Indoor accelerated erosion test method for simulating western saline soil environment
By conducting indoor accelerated erosion tests simulating the saline soil environment of western China, and combining the accelerated deterioration coefficient with the influence of multiple factors, the problem of large differences between existing test methods and actual environments was solved, enabling the study of concrete performance deterioration laws and durability assessment.
Patent Information
- Application Number
- CN202411071498.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing indoor accelerated erosion tests have failed to effectively simulate the effects of multiple factors interacting on concrete in the western saline soil environment, resulting in significant differences between the test results and the actual environment, making it difficult to accurately assess the erosion resistance of concrete.
By investigating the environmental characteristics of saline soil in western China, the accelerated degradation coefficient was calculated. Combined with the acceleration coefficients of ion concentration, wet-dry cycle, and freeze-thaw cycle, the erosion duration of each stage of high temperature, low temperature, wet-dry cycle, and freeze-thaw cycle was determined. Corresponding accelerated test methods were used to simulate the saline soil environment in western China.
This method enables a more realistic simulation of the western saline soil environment under laboratory conditions, shortens the test time, provides a method for evaluating the durability of concrete in complex environments, and provides a theoretical basis for the design of concrete structures in the western saline soil environment.
Smart Images

Figure CN118937198A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete anti-erosion performance evaluation, and in particular to an indoor accelerated erosion test method for simulating a western saline soil environment. Background Art
[0002] With the increasing efforts in infrastructure construction in Qinghai, Tibet, Xinjiang, Ningxia, Gansu and Inner Mongolia, the construction scale and level of a large number of key highway, railway, bridge and tunnel projects have also been significantly improved. However, there are a large number of saline soil environments containing corrosive media such as high concentrations of sulfate ions and chloride ions in western my country. The corrosive ions in the soil will pose a serious threat to the service life of concrete structures. At the same time, due to the special geographical location of the western region, the region presents climatic characteristics such as large temperature difference between day and night, low rainfall and high evaporation. Under the interaction of high temperature, low temperature, dry-wet cycle, freeze-thaw cycle and high concentration of corrosive salt solution, the durability of concrete structures will be greatly reduced.
[0003] Considering that the normal temperature and freeze-thaw cycles in the western region last for a long time, and the corrosion of concrete itself by sulfate and chloride salts is a long-term performance degradation process, it is of great significance to develop an indoor accelerated corrosion scheme that conforms to the western saline soil environment and carry out indoor accelerated tests on the corrosion resistance of concrete under this scheme for the durability of concrete in complex corrosion environments. In order to shorten the test time, a reasonable acceleration method can be used to conduct indoor corrosion tests, select the corresponding acceleration coefficient and duration for different corrosion stages, and ensure that the concentration of the corrosion solution in each stage remains consistent.
[0004] At present, the existing indoor accelerated corrosion tests mainly consider the study of the anti-corrosion performance of concrete under the action of a single factor (such as high temperature, low temperature, dry-wet cycle and freeze-thaw cycle, etc.), and are limited to the general atmospheric environment. The anti-corrosion performance of concrete under the combined action of multiple environments has not been studied; in addition, the setting of indoor accelerated corrosion test parameters is only selected according to the parameters specified in the specification, and is not combined with the actual corrosion environment characteristics, resulting in the low rationality of using conventional test methods for corrosion tests. An corrosion scheme that is closer to the actual environment should be used to test the anti-corrosion performance of concrete.
[0005] Therefore, it is necessary to propose an indoor accelerated erosion scheme and test method simulating the western saline soil environment to study the anti-erosion performance of concrete under the interaction of high temperature, low temperature, dry-wet cycle, freeze-thaw cycle and high concentration of corrosive salts in the western saline soil environment, to determine the simulation parameters of the indoor accelerated erosion test and to study the degradation law of concrete performance, so as to solve the problems existing in the existing research. Summary of the invention
[0006] In order to solve the deficiencies in the above-mentioned prior art, the present invention aims to provide an indoor accelerated erosion test method simulating the western saline soil environment. Based on the actual climatic characteristics and saline soil characteristics of the western saline soil environment, and considering the similarity between the concrete anti-salt erosion effect in the actual western saline soil environment and the laboratory simulation environment, the accelerated degradation coefficient and the duration of the erosion stage are determined. This test method can effectively avoid the problem that traditional indoor accelerated tests do not consider the actual erosion conditions, realize the study of the degradation law of concrete performance under the interaction of multiple factors, and provide a theoretical design basis and technical support for the application of concrete structures in the western saline soil environment.
