Method for testing curing internal stress of adhesive by pre-buried strain gauge method

Through the embedded strain gauge method, the stress changes in the adhesive curing process are monitored in real time, and the problems of complex operation and low accuracy in the existing technology are solved. It provides a high-precision internal stress testing method for adhesive curing, which is suitable for various Application of adhesives.

CN118936698APending Publication Date: 2024-11-12HARBIN INST OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411263048.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing methods for testing the internal stress of adhesive curing are complex in operation, low test accuracy and unavailable in real-time monitoring, which limits the optimization and application range of bonding performance.

Method used

By using the embedded strain gauge method, by fixing the resistance strain gauge on the surface of the substrate and connecting it with the signal acquisition device, the strain data during the adhesive curing process is recorded in real time, and the stress changes with time curve is generated, and the multi-channel strain gauge is measured. Shrinkage stress of adhesive.

Benefits of technology

Real-time monitoring and dynamic data acquisition of the adhesive curing process are realized, easy to operate, can measure the curing stress of various adhesives with high precision, make up for the shortcomings of the existing methods, and have high research and application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118936698A_ABST
    Figure CN118936698A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of material testing, and particularly relates to a method for testing curing internal stress of an adhesive through a strain gauge pre-embedding method, in particular to the method for testing the curing internal stress of the adhesive through the strain gauge pre-embedding method. The problems that an existing method for testing the curing internal stress of the adhesive is complex in operation, low in testing precision and incapable of achieving real-time monitoring are solved. The method comprises the following steps: pre-burying the resistance strain gauge in the adhesive coating, enabling the resistance strain gauge and the cured adhesive to shrink together, reading the numerical value of the strain gauge by using a multi-channel strain gauge, and measuring the shrinkage stress of the adhesive in curing. The device is used for testing the curing internal stress of the adhesive; the method is simple to operate, can overcome the problems of complicated operation, low test precision, incapability of real-time monitoring and the like in the existing method, and can monitor the curing internal stress change of the adhesive in real time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material testing, and in particular relates to a method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method. Background Art

[0002] Adhesive bonding is widely used in the connection of mechanical structures. It can simplify the mechanical structure and thus reduce the overall weight, achieving lightweight design and assembly. However, compared with metal or inorganic non-metallic materials, adhesives have poor physical and chemical stability. The internal bonding stress generated during the curing process will have a great impact on the bonding performance, limiting the application range of adhesives.

[0003] The volume of the adhesive layer shrinks due to the reduction of the effective components of the bonding surface caused by the volatilization of the solvent, or due to the escape of small molecular products in the polycondensation reaction, the shortening of the atomic distance in the polyaddition reaction, etc., which will cause shrinkage of the adhesive layer and generate shrinkage internal stress, affecting the service life of the component. In addition, due to the large difference in the thermal expansion coefficients of the adhesive and the adherend, when the temperature changes, the thermal expansion of the adhesive layer is constrained by the rigid metal, and compressive thermal stress will be generated inside the adhesive layer, causing a small relative displacement between the components, thereby reducing the strength of the joint, and sometimes even causing the joint to rupture by itself, which has a great impact on the bonding performance and limits the application of bonding in some important occasions.

[0004] In order to ensure the accuracy of the instrument and the safety of the equipment, it is necessary to test the curing internal stress generated by the adhesive during the curing process and reduce its harmful effects to the minimum. At present, there are many methods for detecting the curing stress of adhesives, but there are generally problems such as complex operation, low test accuracy, and inability to monitor in real time. Therefore, there is an urgent need for a simple, accurate method and device that can monitor the curing stress of adhesives in real time. Summary of the invention

[0005] The present invention aims to solve the problems of complicated operation, low test accuracy and inability to monitor in real time in existing methods for testing the internal stress of adhesive curing, and to provide a method for testing the internal stress of adhesive curing by using a pre-embedded strain gauge method.

