient and stable state a core issue that needs to be urgently addressed in the field of electronic thermal management. Especially in the context of the continuous miniaturization and lightweight development of electronic devices, the high degree of integration of electronic devices has put forward more stringent requirements on the installation space of the heat dissipation module. Effective heat dissipation of high heat flux density electronic devices in a limited space has become a key factor in determining the overall performance improvement of electronic equipment.
[0003] Traditional single-phase heat exchange methods, such as natural convection, forced convection, and heat conduction, are unable to meet the heat dissipation requirements of high heat flux electronic devices due to their limited heat transfer capacity. In this context, ultra-thin flat heat pipes, as an efficient phase change heat transfer element, have gradually emerged as a reliable alternative to traditional cooling methods in the field of electronic heat dissipation with their excellent thermal conductivity, stable operating state, and adaptive balance capabilities. Its working principle is the phase change cycle of the internal working fluid, which achieves efficient heat transfer through evaporation and condensation processes, thereby significantly improving heat dissipation efficiency.
[0004] The materials or structures used in heat pipes are mainly metal materials such as copper, aluminum, and titanium (Applied Thermal Engineering, 2022, 211: 118459). Their thermal conductivity still has room for improvement, and the internal liquid-absorbing core structure is mainly a single groove or a porous liquid-philic structure formed by sintering / etching (Applied Thermal Engineering, 2024, 256: 124079; International Communications in Heat and Mass Transfer, 2022, 137: 106162). The phase transition results in insufficient core density and capillary force, which poses great challenges to the development of future advanced systems with high heat flux density. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a single-layer diamond-embedded metal-based super-lyophilic micro-nanostructure composite plate and a manufacturing process, application and flat-plate heat pipe. The formed composite plate can achieve high-density phase change nucleation by regulating the diamond particles exposed on the metal base surface, control the growth of bubbles and droplets through grooves, and at the same time couple the grooves and the surface micro-nano porous structure to improve the capillary transmission level, thereby greatly enhancing phase change heat transfer.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A single-layer diamond embedded metal-based super-lyophilic micro-nano structure composite plate used in heat pipes, the composite plate includes a metal base, a single-layer diamond particle embedded in the metal base and a super-lyophilic micro-nano structure on the surface of the metal base; one end of the composite plate is a hot end, and the other end is a cold end; the super-lyophilic micro-nano structure at the hot end is an orthogonal groove array composed of a plurality of strip grooves arranged orthogonally or a parallel groove array composed of a plurality of strip grooves arranged in parallel; the super-lyophilic micro-nano structure at the cold end is a wedge-shaped groove array composed of a plurality of wedge-shaped strip grooves arranged in parallel; the narrow end of the wedge-shaped strip groove points to the cold end direction, and the wide end points to the hot end direction; the surfaces of the orthogonal groove array, the parallel groove array and the wedge groove array all have micro-nano structures. Micro-nano structures refer to micrometer and nanometer structures.
[0008] To optimize the above technical solutions, the specific measures taken also include:
[0009] Furthermore, in the wedge-shaped groove array, the wedge-shaped side profile of the wedge-shaped strip grooves is a fastest curve, and the wedge angle is 1 to 8 degrees.
[0010] Furthermore, in the orthogonal groove array, the parallel groove array and the wedge-shaped groove array, the width and depth of the grooves are both 100-1000 μm.
[0011] Furthermore, the volume fraction of the diamond particles in the composite plate is 10-60%; the surface of the diamond particles is smooth, the particle size is 100-1000 μm, and they are discretely distributed inside the grooves and on the groove ridges, and the volume of each diamond particle exposed from the metal base accounts for 5-50%.
[0012] Furthermore, the metal base is copper or nickel; the thickness of the metal base is 0.1 to 2.0 mm.
[0013] Furthermore, the micro-nano structure is a papillary and / or porous micro-nano structure.
[0014] The present invention also provides a manufacturing process for the above-mentioned single-layer diamond embedded in a metal-based super-lyophilic micro-nano structure composite plate, comprising the following steps: step 1, laying a single layer of diamond particles in a mask plate; step 2, depositing metal between the diamond particles by mask electrodeposition, so that the diamond particles are embedded in the metal base; step 3, using a nanosecond / picosecond / femtosecond laser to process an orthogonal groove array or a parallel groove array and a wedge-shaped groove array on the metal base embedded with the diamond particles, and simultaneously forming a micro-nano porous structure.