[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0008] An indoor accelerated erosion test method simulating the western saline soil environment, the steps are as follows:
[0009] S1: Determine the indoor accelerated erosion simulation scheme for western saline soil environment;
[0010] S2: Erosion test on concrete specimens based on indoor accelerated erosion simulation scheme;
[0011] S3: Conduct macroscopic performance tests on the concrete specimens after the erosion test to obtain erosion results under simulated conditions.
[0012] As a further preferred embodiment of the above technical solution: in step S1, the determination of the indoor accelerated erosion simulation scheme includes the following steps:
[0013] S11: Investigate the environmental characteristics of saline soil in western China;
[0014] S12: Calculating an accelerated degradation coefficient based on the obtained environmental characteristic information;
[0015] S13: Determine the duration of each corrosion stage according to the accelerated degradation coefficient.
[0016] Preferably, in step S11, the environmental characteristic information of the western saline soil includes calculation of the annual average high temperature, annual average low temperature, annual number of freeze-thaw cycles, average normal temperature duration, and statistics of the type and concentration of saline soil erosion solutions.
[0017] Preferably, the annual average high temperature and annual average low temperature duration refer to the product of the number of days with a temperature above 35°C and below -20°C, respectively, and the duration of the maximum daily temperature in summer and autumn and the minimum daily temperature in winter and spring in the western region; the annual number of freeze-thaw cycles refers to the number of times the minimum temperature of a day is lower than 0°C and the maximum temperature of the day is higher than 0°C, and under this condition, it is considered that the concrete is subjected to one freeze-thaw cycle in a day; the annual average normal temperature duration refers to the number of days in a year after removing the annual average high temperature duration, the annual average low temperature duration and the annual number of freeze-thaw cycles; the statistics of the types and concentrations of saline soil erosion solutions are mainly based on geological survey data in the western region to determine the concentration ranges of sulfate ions and chloride ions.
[0018] As a further preferred solution: in step S12, the calculation of the accelerated degradation coefficient includes the calculation of the ion concentration acceleration coefficient, the dry-wet cycle acceleration coefficient and the equivalent freeze-thaw cycle acceleration coefficient. Preferably, the high temperature and low temperature stages are accelerated by increasing the concentration of the salt solution. The freeze-thaw cycle stage is accelerated by increasing the concentration of the salt solution and converting the indoor and outdoor equivalent freeze-thaw damage ratio. The normal temperature stage is accelerated by increasing the concentration of the salt solution and alternating dry-wet cycles, wherein:
[0019] The ion concentration acceleration factor is calculated according to the ion concentration similarity theory, and the ion concentration acceleration factor F under the influence of the corrosion solution concentration is obtained. d ;
[0020]
[0021] In the formula, C s fie With C s lab are the surface ion concentrations of concrete in actual environment and indoor test, respectively;
[0022] The calculation of the dry-wet cycle acceleration factor is based on the average temperature of the laboratory and the average temperature during the dry-wet cycle. The calculation formula is as follows:
[0023]
[0024] Where, T d is the dry-wet cycle acceleration factor, T 1 is the average laboratory temperature, T 2 is the average temperature during the dry-wet cycle, E / R is the activation energy, and K is the temperature unit Kelvin;
[0025] The equivalent freeze-thaw cycle acceleration factor refers to the number of corresponding indoor rapid freeze-thaw cycles that the concrete must undergo when the degree of damage to the concrete is consistent with that after several on-site freeze-thaw cycles.
[0026] Furthermore, the calculation of the dry-wet cycle acceleration factor first requires determining the drying temperature, drying time, cooling time, soaking time, dry-wet ratio and cycle period, and then according to the laboratory average temperature T 1 Calculate the average temperature T during the dry-wet cycle 2 Finally, the dry-wet cycle acceleration factor T is obtained d ; Among them, the average temperature T during the dry-wet cycle is calculated by drying temperature, drying time, cooling time, soaking time, dry-wet ratio and cycle period 2 The formula is as follows:
[0027]
[0028] Where M 1 is the drying time, N 1 is the drying temperature, M 2 is the soaking time, M 3 is the cooling time, and M is the duration of a dry-wet cycle.
[0029] The equivalent freeze-thaw cycle acceleration factor refers to the number of corresponding indoor rapid freeze-thaw cycles that the concrete must undergo when the degree of damage to the concrete after several on-site freeze-thaw cycles is consistent. It is mainly determined based on the rapid freeze-thaw test method formulated in the domestic concrete test regulations. The coefficient N d .
