Pit punching quality detection method for aluminum-plastic film insulating layer

By measuring the leakage current and pit depth of the aluminum-plastic film, combined with the conductive dielectric and voltage, the problem of poor insulation of the aluminum-plastic film in the existing technology is solved, and the accurate identification of unqualified aluminum-plastic films and cell quality is achieved. guarantee.

CN118937922APending Publication Date: 2024-11-12WANXIANG 123 CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411013708.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art cannot accurately identify the problem of poor insulation after the aluminum-plastic film is punched due to poor equipment, parameters or raw materials, resulting in greater risk of loss in battery cells during use.

Method used

By measuring the leakage current relationship between different conductive dielectrics and aluminum-plastic films at fixed voltages, the standard leakage current numerical range is determined, and the insulation voltage withstand test is carried out in combination with the depth of the pit and the ductile rate to identify the insulation performance of aluminum-plastic films after the pit.

Benefits of technology

It can accurately identify polypropylene damage and poor insulation aluminum-plastic films caused by poor equipment, parameters or raw materials, and avoid unqualified battery cell assembly and liquid leakage risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937922A_ABST
    Figure CN118937922A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum-plastic film insulating layer pit punching quality detection method, which comprises the following steps of: (1) measuring the relationship between different conducting media and leakage current to determine a proper conducting medium; (2) measuring leakage current values of the aluminum plastic film under different elongation rates by using the selected conducting medium, and taking the leakage current values as a standard leakage current value range of the aluminum plastic film under the corresponding elongation rate; (3) carrying out a gradient experiment of the punching pit depth on the aluminum plastic film, and determining the elongation rates of the aluminum plastic film with different punching pit depths; and (4) determining a leakage current qualified range of an insulation and voltage resistance test of the punched aluminum plastic film according to the elongation percentage, performing an insulation test on the punched aluminum plastic film through the conductive medium and the voltage used in the step (2), and if the leakage current is within the qualified range, determining that the punched aluminum plastic film is a qualified product. According to the method, the insulation performance of the aluminum plastic film after pit punching is judged by comparing the magnitude of the leakage current, the aluminum plastic film with polypropylene damage can be identified, and the aluminum plastic film with poor insulation performance caused by other problems can be accurately identified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery detection, in particular to a method for detecting the quality of punching holes in an aluminum-plastic film insulation layer. Background Art

[0002] In the existing soft-pack battery production process, the positive and negative electrodes are stacked and welded to form a bare cell, and then the aluminum-plastic film is punched and stretched to form a shell, and then the bare cell is placed in the shell and packaged. The aluminum-plastic film is a three-layer structure. The outer layer is a nylon layer, which has heat resistance, wear resistance and bending resistance; the middle aluminum layer is a barrier layer, which has the function of blocking moisture from entering the battery cell and providing punching plasticity; the inner layer is a polypropylene layer, which is a stable composite layer and heat-sealing layer. It has good chemical stability and prevents the formation of ion paths between the battery cell and the aluminum-plastic film. During the punching process of the aluminum-plastic film, the inner layer may be damaged, or the inner layer may not be damaged in the short term due to poor processing technology or raw materials, but there is a risk of damage in the later stage.

[0003] Patent document CN113391222A discloses a method for analyzing poor insulation of aluminum-plastic film of soft-pack batteries. The method determines the location of poor insulation through solution corrosion. However, the method has the disadvantage that it can only identify aluminum-plastic film with damaged polypropylene insulation layer, but cannot identify aluminum-plastic film with quality problems after punching but without damaged insulation layer, thus causing greater losses to the assembled battery cells in later use. Summary of the invention

[0004] The purpose of the present invention is to provide an aluminum-plastic film which can not only identify the damage of polypropylene after punching, but also accurately identify the aluminum-plastic film with poor insulation after punching due to reasons such as bad equipment, parameters or raw materials.

[0005] A method for detecting the quality of a crater in an aluminum-plastic film insulation layer comprises the following steps:

[0006] (1) Under a fixed voltage and a fixed elongation rate of the aluminum-plastic film, measure the relationship between different conductive media and leakage current to determine the appropriate conductive medium;

[0007] (2) using the selected conductive medium, under a fixed voltage and within a fixed time, measuring the leakage current values ​​of the aluminum-plastic film at different elongation rates, as the standard leakage current value range of the aluminum-plastic film at the corresponding elongation rate;

[0008] (3) Conducting a gradient experiment of the pit depth on the aluminum-plastic film to determine the elongation rate of the aluminum-plastic film at different pit depths;

[0009] (4) According to the elongation of the aluminum-plastic film corresponding to the known pit depth and the leakage current value of the aluminum-plastic film at different elongations, the qualified range of the leakage current value of the insulation withstand voltage test of the aluminum-plastic film after the pit is determined, and the insulation withstand voltage test is performed on the aluminum-plastic film after the pit is performed using the conductive medium and voltage used in step (2). If the leakage current is within the qualified range, it is a qualified product.

[0010] The elongation rate is the percentage of the change in thickness of the aluminum-plastic film after stretching divided by the thickness before stretching.

[0011] Furthermore, in step (1), the fixed voltage ranges from 100-5000V, preferably 1000-3000V.

[0012] Furthermore, in step (1), the conductive medium is selected from an aqueous solution of NaCl, an aqueous solution of KCl, and a polymer ion solution.

[0013] These conductive media are in close contact with the polypropylene layer of the aluminum-plastic film and have good penetration and wetting capabilities, which can accurately identify the locations where insulation defects exist in the polypropylene layer, and ultimately express them through leakage current signals.

[0014] Furthermore, in step (1), the conductive medium is selected from one of 1 mol / L NaCl aqueous solution, 3 mol / L NaCl aqueous solution, and 1 mol / L KCl aqueous solution.

[0015] Furthermore, in the step (1), the fixed elongation of the aluminum-plastic film is in the range of 30-60%.

[0016] Furthermore, in the step (1), the fixed elongation of the aluminum-plastic film is 50%.

[0017] The elongation rate of the aluminum-plastic film punching pit is generally not more than 50%. When selecting a suitable conductive medium, the elongation rate of the aluminum-plastic film punching pit is set to 50%, which is convenient for selecting a conductive medium with higher sensitivity.

[0018] Furthermore, in the step (2), different fixed voltages are used respectively, through the selected conductive medium, to measure the leakage current values ​​of the aluminum-plastic film at different elongation rates within a fixed time.

[0019] Using different fixed voltages to measure the leakage current values ​​at different elongation rates of aluminum-plastic film has two functions. First, confirm the relationship curve between leakage current and elongation rate of aluminum-plastic film to ensure that the experimental data will not be biased or discrete. On the other hand, voltage will affect the leakage current. If the leakage current deviation is too small, it is difficult to make a judgment and easy to misjudge. Using different fixed voltages to measure different groups of leakage current values, the corresponding leakage current value group under the appropriate voltage can be selected as the qualified value range according to the leakage current deviation obtained.

[0020] Furthermore, in step (2), the different fixed voltage values ​​range from 1000 to 5000V.

[0021] Furthermore, in step (2), the fixed time is 10 seconds.

[0022] The leakage current is a cumulative value. The leakage current value is small when the time is short, and the leakage current value is large when the time is long. By fixing the measurement time at 10 seconds, an accurate leakage current value can be obtained.

[0023] Furthermore, in step (3), experiments with different crater depths are performed on the aluminum-plastic film to determine the relationship between the crater depth of the aluminum-plastic film and the thickness of the aluminum layer, and the ductility of the aluminum layer at different crater depths is calculated, and the ductility value of the aluminum-plastic film is equal to the ductility value of the aluminum layer.

[0024] The relationship between the punching depth and the thickness change of the aluminum-plastic film. Under the microscope, the polypropylene layer and the nylon layer are transparent, and it is difficult to measure the thickness. Since the aluminum layer is a part of the aluminum-plastic film, the deformation amount during punching is basically the same. Therefore, based on the elongation value of the aluminum layer as a reference, the elongation value of the aluminum-plastic film is equal to the elongation value of the aluminum layer.

[0025] The present invention measures standard leakage current values ​​of the aluminum-plastic film at different elongations, determines the elongations corresponding to the aluminum-plastic films with different dent depths, measures the leakage current of the aluminum-plastic film after denting, and compares it with the standard leakage current value of the aluminum-plastic film obtained at the corresponding elongation, thereby judging the insulation performance of the aluminum-plastic film after denting. The present invention can not only identify the aluminum-plastic film with damaged polypropylene, but also accurately identify the aluminum-plastic film with poor insulation due to poor equipment, parameters or raw materials, so as to prevent the unqualified aluminum-plastic film with dents from flowing out, and effectively avoid the risk of leakage when assembled into battery cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of aluminum-plastic film leakage current detection used in the embodiment of the present invention;

[0027] Figure 2 This is a result diagram of the change of leakage current of the aluminum-plastic film obtained in the embodiment of the present invention in different conductive media over time;

[0028] Figure 3 1 is a graph showing the numerical results of leakage current of aluminum-plastic films with different elongation rates at different voltages obtained in the embodiments of the present invention;

[0029] Figure 4 It is a schematic diagram of the positions of four points selected for studying the thickness change of the aluminum-plastic film after punching holes in the embodiment of the present invention;

[0030] Figure 5 is a graph showing the relationship between the thickness and position of the aluminum layer (Al) at different pit depths in an embodiment of the present invention;

[0031] Figure 6 It is a schematic diagram of the ductility of the aluminum layer (Al) at different pit depths in the embodiment of the present invention. DETAILED DESCRIPTION

[0032] In order to make the technical solution of the present invention clearer, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0033] The total thickness of the aluminum-plastic film detected by the invention is 70-200 μm, the thickness of the outer nylon layer is 10-40 μm, the thickness of the middle aluminum layer is 30-40 μm, and the thickness of the inner polypropylene layer is 30-80 μm.

[0034] Example

[0035] The aluminum layer thickness of the aluminum-plastic film tested in this test is 40 μm, the polypropylene layer thickness is 80 μm, the nylon layer thickness is 36 μm, and the aluminum-plastic film thickness is 156 μm.

[0036] The first step is the selection of conductive media: Figure 1 As shown, an insulation withstand voltage tester was used. At a voltage of 1000V, when the elongation of the aluminum-plastic film was 50%, 1mol / L NaCl aqueous solution, 3mol / L NaCl aqueous solution, and 1mol / L KCl aqueous solution were used as conductive media to test the intensity of the leakage current. The leakage current at different time points of different conductive media was recorded. The results are shown in Table 1.

[0037] Table 1 Leakage current data of different conductive media at different time points

[0038] Time(S) / μA 1 mol / L NaCl aqueous solution 3mol / LNaCl aqueous solution 1 mol / L KCl aqueous solution 10 0.9 2.8 0.8 30 2.2 6.8 1.9 60 6.6 20.4 5.8

[0039] Plot the data in Table 1 into a graph, such as Figure 2 As shown, in the 3 mol / L NaCl aqueous solution, the leakage current changes greatly with time and has a higher sensitivity, so the 3 mol / L NaCl aqueous solution is selected as the conductive medium.

[0040] In the second step, the aluminum-plastic film is stretched to obtain elongation of 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, and 100%. The aluminum-plastic film with different elongation is placed in a 3 mol / L NaCl aqueous solution as a conductive medium, at a fixed voltage of 1000V and 3000V, for a fixed time of 10 seconds, and the leakage current values ​​of the aluminum-plastic film with different elongation are recorded, and the recorded results are plotted into a graph.

[0041] like Figure 3 As shown in the figure, the leakage current growth relationship under the voltage of 1000V and 3000V is similar, which can determine the validity of the measured leakage current value. At the same time, the leakage current values ​​of aluminum-plastic films with different elongation rates at 3000V are relatively large. In order to ensure the detection rate of defective products and reduce misjudgment, the voltage of 3000V is selected as the test voltage, and the leakage current of aluminum-plastic films with different elongation rates obtained at the voltage of 3000V is used as the standard leakage current value range.

[0042] The third step is to conduct a gradient experiment on the depth of the punching pits on the aluminum-plastic film. The depths of the punching pits are 6mm, 6.5mm, 7mm, 8mm, and 8.5mm respectively. The punching depth can be flexibly changed according to the needs of battery cell production. Under a microscope, the polypropylene layer and the nylon layer are both transparent, and it is difficult to judge the thickness. Therefore, the thickness of the aluminum layer is used to calculate the elongation. Since the deformation of the aluminum-plastic film and the aluminum layer is basically the same when punching the pits, the elongation value of the aluminum-plastic film is equal to the elongation value of the aluminum layer. Figure 4 As shown, four points at different positions after punching are selected, and the thickness of the aluminum layer is measured by microscope. The thickness of the aluminum layer at each position point with different punching depths is recorded. The results are shown in Figure 5 The minimum thickness of the aluminum layer at the four locations is taken to calculate the elongation of the aluminum layer. Elongation = (40-minimum thickness of the aluminum layer) / 40. The results are as follows: Figure 6 As shown in the figure, the elongation of the aluminum-plastic film ranges from 30% to 40% with different pit depths.

[0043] Step 4: Different pit depths, the elongation of the aluminum-plastic film ranges from 30% to 40%. Figure 3 As shown in Table 2, under the condition of 3000V voltage and 3mol / L NaCl aqueous solution as the conductive medium, the leakage current of the aluminum-plastic film does not exceed 5mA within 10 seconds. Under this measurement condition, the leakage current value of the aluminum-plastic film after denting is measured. Within 10 seconds, the aluminum-plastic film with a leakage current less than 5mA after denting is qualified. The test results are shown in Table 2.

[0044] Table 2 Test results

[0045] Punch depth / mm Applied voltage / V NG time / S NG current / mA Quality inspection results 0.0 3000 10 0 qualified 6.0 3000 10 1.1 qualified 6.5 3000 10 3.7 qualified 7.0 3000 9 5.2 Failure 7.5 3000 9 13.5 Failure 8.0 3000 5 18.7 Failure 8.5 3000 3 33.9 Failure

[0046] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for detecting the quality of punching holes in an aluminum-plastic film insulation layer, characterized in that: The following steps are involved: (1) Under a fixed voltage and a fixed elongation rate of the aluminum-plastic film, measure the relationship between different conductive media and leakage current to determine the appropriate conductive medium; (2) using the selected conductive medium, under a fixed voltage and within a fixed time, measuring the leakage current values ​​of the aluminum-plastic film at different elongation rates, as the standard leakage current value range of the aluminum-plastic film at the corresponding elongation rate; (3) Conducting a gradient experiment of the pit depth on the aluminum-plastic film to determine the elongation rate of the aluminum-plastic film at different pit depths; (4) According to the elongation of the aluminum-plastic film corresponding to the known pit depth and the leakage current value of the aluminum-plastic film at different elongations, the qualified range of the leakage current value of the insulation withstand voltage test of the aluminum-plastic film after the pit is determined, and the insulation withstand voltage test is performed on the aluminum-plastic film after the pit is performed using the conductive medium and voltage used in step (2). If the leakage current is within the qualified range, it is a qualified product.

2. A method for detecting the quality of aluminum-plastic film insulation layer pitting according to claim 1, characterized in that: In the step (1), the fixed voltage ranges from 100 to 5000V.

3. A method for detecting the quality of aluminum-plastic film insulation layer punching according to claim 2, characterized in that: In the step (1), the conductive medium is selected from a NaCl aqueous solution, a KCl aqueous solution, and a polymer ion solution.

4. A method for detecting the quality of punching holes in an aluminum-plastic film insulation layer according to claim 3, characterized in that: In the step (1), the conductive medium is selected from one of a 1 mol / L NaCl aqueous solution, a 3 mol / L NaCl aqueous solution, and a 1 mol / L KCl aqueous solution.

5. A method for detecting the quality of punching holes in an aluminum-plastic film insulation layer according to claim 4, characterized in that: In the step (1), the fixed elongation of the aluminum-plastic film is in the range of 30-60%.

6. A method for detecting the quality of punching holes in an aluminum-plastic film insulation layer according to claim 5, characterized in that: In the step (1), the fixed elongation of the aluminum-plastic film is 50%.

7. A method for detecting the quality of punching holes in an aluminum-plastic film insulation layer according to claim 1, characterized in that: In the step (2), different fixed voltages are used respectively, through a selected conductive medium, to measure the leakage current values ​​of the aluminum-plastic film at different elongation rates within a fixed time.

8. A method for detecting the quality of punching holes in an aluminum-plastic film insulation layer according to claim 7, characterized in that: In the step (2), the different fixed voltage values ​​range from 1000 to 5000V.

9. A method for detecting the quality of punching holes in an aluminum-plastic film insulation layer according to claim 8, characterized in that: In the step (2), the fixed time is 10 seconds.

10. A method for detecting the quality of punching holes in an aluminum-plastic film insulation layer according to claim 3, characterized in that: In the step (3), the aluminum-plastic film is subjected to experiments with different crater depths to determine the relationship between the crater depth of the aluminum-plastic film and the thickness of the aluminum layer, and the ductility of the aluminum layer at different crater depths is calculated, and the ductility value of the aluminum-plastic film is equal to the ductility value of the aluminum layer.