[0015] The present invention also provides application of the above-mentioned single-layer diamond embedded in metal-based super-liquid-philic micro-nano structure composite plate in heat transfer.
[0016] The present invention also provides a flat heat pipe, which is formed by embedding two pieces of the above-mentioned single-layer diamond into a metal-based super-liquid-philic micro-nano structure composite plate and packaging them face to face to form a hollow cavity (the edge of the composite plate has a raised side to form a hollow cavity when packaged face to face), and then filling the cavity with a heat transfer medium through a capillary; the heat transfer medium is deionized water, ethanol or acetone, and the filling rate is 5 to 60%.
[0017] The present invention also provides application of the flat plate heat pipe in heat transfer.
[0018] The beneficial effects of the present invention are:
[0019] 1. The present invention embeds a single layer of diamond particles into a metal matrix, which is not only conducive to obtaining an ultra-thin material structure, but also can greatly reduce the heat transfer resistance in the thickness direction and increase its thermal conductivity.
[0020] Second, diamond particles are hydrophobic, and the energy barrier of phase transformation to nucleation is low, making it easy to nucleate. The present invention proposes that a single layer of diamond particles is embedded in a metal-based super-lyophilic micro-nanostructure, which can achieve high-density phase transformation to nucleation by controlling the exposed diamond particles on the surface, that is, providing boiling and condensation nucleation sites, thereby improving the phase transformation efficiency.
[0021] 3. The orthogonal groove array, parallel groove array and wedge-shaped groove array proposed in the present invention can constrain the lateral growth of bubbles / droplets and accelerate their detachment, thereby improving the phase change heat transfer limit.
[0022] 4. The coupling grooves and surface micro-nano structures of the present invention can greatly improve the super-lyophilicity of the structural surface, enhance the capillary transmission level, and achieve long-term and efficient phase change heat transfer.
[0023] 5. The present invention proposes to construct a single-layer diamond embedded in a metal structure by masked electrodeposition, and utilizes laser processing of a micro-nano porous groove array, which can realize large-area ultra-thin structure processing, and is of great significance for promoting industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1is a stereoscopic diagram of a single-layer diamond embedded in a metal-based super-lyophilic micro-nanostructure composite plate according to Example 1;
[0025] Figure 2 is a top view of a single-layer diamond embedded in a metal-based super-lyophilic micro-nanostructure composite plate according to Example 1;
[0026] Figure 3 is a cross-sectional view of a single-layer diamond embedded in a metal-based super-lyophilic micro-nanostructure composite plate of Example 1;
[0027] Figure 4 This is an electron photo of the droplet transfer process of the wedge-shaped groove array at the cold end of the super-lyophilic micro-nanostructure heat transfer plate without embedded diamond particles;
[0028] Figure 5 This is a SEM image of a single-layer diamond embedded in a metal-based super-lyophilic micro-nanostructure composite plate according to Example 2. DETAILED DESCRIPTION
[0029] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0030] Example 1
[0031] like Figures 1 to 3 As shown, this embodiment provides a single-layer diamond embedded in a metal-based super-lyophilic micro-nano structure composite plate for use in a heat pipe, comprising a metal base 1, a single-layer diamond particle 2 embedded in the metal base, and a super-lyophilic micro-nano structure on the surface of the metal base.
[0032] The metal base 1 is copper and has a thickness of 1.1 mm.
[0033] One end of the composite plate is the hot end, and the other end is the cold end. The super-lyophilic micro-nanostructure of the hot end is an orthogonal groove array 31 composed of a plurality of strip grooves arranged orthogonally. The width of the groove is 100 μm, the depth is 200 μm, and the cross-sectional profile is U-shaped. The super-lyophilic micro-nanostructure of the cold end is a wedge-shaped groove array 32 composed of a plurality of wedge-shaped strip grooves arranged in parallel. The narrow end of the wedge-shaped strip groove points to the cold end direction, and the wide end points to the hot end direction. The length of the groove is 50 mm, the depth is 100 μm, the wedge angle is 4°, and the wedge side profile is the fastest curve. The surfaces of the orthogonal groove array 31 and the wedge-shaped groove array 32 both have papillae and porous micro-nanostructures formed by laser ablation.