[0030] Preferably, in step S13, the determination of the duration of each erosion stage includes the determination of the duration of the high temperature and low temperature erosion stages, the duration of the freeze-thaw cycle erosion stage, and the duration of the normal temperature erosion stage, wherein:
[0031] The duration of high-temperature and low-temperature erosion stages is determined based on the calculation results of the ion concentration acceleration coefficient;
[0032] The duration of the freeze-thaw cycle erosion phase is determined based on the calculation results of the equivalent freeze-thaw cycle acceleration coefficient, and the time and number of rapid freeze-thaw cycles are set;
[0033] The duration of the normal temperature erosion stage is determined based on the calculation results of the dry-wet cycle acceleration coefficient.
[0034] As a further preferred embodiment of the above technical solution: in step S2, the corrosion test of the concrete specimen based on the indoor accelerated corrosion simulation scheme includes four stages: high temperature corrosion, dry-wet cycle corrosion, freeze-thaw cycle corrosion and low temperature corrosion. The specific steps are as follows:
[0035] S21: Put the concrete specimen into a high-temperature curing box and soak it with a salt solution. During the soaking, the solution is higher than the concrete specimen. At the same time, it is sealed with a plastic wrap. The temperature of the salt solution in the high-temperature curing box is maintained at a constant temperature to simulate the erosion when the ground temperature reaches a high temperature in summer. In order to ensure the stability of the salt solution concentration in the high-temperature curing box, the solution is replaced after each large cycle.
[0036] S22: After the high temperature erosion stage is completed, the concrete specimen is first placed in an oven for drying. After the drying is completed, the concrete specimen is placed at room temperature for cooling. After cooling, it is placed in a salt solution for immersion, which is a dry-wet cycle. The salt solution level is higher than the top surface of the concrete specimen, and the salt solution is replaced once at a specified time to ensure the stability of the solution concentration, and the set number of dry-wet cycles is completed;
[0037] S23: A freeze-thaw cycle erosion test of concrete specimens is conducted using a concrete freeze-thaw test chamber. The concrete specimens after dry-wet cycles are placed in the freeze-thaw cycle chamber, and a saturated salt solution is injected into the concrete specimen box. The water level in the box is always kept higher than the top surface of the concrete specimen.
[0038] S24: Use a low-temperature test chamber to conduct a low-temperature corrosion stage test of concrete testing. Take out the concrete specimens after freeze-thaw cycles, wipe the surface moisture with a dry cloth, place them in a ventilated place to dry naturally, then soak them in a salt solution until they reach a saturated state, and then place them in a low-temperature test chamber for low-temperature corrosion;
[0039] S25: Take high temperature corrosion, dry-wet cycle corrosion, freeze-thaw cycle corrosion and low temperature corrosion as a large corrosion cycle, and complete the corrosion test of the set cycle on the concrete specimen.
[0040] As a further preferred embodiment of the above technical solution: in step S3, the macroscopic performance test indicators include mass change rate, compressive strength, flexural strength and relative dynamic elastic modulus.
[0041] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0042] 1. From the perspective of considering the diversity of erosion factors, the present invention comprehensively considers the combined effects of high temperature, low temperature, dry-wet cycle, freeze-thaw cycle and high-concentration erosive salt solution in the western saline soil environment. By investigating the basic information such as the western saline soil environment and climate, the annual average high temperature, low temperature, freeze-thaw cycle number and normal temperature duration are determined, and the type and concentration of erosive salt solution are statistically analyzed. By comprehensively considering multiple factors, the erosion process of concrete in the actual environment can be more realistically simulated, avoiding the limitations of single-factor erosion research.
[0043] 2. The present invention ensures that the indoor accelerated corrosion test is similar to the corrosion process in the actual environment from the aspect of solving the similarity of the degradation coefficient by calculating the ion concentration acceleration coefficient, the dry-wet cycle acceleration coefficient and the equivalent freeze-thaw cycle acceleration coefficient; through the ion concentration similarity theory, the comparison between the laboratory temperature and the actual ambient temperature and the rapid freeze-thaw test method, the degradation coefficient of different corrosion stages is accurately solved, so that the test results have a higher practical reference value.
[0044] 3. From the feasibility of the accelerated erosion scheme, the present invention has formulated the erosion duration of each stage of high temperature, low temperature, dry-wet cycle and freeze-thaw cycle according to the accelerated degradation coefficient and actual climatic conditions. The accelerated test is carried out by increasing the concentration of the erosion solution, alternating dry-wet cycles and rapid freeze-thaw cycles, which effectively shortens the experimental time. The indoor accelerated erosion simulation scheme of the present invention is not only feasible under laboratory conditions, but also can provide an effective concrete durability assessment method, providing a theoretical basis and technical support for the design of concrete structures under saline soil environments in the west. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required in the embodiments are briefly introduced below.