[0006] A method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge is accomplished by the following steps:

[0007] 1. Select the embedded strain gauge whose measurement range and accuracy meet the test requirements;

[0008] 2. Pre-treat the surface of the substrate to be tested, and fix several pre-embedded strain gauges on the surface of the substrate, ensuring that the sensing part of the pre-embedded strain gauges is exposed in the area to be bonded and in close contact with the substrate;

[0009] 3. Connect the embedded strain gauge to the bridge circuit, and paste the same strain gauge outside the adhesive as temperature compensation and connect it to the bridge circuit;

[0010] 4. Evenly apply the test adhesive on the surface of the substrate to cover the embedded strain gauge and its surrounding area, ensuring that the adhesive completely covers the sensing part of the strain gauge. Connect the embedded strain gauge to the signal acquisition device, continuously record the strain data during the curing process through the data acquisition system, and generate a stress-time curve through the data processing system to obtain the shrinkage stress of the adhesive during curing.

[0011] Beneficial effects of the present invention:

[0012] The present invention provides a method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method. The method includes pre-embedding a resistance strain gauge in an adhesive coating so that the resistance strain gauge shrinks together with the curing adhesive, and using a multi-channel strain gauge to read the strain gauge value to measure the shrinkage stress of the adhesive during curing. This testing method can monitor the stress changes during the curing process of the adhesive in real time and provide dynamic data support. It is simple to operate and easy to implement. It is suitable for curing stress testing of various adhesives and can make up for the shortcomings of existing testing methods. The present invention provides a new idea for testing the curing internal stress of adhesives and has a high research and application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a schematic diagram of the method of testing the internal stress of adhesive curing by the embedded strain gauge method. DETAILED DESCRIPTION

[0014] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0015] Specific implementation method 1: In this implementation method, a method for testing the internal stress of adhesive curing by a pre-embedded strain gauge method is completed according to the following steps:

[0016] 1. Select the embedded strain gauge whose measurement range and accuracy meet the test requirements;

[0017] 2. Pre-treat the surface of the substrate to be tested, and fix several pre-embedded strain gauges on the surface of the substrate, ensuring that the sensing part of the pre-embedded strain gauges is exposed in the area to be bonded and in close contact with the substrate;

[0018] 3. Connect the embedded strain gauge to the bridge circuit, and paste the same strain gauge outside the adhesive as temperature compensation and connect it to the bridge circuit;

[0019] 4. Evenly apply the test adhesive on the surface of the substrate to cover the embedded strain gauge and its surrounding area, ensuring that the adhesive completely covers the sensing part of the strain gauge. Connect the embedded strain gauge to the signal acquisition device, continuously record the strain data during the curing process through the data acquisition system, and generate a stress-time curve through the data processing system to obtain the shrinkage stress of the adhesive during curing.

[0020] In this embodiment, the close contact with the substrate can avoid distortion of the strain signal.

[0021] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: the embedded strain gauge in step 1 is a resistance element made of conductive material, and its resistance value changes under stress; the embedded strain gauge is electrically connected to the signal acquisition device to transmit the strain signal in real time. The rest is the same as specific implementation method 1.

[0022] Specific implementation method 3: This implementation method is different from the specific implementation method 1 in that the substrate to be tested in step 2 is quartz glass or 2024Al alloy. The rest is the same as the specific implementation method 1.

[0023] Specific implementation method 4: This implementation method is different from specific implementation method 1 in that the pretreatment in step 2 is to clean the surface of the substrate to be tested; first use 400# sandpaper to polish until there are no obvious scratches, and then wipe the polished surface with alcohol. Others are the same as specific implementation method 1.

[0024] Specific implementation method 5: This implementation method is different from specific implementation method 1 in that the fixing in step 2 is performed preliminarily by using a special fixing glue or other fixing device. The rest is the same as specific implementation method 1.

[0025] Specific implementation example 6: This implementation example is different from specific implementation example 1 in that: in step 4, before the test adhesive is coated, the bubbles in the test adhesive are emptied by centrifugation or vacuuming. The rest is the same as specific implementation example 1.

[0026] Specific implementation method 7: This implementation method is different from specific implementation method 1 in that: in step 4, the coating thickness of the tested adhesive is controlled at 0.2-0.3 mm; a wire of corresponding size is used to control the coating thickness. The rest is the same as specific implementation method 1.

[0027] This embodiment ensures the accuracy of the test result by controlling the thickness and uniformity of the adhesive.

[0028] Specific implementation eight: This implementation differs from specific implementation one in that: the signal acquisition device in step four is a multi-channel strain gauge, which includes a Wheatstone bridge circuit for converting the resistance change of the embedded strain gauge into a voltage signal; the data acquisition system is used to collect voltage signals in real time and store or transmit them to a data processing system; the data processing system is used to analyze the internal stress generated by the adhesive during the curing process. Others are the same as specific implementation one.

[0029] Specific embodiment 9: This embodiment differs from specific embodiment 1 in that the data processing system in step 4 combines the recorded strain data with the elastic modulus of the adhesive, calculates the internal stress generated during the curing process of the adhesive through Hooke's law, and analyzes the law of stress change over time. The rest is the same as specific embodiment 1.

[0030] In this embodiment, the resistance change of the strain gauge is converted into the output voltage change of the bridge. The output voltage is proportional to the strain. The output voltage of the bridge is amplified by the amplifier circuit and indicated or recorded by an indicating instrument or a recording instrument, or processed and analyzed by a data acquisition system to obtain the value or curve of the strain.

[0031] Specific embodiment 10: This embodiment differs from specific embodiment 9 in that the calculation formula of the internal stress generated during the curing process of the adhesive is as follows:

[0032] σ i =E(ε0-ε i )

[0033] Where: i is the curing internal stress measured at the location of the i-th strain gauge, E is the tensile elastic modulus of the adhesive layer, and ε0 is the curing shrinkage strain measured by the temperature compensation sheet embedded in the outside of the adhesive layer (ε0>ε i ), ε i is the curing shrinkage strain of the adhesive layer at the position of the i-th strain gauge. The rest is the same as the ninth embodiment.

[0034] The following examples are used to verify the beneficial effects of the present invention:

[0035] A method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge is accomplished by the following steps:

[0036] 1. Select the embedded strain gauge whose measurement range and accuracy meet the test requirements;

[0037] 2. Pre-treat the surface of the substrate to be tested to ensure that it is clean and flat, fix five strain gauges at different positions of the quartz glass substrate, and connect them to a multi-channel strain gauge to read the strain gauge value, ensuring that the sensing part of the embedded strain gauge is exposed in the area to be bonded and in close contact with the substrate; the substrate to be tested is quartz glass;

[0038] 3. Connect the embedded strain gauge to the bridge circuit, and paste the same strain gauge outside the adhesive as temperature compensation and connect it to the bridge circuit;

[0039] 4. Apply the test adhesive evenly on the surface of the substrate to cover the embedded strain gauge and its surrounding area, ensure that the adhesive completely covers the sensing part of the strain gauge, connect the embedded strain gauge to the signal acquisition device, regularly collect the stress value of the strain gauge at this location, and continuously record the strain data during the curing process through the data acquisition system to obtain the curve of shrinkage stress at different positions versus curing time. After the adhesive is cured, the difference in stress values ​​at different positions is the final residual stress. The strain gauge and adhesive are heated on a platform to maintain the temperature at 60°C during the test, and the same strain gauge is placed outside the adhesive for temperature compensation to reduce the impact of temperature on the strain gauge. As shown in the attached figure, the position coordinates D of the strain gauge are 0mm, 20mm, 35mm, 50mm, and 70mm respectively.