[0034] The volume fraction of the diamond particles 2 embedded in the metal matrix 1 is 30%, and they are discretely distributed inside the grooves and at the groove ridges. The surface of the diamond particles 2 is smooth, the particle size is 600 μm, and the volume of each diamond particle 2 exposed in the metal matrix accounts for 5-50%.
[0035] The method for preparing a single-layer diamond-embedded metal-based super-lyophilic micro-nanostructure composite plate comprises the following steps:
[0036] Step 1: Laying a single layer of diamond particles in a mask plate;
[0037] Step 2: depositing metal between diamond particles by masked electrodeposition, so that the diamond particles are embedded in the metal matrix;
[0038] Step 3: Use ultraviolet nanosecond laser to process orthogonal groove arrays and wedge-shaped groove arrays on the metal substrate embedded with diamond particles, and simultaneously form papillae and porous micro-nano structures on the groove surface.
[0039] The thermal diffusion coefficient of the single-layer diamond embedded in the metal-based super-lyophilic micro-nanostructure composite plate was measured by laser flash method (LFA 467, Netzsch, Germany), and the thermal conductivity of the material was obtained by combining the material density and specific heat capacity to obtain a high value of 884.9 W / m·K.
[0040] This embodiment also provides a flat heat pipe, which is formed by embedding two single-layer diamonds into a metal-based super-liquid-philic micro-nano structure composite plate face to face to form a hollow cavity, and then filling the cavity with a heat transfer medium through a capillary tube. The heat transfer medium is deionized water, and the filling rate is 10%.
[0041] In addition, the cold end wedge groove array of the heat transfer plate without embedded diamond particles (otherwise the same as in this embodiment) transfers the droplet process as shown in FIG. Figure 4 As shown, it can be seen that the wedge-shaped strip grooves can accelerate the transmission and separation of phase change products (such as droplet condensate), thereby improving the phase change heat transfer limit.
[0042] Example 2
[0043] The present embodiment provides a single-layer diamond-embedded metal-based super-lyophilic micro-nano structure composite plate for use in a heat pipe, comprising a metal base, a single-layer diamond particle embedded in the metal base, and a super-lyophilic micro-nano structure on the surface of the metal base.
[0044] The metal base is copper with a thickness of 1.0 mm.
[0045] One end of the composite plate is the hot end, and the other end is the cold end. The super-lyophilic micro-nanostructure of the hot end is a parallel groove array composed of several strip grooves arranged in parallel. The width of the groove is 100μm and the depth is 150μm. The super-lyophilic micro-nanostructure of the cold end is a wedge-shaped groove array composed of several wedge-shaped strip grooves arranged in parallel. The narrow end of the wedge-shaped strip groove points to the cold end direction, and the wide end points to the hot end direction. The length of the groove is 100mm, the depth is 150μm, the wedge angle is 4°, and the wedge side profile is the fastest curve. The surfaces of the parallel groove array and the wedge groove array both have porous micro-nanostructures formed by laser ablation.
[0046] The volume fraction of diamond particles embedded in the metal matrix is 50%, which are discretely distributed inside the groove and at the groove ridge. The surface of the diamond particles is smooth, the particle size is 400 μm, and the volume of each diamond particle exposed in the metal matrix accounts for 5 to 50%.
[0047] The method for preparing a single-layer diamond-embedded metal-based super-lyophilic micro-nanostructure composite plate comprises the following steps:
[0048] Step 1: Laying a single layer of diamond particles in a mask plate;
[0049] Step 2: depositing metal between diamond particles by masked electrodeposition, so that the diamond particles are embedded in the metal matrix;
[0050] Step 3: Use ultraviolet nanosecond laser to process parallel groove arrays and wedge-shaped groove arrays on the metal substrate embedded with diamond particles, and simultaneously form a porous micro-nano structure on the groove surface, such as Figure 5 shown.