[0046] Figure 1 A schematic diagram of a process for establishing an indoor accelerated erosion simulation scheme for the present invention;
[0047] Figure 2 A temperature change diagram of the Baijiantan area provided in Examples 1-3 of the present invention;
[0048] Figure 3 The corresponding relationship between the actual erosion time and the indoor erosion time provided in Examples 1-3 of the present invention;
[0049] Figure 4 The indoor erosion simulation scheme for the western saline soil environment provided in Examples 1-3 of the present invention;
[0050] Figure 5 The results of the effects of different water-cement ratios, fiber types and mineral admixture types provided in Example 1 of the present invention on the macroscopic properties of concrete specimens under the erosion simulation scheme of the present invention;
[0051] Figure 6 The results of the effects of different curing schemes provided in Example 2 of the present invention on the macroscopic performance of concrete specimens under the erosion simulation scheme of the present invention;
[0052] Figure 7 The macroscopic performance influence results of concrete specimens corroded by different salt solution types provided in Example 3 of the present invention under the corrosion simulation scheme of the present invention. DETAILED DESCRIPTION
[0053] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiments will be described clearly and completely in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments, not all of the embodiments. For ordinary technicians in this field, other embodiments can be obtained without creative work.
[0054] Embodiment 1:
[0055] Reference Figure 1-5 The present invention is an indoor accelerated erosion test method for simulating the saline soil environment in the western region. Taking the Baijiantan area in Xinjiang as an example, the specific steps are as follows:
[0056] S1: Establish an indoor accelerated erosion simulation scheme for saline soil environment in the west;
[0057] S2: Erosion test on concrete specimens based on indoor accelerated erosion simulation scheme;
[0058] S3: Conduct macroscopic performance tests on the concrete specimens after the erosion test to obtain erosion results under simulated conditions.
[0059] Specifically, the steps to establish an indoor accelerated erosion simulation program include surveying environmental characteristic information of western saline soils, calculating accelerated degradation coefficients, and determining the duration of erosion stages;
[0060] The environmental characteristics of saline soil in western China include: calculation of annual average high temperature, annual average low temperature, annual number of freeze-thaw cycles, annual average normal temperature duration, and statistics of saline soil erosion solution types and concentrations;
[0061] According to the historical meteorological data of Baijiantan area, and referring to the standards for issuing high temperature and low temperature warning signals in Karamay City, weather with a temperature greater than 35℃ is defined as high temperature weather, and weather with a temperature below -20℃ is defined as low temperature weather; according to the meteorological data of Baijiantan area provided by the National Meteorological Administration, the number of days with temperatures above 35℃ and below -20℃ in the area from 2013 to 2022 was counted, and the results are as follows: Figure 2 As shown;
[0062] According to the statistical results, the average annual high temperature days in the region are 20 days, and the average annual low temperature days are 19 days. The maximum daily temperature in summer and autumn and the minimum daily temperature in winter and spring in Xinjiang last for 3 hours. It is calculated that the annual average high temperature duration is 20×3=60 hours, about 3 days, and the annual average low temperature duration is 19×3=57 hours, about 3 days.
[0063] The number of freeze-thaw cycles per year refers to the number of times the lowest temperature of a day is below 0°C and the highest temperature of the day is above 0°C. Under this condition, the concrete is considered to be subjected to one freeze-thaw cycle. According to the statistical results of meteorological data, the average number of freeze-thaw cycles per year in this area is 95 times, that is, 95 days.
[0064] The annual average normal temperature duration is the number of days in a year after removing the annual average high temperature duration, the annual average low temperature duration and the annual number of freeze-thaw cycles. Considering that a year is 365 days, the annual average normal temperature duration is 365-3-3-95=264d.
[0065] Furthermore, in order to better reflect the rationality of the indoor accelerated corrosion simulation scheme formulated by the present invention and the reliability of the indoor accelerated corrosion test, this embodiment simulates the erosion conditions of the field environment in the region for 5 years, and the durations of high temperature, normal temperature, low temperature and freeze-thaw cycles are 15d, 1320d, 15d and 475d respectively;
[0066] The statistics of saline soil erosion solution types and concentrations are mainly based on geological survey data in the western region to determine the concentration range of sulfate ions and chloride ions. The Baijiantan area in Xinjiang is located in an area where saline soils are widely distributed in my country. The soil pH is 7.76-10.58, and the erosion salt types are mainly sulfate and chloride. The sulfate ion concentration is 10000-20000 mg / L, and the chloride ion concentration is less than 10000 mg / L.