[0040] During the 200-minute test, the test results at the five locations all showed a trend of gradually increasing shrinkage stress. The increase in shrinkage stress is due to the evaporation of the solvent and the reduction of effective ingredients at the bonding surface. According to the test results, D = 35mm has the smallest shrinkage stress, and D = 0mm and D = 70mm have the largest shrinkage stress. The shrinkage stress at the edge of the adhesive layer is greater, and the shrinkage stress at the center is the smallest.

Claims

1. A method for testing the internal stress of adhesive curing by using a pre-embedded strain gauge, characterized in that The method of testing the internal stress of adhesive curing by the embedded strain gauge method is completed in the following steps:

1. Select the embedded strain gauge whose measurement range and accuracy meet the test requirements; 2. Pre-treat the surface of the substrate to be tested, and fix several pre-embedded strain gauges on the surface of the substrate, ensuring that the sensing part of the pre-embedded strain gauges is exposed in the area to be bonded and in close contact with the substrate; 3. Connect the embedded strain gauge to the bridge circuit, and paste the same strain gauge outside the adhesive as temperature compensation and connect it to the bridge circuit; 4. Evenly apply the test adhesive on the surface of the substrate to cover the embedded strain gauge and its surrounding area, ensuring that the adhesive completely covers the sensing part of the strain gauge. Connect the embedded strain gauge to the signal acquisition device, continuously record the strain data during the curing process through the data acquisition system, and generate a stress-time curve through the data processing system to obtain the shrinkage stress of the adhesive during curing.

2. The method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method according to claim 1, characterized in that The embedded strain gauge in step 1 is a resistance element made of conductive material, and its resistance value changes under the action of stress; The embedded strain gauge is electrically connected to the signal acquisition device to transmit the strain signal in real time.

3. The method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method according to claim 1, characterized in that The substrate to be tested in step 2 is quartz glass or 2024Al alloy.

4. The method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method according to claim 1, characterized in that The pretreatment described in step 2 is to clean the surface of the substrate to be tested; first use 400# sandpaper to polish until there are no obvious scratches, and then wipe the polished surface with alcohol.

5. The method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method according to claim 1, characterized in that The fixing described in step 2 is performed preliminarily by using a special fixing glue or other fixing devices.

6. The method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method according to claim 1, characterized in that In step 4, before coating the test adhesive, the bubbles in the test adhesive are emptied by centrifugation or vacuum operation.

7. The method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method according to claim 1, characterized in that In step 4, the adhesive coating thickness is tested to be controlled at 0.2 to 0.3 mm; a wire of corresponding size is used to control the coating thickness.

8. The method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method according to claim 1, characterized in that The signal acquisition device described in step 4 is a multi-channel strain gauge, which includes a Wheatstone bridge circuit for converting the resistance change of the embedded strain gauge into a voltage signal; the data acquisition system is used to collect the voltage signal in real time and store or transmit it to the data processing system; the data processing system is used to analyze the internal stress generated by the adhesive during the curing process.

9. The method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method according to claim 1, characterized in that In step 4, the data processing system combines the recorded strain data with the elastic modulus of the adhesive, calculates the internal stress generated during the curing process of the adhesive through Hooke's law, and analyzes the law of stress change over time.

10. The method for testing the curing internal stress of an adhesive by using a pre-embedded strain gauge method according to claim 9, characterized in that The calculation formula for the internal stress generated during the curing process of the adhesive is as follows: s i =E(ε0-ε i ) Where: i is the curing internal stress measured at the location of the i-th strain gauge, E is the tensile elastic modulus of the adhesive layer, and ε0 is the curing shrinkage strain measured by the temperature compensation sheet embedded in the outside of the adhesive layer (ε0>ε i ), ε i is the curing shrinkage strain of the adhesive layer at the location of the i-th strain gauge.

Citation Information

Cited By

  • Pressure monitoring method and device, storage medium and computer program

    CN121298085A

  • Pressure sensing device and pressure value determination method

    CN121347272A