[0051] This embodiment also provides a flat heat pipe, which is formed by embedding two single-layer diamonds into a metal-based super-liquid-philic micro-nano structure composite plate face to face to form a hollow cavity, and then filling the cavity with a heat transfer medium through a capillary tube. The heat transfer medium is ethanol, and the filling rate is 10%.
[0052] In the present invention, unless otherwise specified, the scientific and technical terms used herein have the meanings commonly understood by those skilled in the art. In addition, the reagents, materials and operating procedures used herein are reagents, materials and conventional procedures widely used in the corresponding fields.
[0053] It should be noted that the terms such as "upper", "lower", "left", "right", "front", "back", etc. cited in the invention are only for the convenience of description and are not used to limit the scope of implementation of the present invention. Changes or adjustments in their relative relationships should be regarded as the scope of implementation of the present invention without substantially changing the technical content.
[0054] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A single-layer diamond-embedded metal-based super-lyophilic micro-nanostructure composite plate for heat pipes, characterized by: The composite plate includes a metal substrate, a single layer of diamond particles embedded in the metal substrate, and a super-lyophilic micro-nano structure on the surface of the metal substrate; One end of the composite plate is the hot end, and the other end is the cold end; The super-lyophilic micro-nanostructure at the hot end is an orthogonal groove array composed of a plurality of strip grooves arranged orthogonally or a parallel groove array composed of a plurality of strip grooves arranged in parallel; The super-lyophilic micro-nanostructure at the cold end is a wedge-shaped groove array composed of a number of wedge-shaped strip grooves arranged in parallel; The narrow end of the wedge-shaped groove points to the cold end, and the wide end points to the hot end; The surfaces of the orthogonal groove array, the parallel groove array and the wedge-shaped groove array all have micro-nano structures.
2. The single-layer diamond-embedded metal-based super-lyophilic micro-nano structure composite plate for heat pipe according to claim 1, characterized in that: In the wedge-shaped groove array, the wedge-shaped side profile of the wedge-shaped strip groove is a fastest curve, and the wedge angle is 1 to 8 degrees.
3. The single-layer diamond-embedded metal-based super-lyophilic micro-nano structure composite plate for heat pipe according to claim 1, characterized in that: In the orthogonal groove array, the parallel groove array and the wedge-shaped groove array, the width and depth of the grooves are both 100-1000 μm.
4. The single-layer diamond-embedded metal-based super-lyophilic micro-nano structure composite plate for heat pipe according to claim 1, characterized in that: The volume fraction of the diamond particles in the composite plate is 10 to 60%; The surface of the diamond particles is smooth, the particle size is 100 to 1000 μm, and the volume of each diamond particle exposed from the metal base accounts for 5 to 50%.
5. The single-layer diamond-embedded metal-based super-lyophilic micro-nano structure composite plate for heat pipe according to claim 1, characterized in that: The metal base is copper or nickel; The thickness of the metal base is 0.1 to 2.0 mm.
6. The single-layer diamond-embedded metal-based super-lyophilic micro-nano structure composite plate for heat pipe according to claim 1, characterized in that: The micro-nano structure is a papillary and / or porous micro-nano structure.
7. The manufacturing process of the single-layer diamond embedded metal-based super-lyophilic micro-nano structure composite plate according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: Laying a single layer of diamond particles in a mask plate; Step 2: depositing metal between diamond particles by masked electrodeposition, so that the diamond particles are embedded in the metal matrix; Step 3: Use nanosecond / picosecond / femtosecond laser to process orthogonal groove arrays or parallel groove arrays and wedge-shaped groove arrays on the metal substrate embedded with diamond particles, and simultaneously form a micro-nano porous structure.
8. Application of the single-layer diamond embedded metal-based super-lyophilic micro-nano structure composite plate as claimed in any one of claims 1 to 6 in heat transfer.
9. A flat plate heat pipe, characterized in that: The hollow cavity is formed by embedding two single-layer diamonds as claimed in any one of claims 1 to 6 into a metal-based super-lyophilic micro-nanostructure composite plate and encapsulating them face to face, and then filling the cavity with a heat transfer medium through a capillary; The heat transfer medium is deionized water, ethanol or acetone, and the liquid filling rate is 5-60%.
10. Use of the flat plate heat pipe according to claim 9 in heat transfer.