[0067] The calculation of accelerated degradation coefficient includes the calculation of ion concentration acceleration coefficient, dry-wet cycle acceleration coefficient and equivalent freeze-thaw cycle acceleration coefficient;
[0068] The ion concentration acceleration coefficient is calculated according to the ion concentration similarity theory according to the following formula, where the sulfate solution used in this embodiment is a 10% Na 2 SO 4 Solution, compound salt solution is 10% Na 2 SO 4 +5% NaCl solution, the actual sulfate concentration in saline soil environment is about 2%, and the chloride concentration is about 1%; the concentration of the erosion salt solution selected in this embodiment is 5 times the actual concentration of the erosion salt solution, so the ion concentration under the influence of the erosion solution concentration accelerates the degradation coefficient F d is 5;
[0069]
[0070] In the formula, C s fie With C s lab are the surface ion concentrations of concrete in actual environment and indoor test, %.
[0071] The calculation of the dry-wet cycle acceleration factor first requires the determination of the drying temperature, drying time, cooling time, soaking time, dry-wet ratio and cycle period; the drying time and the drying time are considered to be stable, and to avoid the influence of temperature stress on the damage process of the concrete specimen. In this embodiment, the drying temperature is set to 60°C, the drying time is 6h, and the specimen is placed at room temperature for cooling for 2h and then soaked in the corrosive salt solution for 16h. A dry-wet cycle period is 24h, and the dry-wet ratio is 1:2;
[0072] The laboratory temperature for the indoor accelerated test in this embodiment was measured by a thermometer to be 15°C, that is, the average temperature T 1 ; The average temperature T during the dry-wet cycle can be calculated as follows 2 ;
[0073]
[0074] Where M 1 is the drying time, h; N 1 is the drying temperature, ℃; M 2 is the soaking time, h; M 3 is the cooling time, h; M is the duration of a dry-wet cycle, h;
[0075] According to the activation energy coefficient obtained from the Atkinson erosion system, the dry-wet cycle acceleration coefficient T of this embodiment is calculated according to the following formula: d , T d The calculated result is 8.64;
[0076]
[0077] Where, T 1 is the indoor test environment temperature, ℃; T 2 is the average temperature under the dry and wet system, °C; K is the temperature unit Kelvin; E / R is the activation energy, and Atkinson measured its value as 14242 through experiments;
[0078] The equivalent freeze-thaw cycle acceleration factor refers to the number of corresponding indoor rapid freeze-thaw cycles that the concrete must undergo when the degree of concrete damage is consistent with that after several on-site freeze-thaw cycles; according to the rapid freeze-thaw test method formulated according to the domestic concrete test regulations, the comparison relationship between concrete freeze-thaw damage in indoor tests and natural environments is between 1:10-1:15. In this embodiment, the middle value of 1:12 is selected as the equivalent freeze-thaw cycle acceleration factor N d , that is, it is considered that one indoor rapid freeze-thaw cycle is equivalent to 12 freeze-thaw cycles in the natural environment, so the equivalent freeze-thaw cycle acceleration factor N in this embodiment is d is 12.
[0079] Furthermore, the determination of the duration of the erosion stage includes the determination of the duration of the high temperature and low temperature erosion stages, the duration of the freeze-thaw cycle erosion stage, and the duration of the normal temperature erosion stage;
[0080] Specifically, the duration of the high temperature and low temperature corrosion stages is determined according to the calculation result of the ion concentration acceleration coefficient; in this embodiment, the ion concentration acceleration coefficient F calculated according to the above calculation is d , the accelerated degradation coefficients of high temperature and low temperature corrosion stages are obtained as S d1 =S d2 =F d =5, that is, the high temperature and low temperature corrosion time in the field environment for 5 years (both are 15 days), and the corresponding high temperature and low temperature corrosion time in the laboratory are both 3 days;
[0081] The duration of the freeze-thaw cycle erosion phase is determined according to the calculation result of the equivalent freeze-thaw cycle acceleration coefficient, and a rapid freeze-thaw cycle time is set; in this embodiment, the equivalent freeze-thaw cycle acceleration coefficient N calculated above is d , the accelerated degradation coefficient of the freeze-thaw erosion cycle erosion stage is obtained as S d3 =F d ×N d =5×12=60; set the indoor rapid freeze-thaw cycle to be performed every 6 hours, 4 times a day, that is, the actual environmental freeze-thaw erosion time corresponds to the indoor freeze-thaw cycle erosion stage duration of 2 days;
[0082] The duration of the normal temperature erosion stage is determined according to the calculation result of the dry-wet cycle acceleration coefficient; in this embodiment, the dry-wet cycle acceleration coefficient T calculated above is d , the accelerated degradation coefficient of the dry-wet cycle erosion stage is obtained as S d3 =F d ×T d =5×8.64=43.2, that is, the laboratory dry-wet cycle erosion time corresponding to the normal temperature erosion time in the actual environment is about 30 days; the corresponding relationship between the western saline soil erosion environment and the duration of each erosion stage in the indoor accelerated erosion scheme can be obtained, such as Figure 3 As shown, and based on the corresponding relationship, the following is established Figure 4 An indoor accelerated erosion simulation scheme for a western saline soil environment is shown.
[0083] Indoor erosion tests are carried out based on the established indoor accelerated erosion simulation scheme, including four stages: high temperature erosion, dry-wet cycle erosion, freeze-thaw cycle erosion and low temperature erosion:
[0084] 1) High temperature erosion stage
[0085] The concrete specimens were placed in a high-temperature curing box and soaked in a salt solution. The solution was 20 cm higher than the concrete specimens during the soaking. The specimens were sealed with plastic wrap. The temperature of the salt solution in the high-temperature curing box was maintained at a constant temperature of 45°C to simulate the erosion when the ground temperature reached high temperatures in summer. To ensure the stability of the salt solution concentration in the high-temperature curing box, the solution was replaced after each large cycle. The high-temperature erosion stage lasted for 3 days.
[0086] 2) Dry-wet cycle erosion stage
[0087] After the high-temperature erosion stage, the concrete specimens were first placed in a 60°C oven for drying. After the drying, the concrete specimens were placed at room temperature for cooling for 2 hours, and then the cooled specimens were immersed in a salt solution for 16 hours. This was a dry-wet cycle with a cycle of 24 hours. The salt solution level was 20 cm higher than the surface of the concrete specimens, and the salt solution was replaced every 15 days to ensure the stability of the solution concentration. The dry-wet cycle erosion stage lasted for 15 days.
[0088] 3) Freeze-thaw cycle erosion stage
[0089] The concrete freeze-thaw test box is used to conduct freeze-thaw cycle erosion test on concrete specimens. The concrete specimens after dry-wet cycles are placed in the freeze-thaw cycle box, and saturated salt solution is injected into the specimen box. The water level in the box should always be kept at least 5 cm higher than the top surface of the concrete specimen. The rapid freeze-thaw method is used, and a rapid freeze-thaw cycle is performed every 6 hours. The minimum and maximum temperatures at the center of the concrete specimen should be controlled at -20°C and 10°C, respectively, and the number of freeze-thaw cycles is set to 8 times, that is, the duration of the freeze-thaw cycle erosion stage is 2 days;
[0090] 4) Low temperature corrosion stage
[0091] A low-temperature test chamber was used to conduct a low-temperature corrosion stage test on concrete specimens. The concrete specimens after freeze-thaw cycles were taken out, and the surface moisture was wiped off with a dry cloth, and placed in a ventilated place to dry naturally. The dried concrete specimens were soaked in a salt solution for 2 days to reach a saturated state, and then placed in a -35°C low-temperature test chamber for corrosion. The low-temperature corrosion stage lasted for 3 days.
[0092] The indoor accelerated corrosion test method of the present invention takes high temperature corrosion, dry-wet cycle corrosion, freeze-thaw cycle corrosion and low temperature corrosion as one large corrosion cycle. In this embodiment, 40 days is taken as one corrosion cycle, and a total of 6 corrosion cycles are designed, totaling 240 days, which is equivalent to placing the concrete specimen in the actual western saline soil environment for corrosion for 30 years.
[0093] In this embodiment, the mix ratio of the concrete specimens is shown in Table 1. The macroscopic properties such as compressive strength, flexural strength and relative dynamic elastic modulus can be tested by corroding the concrete specimens to corresponding cycles.
[0094] Table 1 Mix ratio of concrete specimens
[0095]
[0096]
[0097] In the specimen numbers in Table 1, the number before “-” indicates the water-cement ratio of the concrete specimen, “S” and “P” represent steel fiber and polyvinyl alcohol fiber, respectively, and “SF” represents silica fume.
[0098] In this embodiment, high temperature curing is used for curing of concrete specimens, and a concentration of 10% Na 2 SO 4 A sulfate solution is used as the etching salt solution.
[0099] The macroscopic performance test results of concrete specimens with different water-binder ratios, fiber types and mineral admixture types under the indoor accelerated corrosion simulation scheme of the present invention are shown in Tables 2 to 5, and the degradation rules are as follows: Figure 5 As shown, Figure 5 (a) represents the mass change rate, Figure 5 (b) indicates compressive strength, Figure 5 (c) represents the flexural strength, Figure 5 (d) represents the relative dynamic elastic modulus.
