Method for testing toughening modification effect of epoxy resin adhesive

By measuring the volume shrinkage rate of epoxy resin adhesive, the problems of large measurement error of linear shrinkage rate and high cost of tensile testing machines in the prior art are solved, and a simple and effective toughening modification test method can be effectively evaluated. Modification effect of toughener.

CN118937647APending Publication Date: 2024-11-12LUOYANG XIZHIAO NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975944.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, when determining the curing shrinkage rate of epoxy adhesive, the linear shrinkage rate method has uneven curing, resulting in large measurement errors, and the tensile testing machine occupies a large space and is costly, so it is impossible to effectively express the bonding strength of the toughening agent. .

Method used

Provide a test method for toughening modification effect of epoxy resin adhesive. By preparing component A and component B glue solution, removing solvents using vacuum oven, and curing at room temperature, measuring uncured and The density difference after curing was calculated, and the volume shrinkage rate was calculated to evaluate the toughening modification effect.

Benefits of technology

This method simplifies operation, reduces equipment costs, provides a diverse comparison method, can effectively evaluate the modification effects of different toughening agents, make up for the defects of the tensile test machine, and improves the scientificity and accuracy of measurement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954509030000023
    Figure BDA0004954509030000023
  • Figure BDA0004954509030000031
    Figure BDA0004954509030000031
  • Figure BDA0004954509030000033
    Figure BDA0004954509030000033
Patent Text Reader

Abstract

The invention discloses a method for testing the toughening modification effect of an epoxy resin adhesive, the method is based on the fact that the curing shrinkage rate is an important characterization index of the bonding strength of the epoxy adhesive, and the specific testing method comprises the steps of preparation of the epoxy adhesive, determination of the curing shrinkage rate of the adhesive and analysis treatment of a sample result. Redundant solvent in the epoxy glue solution is removed by a vacuum oven, and the volume expansion of the adhesive caused by solvent volatilization is reduced by a normal-temperature curing method, so that the accuracy of an experimental result is ensured, and the test error between parallel samples is reduced; the testing method is low in cost and simple to operate, makes up the vacancy of lack of tension testing machine equipment for testing the bonding strength of the adhesive, and meanwhile, the detection method for toughening modified epoxy resin provided by the invention can change the types of the toughening agents and carry out transverse comparison, and provides a diversified comparison mode for comparing the toughening effect of the adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy adhesives, and particularly relates to a method for testing the toughening and modification effect of epoxy resin adhesives. Background Art

[0002] Tensile testing machines are generally used to measure the bonding strength of toughened modified adhesives, but tensile testing machines take up a lot of space and are expensive. The bonding strength of some toughened adhesives is not reflected in the tensile strength. Curing shrinkage is an important indicator of the bonding strength of epoxy adhesives, especially when using toughening agent-modified epoxy resins. There are currently two common methods for determining curing shrinkage, namely volume shrinkage and linear shrinkage. The linear shrinkage determination method is a standard established for thermosetting resins. It mainly determines the change in size on a certain linear scale before and after the adhesive is cured. However, the uneven curing of the adhesive forms an irregular shape, which results in a large measurement error, and the experimental results obtained are not scientific. Summary of the invention

[0003] In order to overcome the above problems, the present invention provides a testing method for the toughening and modification effect of epoxy resin adhesive, which can not only detect the volume shrinkage of epoxy adhesive, but also horizontally compare the toughening and modification effects of different toughening agents.

[0004] The technical solution adopted by the present invention is:

[0005] A method for testing the toughening and modification effect of an epoxy resin adhesive comprises the following steps:

[0006] Step 1: Prepare component A glue: dissolve 0-10 parts of toughening agent in a low boiling point solvent, and mix evenly with 100 parts of epoxy resin at room temperature, and remove the solvent of the mixture in a vacuum oven to obtain component A glue;

[0007] Step 2: Prepare component B glue: mix 70 parts of curing agent and 30 parts of accelerator evenly to obtain component B glue;

[0008] Step 3: Mix the glue of component A and the glue of component B and divide them into two glues;

[0009] Step 4: Fill the container with one of the adhesive solutions and measure the relative density of the adhesive before curing, which is recorded as ρ1;

[0010] Step 5: Apply another portion of the adhesive solution to the mold and cure it at room temperature for 24 hours. After demoulding, a solid adhesive film is obtained. 5g-10g of the solid adhesive film is weighed and placed in a container. The relative density is measured and recorded as ρ2;

[0011] Step 6: Calculate volume shrinkage

[0012] Among them, the toughening agent in step 1 is a combination of one or more of dibutyl phthalate, dioctyl phthalate, liquid polysulfide rubber, liquid nitrile rubber, liquid chloroprene rubber, liquid polyether, and CSR.