[0100] Table 2 Test results of specimen mass change rate under different water-binder ratios, fiber types and mineral admixture types
[0101]
[0102] Table 3 Compressive strength test results of specimens under different water-binder ratios, fiber types and mineral admixture types
[0103]
[0104]
[0105] Table 4 Flexural strength test results of specimens at different water-binder ratios, fiber types and mineral admixture types
[0106]
[0107] Table 5 Test results of relative dynamic elastic modulus of specimens under different water-binder ratios, fiber types and mineral admixture types
[0108]
[0109] Embodiment 2:
[0110] Different from Example 1, considering the influence of different curing systems on the macroscopic properties of concrete specimens such as compressive strength, flexural strength and relative dynamic elastic modulus under the indoor accelerated erosion simulation scheme of the present invention, an indoor accelerated erosion test was carried out. The concrete specimen mix ratio of this embodiment is shown in Table 6.
[0111] Table 6 Mix ratio of concrete specimens
[0112]
[0113] In the specimen numbers in Table 6, "BY" stands for standard curing, and the specimen numbers without "BY" adopt high-temperature curing. Standard curing means placing the concrete specimens in a standard curing room with a temperature of 20±2℃ and a relative humidity of 95% for curing to 28 days. High-temperature curing means placing the concrete specimens in 90℃ hot water for curing for 72 hours, and then placing them in a standard curing room with a temperature of 20±2℃ and a relative humidity of 95% for curing to 28 days.
[0114] The macro performance test results of concrete specimens with different curing systems under this erosion scheme are shown in Tables 7 to 10. The degradation rules are as follows: Figure 6 As shown, Figure 6 (a) represents the mass change rate, Figure 6 (b) indicates compressive strength, Figure 6 (c) represents the flexural strength, Figure 6 (d) represents the relative dynamic elastic modulus.
[0115] Table 7 Test results of specimen quality change rate under different curing systems
[0116]
[0117] Table 8 Compressive strength test results of specimens under different curing systems
[0118]
[0119] Table 9 Flexural strength test results of specimens under different curing systems
[0120]
[0121] Table 10 Test results of relative dynamic elastic modulus of specimens under different curing systems
[0122]
[0123] Embodiment 3:
[0124] Different from Examples 1-2, an indoor accelerated corrosion test was conducted considering the influence of different types of corrosive salt solutions on the macroscopic properties of concrete specimens such as compressive strength, flexural strength and relative dynamic elastic modulus under the indoor accelerated corrosion simulation scheme of the present invention. The formulation ratio of the concrete specimens in this embodiment is shown in Table 11.
[0125] Table 11 Mix ratio of concrete specimens
[0126]
[0127] Preferably, "FH" represents a concentration of 10% Na 2 SO 4 +5% NaCl composite salt solution corrosion, the specimen number without "FH" is 10% Na 2 SO 4 of sulfate solutions.
[0128] The macro performance test results of concrete specimens with different types of corrosive salt solutions under this scheme are shown in Tables 12 to 15. The degradation rules are as follows: Figure 7 As shown, Figure 7 (a) represents the mass change rate, Figure 7 (b) indicates compressive strength, Figure 7 (c) represents the flexural strength, Figure 7 (d) represents the relative dynamic elastic modulus.
[0129] Table 12 Test results of mass change rate of concrete specimens under different types of corrosive salt solutions
[0130]
[0131] Table 13 Compressive strength test results of concrete specimens under different types of corrosive salt solutions
[0132]
[0133] Table 14 Test results of flexural strength of concrete specimens under different types of corrosive salt solutions
[0134]
[0135] Table 15 Test results of relative dynamic elastic modulus of concrete specimens under different types of corrosive salt solutions
[0136]
[0137] It should be clear that the above detailed description of the embodiments of the present invention provided in the accompanying drawings is only used to further illustrate the present invention and is not intended to limit the scope of the invention claimed for protection, but only represents selected embodiments of the present invention. Based on the embodiments of the present invention, some non-essential improvements and adjustments made by ordinary technicians in this field according to the above content of the present invention belong to the protection scope of the present invention.
Claims
1. An indoor accelerated erosion test method simulating the western saline soil environment, characterized in that: The following steps are involved: S1: Determine the indoor accelerated erosion simulation scheme for western saline soil environment; S2: Erosion test on concrete specimens based on indoor accelerated erosion simulation scheme; S3: Conduct macroscopic performance tests on the concrete specimens after the erosion test to obtain erosion results under simulated conditions.
2. The indoor accelerated erosion test method for simulating the western saline soil environment according to claim 1, characterized in that: In step S1, determining the indoor accelerated erosion simulation scheme includes the following steps: S11: Investigate the environmental characteristics of saline soil in western China; S12: Calculating an accelerated degradation coefficient based on the obtained environmental characteristic information; S13: Determine the duration of each corrosion stage according to the accelerated degradation coefficient.
3. The indoor accelerated erosion test method for simulating the western saline soil environment according to claim 2, characterized in that: In step S11, the environmental characteristic information of the western saline soil includes the calculation of the annual average high temperature, the annual average low temperature, the annual number of freeze-thaw cycles, the average normal temperature duration, and the statistics of the type and concentration of the saline soil erosion solution.
4. The indoor accelerated erosion test method for simulating the western saline soil environment according to claim 3, characterized in that: In step S12, the calculation of the accelerated degradation coefficient includes the calculation of the ion concentration acceleration coefficient, the dry-wet cycle acceleration coefficient and the equivalent freeze-thaw cycle acceleration coefficient, wherein: The ion concentration acceleration factor is calculated according to the ion concentration similarity theory, and the ion concentration acceleration factor F under the influence of the corrosion solution concentration is obtained. d ; In the formula, C s fie With C s lab are the surface ion concentrations of concrete in actual environment and indoor test, respectively; The calculation of the dry-wet cycle acceleration factor is based on the average temperature of the laboratory and the average temperature during the dry-wet cycle. The calculation formula is as follows: Where, T d is the dry-wet cycle acceleration factor, T1 is the average temperature of the laboratory, T2 is the average temperature during the dry-wet cycle, E / R is the activation energy, and K is the temperature unit Kelvin; The equivalent freeze-thaw cycle acceleration factor refers to the number of corresponding indoor rapid freeze-thaw cycles that the concrete must undergo when the degree of damage to the concrete is consistent with that after several on-site freeze-thaw cycles.
5. The indoor accelerated erosion test method for simulating the western saline soil environment according to claim 4, characterized in that: The calculation process of the dry-wet cycle acceleration coefficient is as follows: Determine the drying temperature, drying time, cooling time, soaking time, dry-wet ratio and cycle period; The average temperature T2 during the dry-wet cycle is calculated based on the average laboratory temperature T1, and then the dry-wet cycle acceleration coefficient is obtained by combining T1 and T2. The calculation formula for T2 is as follows: Wherein, M1 is the drying time, N1 is the drying temperature, M2 is the soaking time, M3 is the cooling time, and M is the duration of a dry-wet cycle.
6. The indoor accelerated erosion test method for simulating the western saline soil environment according to claim 5, characterized in that: In step S13, the determination of the duration of each corrosion stage includes the determination of the duration of the high temperature and low temperature corrosion stages, the duration of the freeze-thaw cycle corrosion stage and the duration of the normal temperature corrosion stage, wherein: the duration of the high temperature and low temperature corrosion stages is determined according to the calculation result of the ion concentration acceleration coefficient; The duration of the freeze-thaw cycle erosion phase is determined based on the calculation results of the equivalent freeze-thaw cycle acceleration coefficient, and the time and number of rapid freeze-thaw cycles are set; The duration of the normal temperature erosion stage is determined based on the calculation results of the dry-wet cycle acceleration coefficient.
7. The indoor accelerated erosion test method for simulating the western saline soil environment according to claim 6, characterized in that: In step S2, the corrosion test of the concrete specimen includes four stages: high temperature corrosion, dry-wet cycle corrosion, freeze-thaw cycle corrosion and low temperature corrosion. The specific steps are as follows: S21: Place the concrete specimen in a high temperature curing box, soak the concrete specimen with a salt solution, seal it and maintain a constant temperature; S22: After the high temperature erosion stage, the concrete specimen is dried and cooled at room temperature, and then immersed in a salt solution, which is a dry-wet cycle, and the set number of dry-wet cycles is completed; S23: placing the concrete specimen after the dry-wet cycle in a freeze-thaw cycle box, injecting a saturated salt solution into the concrete specimen box, and the water level in the box is higher than the top surface of the concrete specimen; S24: Wipe off the moisture on the surface of the concrete specimen after freeze-thaw cycles and dry it naturally in a ventilated place. After drying, soak it in a salt solution until it reaches a saturated state, and then put it in a low-temperature test chamber for low-temperature corrosion; S25: Take high temperature corrosion, dry-wet cycle corrosion, freeze-thaw cycle corrosion and low temperature corrosion as a large corrosion cycle, and complete the corrosion test of the set cycle on the concrete specimen.
8. The indoor accelerated erosion test method for simulating the western saline soil environment according to claim 7, characterized in that: In step S21 and step S22, when the concrete specimen is immersed in the salt solution, the liquid level of the salt solution is higher than the concrete specimen.
Citation Information
Patent Citations
Salt freezing-dry and wet cycle coupling test device and method for cement-based materials
CN108426823A
Acceleration test method of semiconductor memory
CN1183647A
Post-constructed PC balcony
KR102223854B1