[0013] Wherein, in step 1, the low boiling point solvent is a combination of one or more of butanone, ethylene glycol monomethyl ether, acetone and tetrahydrofuran.

[0014] Among them, the curing agent in step 2 is a mixture of one or more of ethylenediamine, diethylenetriamine, m-phenylenediamine, benzyldimethylamine, isophoronediamine, 2-ethyl-4-methylimidazole, 4,4'-methylenebis(2-methyl-6-ethylaniline), phthalic anhydride, maleic anhydride, and hexahydrophthalic anhydride.

[0015] Among them, the accelerator in step 2 is a mixture of one or more of dicyandiamide, boron trifluoride monoethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, N-(2-hydroxyphenyl)-N',N'-dimethylurea, N-(5-chloro-2-hydroxybenzene)-N',N'-dimethylurea, N,N-dimethylethanolamine, nonylphenol, and resorcinol.

[0016] Wherein, the container is a specific gravity bottle.

[0017] Among them, the volume shrinkage rate in step 6 Calculated based on ρ1 and ρ2;

[0018] The calculation formula of ρ1 is as follows:

[0019]

[0020] Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; ρ0 is the water density at room temperature;

[0021] The formula for calculating ρ2 is as follows:

[0022]

[0023] Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; m3 is the mass of the pycnometer after a certain mass of solid film is filled; ρ0 is the water density at room temperature;

[0024] The calculation formula is as follows:

[0025]

[0026] The advantages of the present invention are as follows:

[0027] 1. During the testing process, the operation is simple, which makes up for the lack of tensile testing equipment to measure the bonding strength and reduces the R&D cost of the enterprise;

[0028] 2. The type of toughening agent can be changed for horizontal comparison, providing a diverse comparison method for comparing the toughening effect of adhesives. DETAILED DESCRIPTION

[0029] The present invention will be further described below, but the present invention is not limited to these contents.

[0030] Example 1

[0031] A method for testing the toughening and modification effect of an epoxy resin adhesive comprises the following steps:

[0032] Step 1: Prepare component A glue: 100 parts of liquid epoxy resin without toughening agent, and remove the solvent in a vacuum oven;

[0033] Step 2: Prepare component B glue: mix 70 parts of curing agent and 30 parts of accelerator evenly;

[0034] Step 3: Mix the glue of component A and the glue of component B and divide them into two glues;

[0035] Step 4: Fill the container with one of the adhesive solutions and measure the relative density of the adhesive before curing, which is recorded as ρ1;

[0036] Step 5: Apply another portion of the adhesive solution to the mold and cure it at room temperature for 24 hours. After demoulding, a solid adhesive film is obtained. Weigh 5 g of the solid adhesive film and place it in a container. Measure the relative density, which is recorded as ρ2;

[0037] Step 6: Calculate volume shrinkage

[0038] Among them, the calculation formula of ρ1 is as follows:

[0039]

[0040] Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; ρ0 is the water density at room temperature;

[0041] The formula for calculating ρ2 is as follows:

[0042]

[0043] Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; m3 is the mass of the pycnometer after a certain mass of solid film is filled; ρ0 is the water density at room temperature;

[0044] The calculation formula is as follows:

[0045]

[0046] Embodiment 2:

[0047] A method for testing the toughening and modification effect of an epoxy resin adhesive comprises the following steps:

[0048] Step 1: Prepare component A glue: dissolve 5 parts of toughening agent in a low boiling point solvent, mix well with 100 parts of epoxy resin at room temperature, and remove the solvent of the mixture in a vacuum oven;

[0049] Step 2: Prepare component B glue: mix 70 parts of curing agent and 30 parts of accelerator evenly;

[0050] Step 3: Mix the glue of component A and the glue of component B and divide them into two glues;

[0051] Step 4: Fill the container with one of the adhesive solutions and measure the relative density of the adhesive before curing, which is recorded as ρ1;

[0052] Step 5: Apply another portion of the adhesive solution to the mold and cure it at room temperature for 24 hours. After demoulding, a solid adhesive film is obtained. Weigh 5 g of the solid adhesive film and place it in a container. Measure the relative density, which is recorded as ρ2;

[0053] Step 6: Calculate volume shrinkage

[0054] Among them, the calculation formula of ρ1 is as follows:

[0055]

[0056] Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; ρ0 is the water density at room temperature;

[0057] The formula for calculating ρ2 is as follows:

[0058]

[0059] Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; m3 is the mass of the pycnometer after a certain mass of solid film is filled; ρ0 is the water density at room temperature;

[0060] The calculation formula is as follows:

[0061]

[0062] Example 3

[0063] A method for testing the toughening and modification effect of an epoxy resin adhesive comprises the following steps:

[0064] Step 1: Prepare component A glue: dissolve 10 parts of toughening agent in a low boiling point solvent, mix well with 100 parts of epoxy resin at room temperature, and remove the solvent of the mixture in a vacuum oven;

[0065] Step 2: Prepare component B glue: mix 70 parts of curing agent and 30 parts of accelerator evenly;

[0066] Step 3: Mix the glue of component A and the glue of component B and divide them into two glues;

[0067] Step 4: Fill the container with one of the adhesive solutions and measure the relative density of the adhesive before curing, which is recorded as ρ1;

[0068] Step 5: Apply another portion of the adhesive solution to the mold and cure it at room temperature for 24 hours. After demoulding, a solid adhesive film is obtained. Weigh 5 g of the solid adhesive film and place it in a container. Measure the relative density, which is recorded as ρ2;

[0069] Step 6: Calculate volume shrinkage

[0070] Among them, the calculation formula of ρ1 is as follows:

[0071]

[0072] Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; ρ0 is the water density at room temperature;

[0073] The formula for calculating ρ2 is as follows:

[0074]

[0075] Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; m3 is the mass of the pycnometer after a certain mass of solid film is filled; ρ0 is the water density at room temperature;

[0076] The calculation formula is as follows:

[0077]

[0078] It is pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all fall within the protection scope of the present invention.

Claims

1. A method for testing the toughening and modification effect of epoxy resin adhesive, characterized in that: The following steps are involved: Step 1: Prepare component A glue: dissolve 0-10 parts of toughening agent in a low boiling point solvent, and mix evenly with 100 parts of epoxy resin at room temperature, and remove the solvent of the mixture in a vacuum oven to obtain component A glue; Step 2: Prepare component B glue: mix 70 parts of curing agent and 30 parts of accelerator evenly to obtain component B glue; Step 3: Mix the glue of component A and the glue of component B and divide them into two glues; Step 4: Fill the container with one of the adhesive solutions and measure the relative density of the adhesive before curing, which is recorded as ρ1; Step 5: Apply another portion of the adhesive solution to the mold and cure it at room temperature for 24 hours. After demoulding, a solid adhesive film is obtained. 5g-10g of the solid adhesive film is weighed and placed in a container. The relative density is measured and recorded as ρ2; Step 6: Calculate the volume shrinkage φ.

2. The method for testing the toughening and modification effect of an epoxy resin adhesive according to claim 1, characterized in that: The toughening agent in step 1 is a combination of one or more of dibutyl phthalate, dioctyl phthalate, liquid polysulfide rubber, liquid nitrile rubber, liquid chloroprene rubber, liquid polyether, and CSR.

3. The test method for toughening and modifying effect of epoxy resin adhesive according to claim 1, characterized in that: In the step 1, the low boiling point solvent is a combination of one or more of butanone, ethylene glycol monomethyl ether, acetone and tetrahydrofuran.

4. The method for testing the toughening and modification effect of an epoxy resin adhesive according to claim 1, characterized in that: The curing agent in step 2 is a mixture of one or more of ethylenediamine, diethylenetriamine, m-phenylenediamine, benzyldimethylamine, isophoronediamine, 2-ethyl-4-methylimidazole, 4,4'-methylenebis(2-methyl-6-ethylaniline), phthalic anhydride, maleic anhydride, and hexahydrophthalic anhydride.

5. The method for testing the toughening and modification effect of an epoxy resin adhesive according to claim 1, characterized in that: The accelerator in step 2 is a mixture of one or more of dicyandiamide, boron trifluoride monoethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, N-(2-hydroxyphenyl)-N',N'-dimethylurea, N-(5-chloro-2-hydroxybenzene)-N',N'-dimethylurea, N,N-dimethylethanolamine, nonylphenol, and resorcinol.

6. The method for testing the toughening and modification effect of an epoxy resin adhesive according to claim 1, characterized in that: The container is a specific gravity bottle.

7. The method for testing the toughening and modification effect of an epoxy resin adhesive according to claim 1, characterized in that: In step 6, the volume shrinkage φ is calculated based on ρ1 and ρ2; The ρ1 calculation formula is as follows: Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; ρ0 is the water density at room temperature; The ρ2 calculation formula is as follows: Where: m0 is the mass of the pycnometer; m1 is the mass of the pycnometer filled with water; m2 is the mass of the pycnometer filled with liquid epoxy adhesive; m3 is the mass of the pycnometer after a certain mass of solid film is filled; ρ0 is the water density at room temperature; Said The calculation formula is as follows: