Method for manufacturing circularly polarizing plate

By optimizing the manufacturing method of circular polarizers, especially by processing the through-hole area in the winding and peeling off the protective film, the problem of poor appearance of hole marks caused by tight winding was solved, and higher quality circular polarizers were produced.

CN118938373APending Publication Date: 2024-11-12NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410573640.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the manufacturing of circular polarizers, existing technologies often suffer from poor appearance due to through-hole marks (hole marks) caused by tight winding.

Method used

A method for manufacturing a circular polarizer includes processes Sa, Sb, Sc, and optional Se. The specific steps are as follows: preparing a winding of a first protective film, a first polarizer protective layer, a polarizer, and a second protective film stacked sequentially; extracting and processing the through-hole portion of the polarizer to decolorize and form a non-polarized portion; peeling off the first and second protective films; and superimposing a phase difference layer on one side of the polarizer protective layer. The thickness and hardness of the protective film are optimized to reduce hole marks.

Benefits of technology

It effectively suppresses appearance defects caused by through-hole marks, and improves the productivity and quality of circular polarizers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118938373A_ABST
    Figure CN118938373A_ABST
Patent Text Reader

Abstract

Provided is a method for producing a circularly polarizing plate capable of suppressing the occurrence of appearance defects caused by hole traces. The manufacturing method includes a step Sa, a step Sb, a step Sc, and a step Sd. In step Sa, a wound material of a polarizing film laminate (10) is prepared, said wound material being provided with a first protective film (11), a first polarizer protective layer (12), a polarizer (13), and a second protective film (14) having a through-hole (14a) in this order. In the step Sb, while the polarizing film laminate (10) is drawn out from the wound material, the portion exposed from the through-hole (14a) in the polarizer (13) is brought into contact with the processing liquid, thereby decolorizing and forming the non-polarizing portion. In the step Sc, the first protective film (11) and the second protective film (14) are peeled off from the polarizing film laminate (10). In step Sd, a phase difference layer is laminated on the side of the first polarizer protective layer (12) opposite to the polarizer (13) side.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing a circular polarizing plate. Background Art

[0002] In image display devices such as organic EL display devices and liquid crystal display devices, components including optical anisotropic films such as polarizing films and phase difference films are used. In particular, in organic EL display devices, visual recognition is easily reduced due to external light reflection caused by metal electrodes. Therefore, in order to prevent the external light reflection, a circular polarizer composed of a polarizing film and a phase difference film is used.

[0003] In order to cope with the diversification of the shapes and the improvement of the functions of image display devices, a polarizing plate having a partial polarization function is required. As such a polarizing plate, a polarizing plate having a polarizer having a non-polarizing portion formed by chemical treatment is known.

[0004] Patent Document 1 proposes a method for manufacturing a polarizer having a non-polarizing portion as follows: after laminating a surface protective layer having a plurality of through holes with a polarizer, a polarizing film laminate including the polarizer and the surface protective layer is rolled into a roll, and then the exposed portion of the polarizer (the portion exposed from the through holes of the surface protective layer) is bleached to form a non-polarizing portion. Hereinafter, the rolled product of the polarizing film laminate is sometimes described as a "polarizing film laminate roll".

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2016-53645 Summary of the invention

[0008] Problems to be solved by the invention

[0009] When a laminate including a surface protection layer having a plurality of through holes is rolled up, dents (hole marks caused by the through holes in the surface protection layer) may sometimes be generated in the laminate due to the tight rolling. In the technology described in Patent Document 1, there is still room for improvement in suppressing the occurrence of poor appearance caused by hole marks in the roll of the polarizing film laminate.

[0010] In view of the above problems, an object of the present invention is to provide a method for producing a circularly polarizing plate capable of suppressing the occurrence of appearance defects due to hole marks.

[0011] Means used to solve problems

[0012] <Aspects of the Invention>

[0013] The present invention includes the following aspects.

[0014] [1] A method for manufacturing a circular polarizer, comprising:

[0015] Step Sa of preparing a roll of a polarizing film laminate that sequentially includes a first protective film, a first polarizer protective layer, a polarizer, and a second protective film having a through hole;

[0016] Step Sb, wherein the polarizing film laminate is unwound from the roll while contacting the exposed portion of the through hole in the polarizer with a treatment liquid to thereby decolorize and form a non-polarizing portion;

[0017] Step Sc, which is to peel off the first protective film and the second protective film from the polarizing film laminate; and

[0018] Step Sd of laminating a phase difference layer on the side of the first polarizer protective layer opposite to the polarizer side.

[0019] [2] The method for producing a circularly polarizing plate according to [1], further comprising, after the step Sc, a step Se of laminating a second polarizer protective layer on the surface of the polarizer from which the second protective film has been peeled off.

[0020] [3] The method for producing a circular polarizing plate according to [1] or [2] above, wherein the thickness of the first protective film is 50 μm or less.

[0021] [4] The method for producing a circular polarizer according to any one of [1] to [3] above, wherein in the step Sc, the thickness of the polarizing film laminate after the first protective film and the second protective film are peeled off is 50 μm or less.

[0022] [5] The method for producing a circularly polarizing plate according to any one of [1] to [4], wherein the first polarizer protective layer and the polarizer are bonded to each other with an adhesive.

[0023] [6] The method for producing a circularly polarizing plate according to any one of [1] to [5], wherein the pencil hardness of the surface of the first polarizer protective layer on the first protective film side is 4B or more.

[0024] [7] The method for producing a circular polarizing plate according to any one of [1] to [6] above, wherein the second protective film has a thickness of 20 μm to 150 μm.

[0025] [8] The method for producing a circular polarizing plate according to any one of [1] to [7] above, wherein the diameter of the opening of the through hole is 1 mm to 10 mm.

[0026] Effects of the Invention

[0027] According to the present invention, it is possible to provide a method for producing a circularly polarizing plate capable of suppressing the occurrence of appearance defects due to hole marks. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a perspective view showing an example of a polarizing film laminate roll.

[0029] Figure 2 This is a partial cross-sectional view showing an example of a laminated state of a surface layer portion of a polarizing film laminate roll.

[0030] Figure 3 This is a process diagram showing an example of a process of forming a non-polarizing portion.

[0031] Figure 4 This is a partial cross-sectional view showing an example of a polarizing film laminate after the non-polarizing portion is formed.

[0032] Figure 5 This is a partial cross-sectional view showing an example of a polarizing film laminate after the first protective film and the second protective film are peeled off.

[0033] Figure 6 This is a partial cross-sectional view showing an example of a polarizing film laminate after laminating the second polarizer protective layer.

[0034] Figure 7 This is a partial cross-sectional view showing an example of a circularly polarizing plate obtained by the production method of the present invention.

[0035] Explanation of symbols

[0036] 10: Polarizing film laminate

[0037] 11: The first protective film

[0038] 12: First polarizer protective layer

[0039] 13: Polarizer

[0040] 13a: Non-polarized part

[0041] 14: Second protective film

[0042] 14a: Through hole

[0043] 21: Treatment fluid

[0044] 42: Second polarizer protective layer

[0045] 52: First phase difference layer (phase difference layer)

[0046] 54: Second phase difference layer (phase difference layer)

[0047] 200: Circular polarizer DETAILED DESCRIPTION

[0048] Hereinafter, preferred embodiments of the present invention will be described. In addition, in this specification, all academic documents and patent documents described in this specification are cited as references.

[0049] First, the terms used in this specification are explained. "C plate" refers to a phase difference film (phase difference layer) having anisotropy of refractive index in the thickness direction. In addition, among C plates, a phase difference film (phase difference layer) that shows a negative value of delay in the thickness direction is called a "positive C plate", and a phase difference film (phase difference layer) that shows a positive value of delay in the thickness direction is called a "negative C plate".

[0050] The value of pencil hardness is a value measured under a load of 500 g based on the provisions of JIS K 5600-5-4. If there is no provision, the value of the "thickness" of the layered material (more specifically, the first protective film, the first polarizer protective layer, the polarizer, the second protective film, the phase difference layer, the second polarizer protective layer, etc.) is the arithmetic mean of 10 measured values ​​obtained by observing a cross section of the layered material cut in the thickness direction with an electron microscope, randomly selecting 10 measurement locations from the cross-sectional image, and measuring the thickness of the selected 10 measurement locations.

[0051] In the following, "system" is sometimes added after the compound name to collectively refer to the compound and its derivatives. In addition, if there is no provision, when "system" is added after the compound name to indicate the polymer name, it means that the repeating unit of the polymer is derived from the compound or its derivative. In addition, acrylic acid and methacrylic acid are sometimes collectively referred to as "(meth)acrylic acid". Unless otherwise specified, the components, functional groups, etc. exemplified in this specification can be used alone or in combination of two or more.

[0052] For ease of understanding, in the drawings referred to in the following description, each component is schematically shown as the main body, and the size, number, shape, etc. of each component shown in the drawings may be different from the actual one for the convenience of drawing preparation. In addition, for the convenience of description, in the drawings described later, the same components as those in the drawings described previously are sometimes marked with the same symbols, and their descriptions are omitted.

[0053] <Method for producing circular polarizing plate>

[0054] The manufacturing method of the circular polarizer of the present embodiment comprises steps Sa, Sb, Sc and Sd. In step Sa, a roll (polarizing film laminate roll) of a polarizing film laminate having a first protective film, a first polarizer protective layer, a polarizer, and a second protective film having a through hole is prepared in sequence. In step Sb, while the polarizing film laminate is pulled out from the polarizing film laminate roll, the portion exposed from the through hole in the polarizer is brought into contact with a treatment liquid, thereby bleaching and forming a non-polarized portion. In step Sc, the first protective film and the second protective film are peeled off from the polarizing film laminate. In step Sd, a phase difference layer is laminated on the side of the first polarizer protective layer opposite to the polarizer side.

[0055] In addition, the method for manufacturing a circular polarizer of the present embodiment may further include steps (other steps) other than step Sa, step Sb, step Sc, and step Sd. As other steps, for example, step Se of laminating a second polarizer protective layer on the surface of the polarizer after peeling off the second protective film can be cited after step Sc.

[0056] Hereinafter, step Sa is sometimes described as a “winding preparation step”. In addition, step Sb is sometimes described as a “non-polarizing portion forming step”. In addition, step Sc is sometimes described as a “protective film peeling step”. In addition, step Sd is sometimes described as a “phase difference layer lamination step”. In addition, step Se is sometimes described as a “second polarizer protective layer lamination step”.

[0057] Below, with appropriate reference to the attached Figure 1 Each step included in an example of a method for producing a circular polarizing plate according to the present embodiment will be described.

[0058] [Wound material preparation process]

[0059] Regarding the winding material preparation process, refer to Figure 1 and Figure 2 While explaining. Figure 1 It is a perspective view showing an example of a polarizing film laminate roll. Figure 2 This is a partial cross-sectional view showing an example of a laminated state of a surface layer portion of a polarizing film laminate roll.

[0060] The roll preparation step is a step of preparing a polarizing film laminate roll. First, the polarizing film laminate roll will be described. Figure 1 The polarizing film stack roll 100 shown is a wound product of the polarizing film stack 10. Figure 2As shown, the polarizing film laminate 10 sequentially comprises a first protective film 11, a first polarizer protective layer 12, a polarizer 13, and a second protective film 14 having a through hole 14a. An adhesive layer 15 is present between the first polarizer protective layer 12 and the polarizer 13. In other words, the first polarizer protective layer 12 and the polarizer 13 are bonded by an adhesive. If the first polarizer protective layer 12 and the polarizer 13 are bonded by an adhesive, the adhesion between the first polarizer protective layer 12 and the polarizer 13 is improved, and therefore, the polarizer 13 can be protected more reliably. In addition, in the present embodiment, the first polarizer protective layer 12 and the polarizer 13 are bonded by an adhesive, but the present invention is not limited thereto, and the first polarizer protective layer 12 and the polarizer 13 can also be bonded by an adhesive.

[0061] like Figure 2 As shown, the second protective film 14 is in contact with the polarizer 13, and a portion of the polarizer 13 is exposed from the through hole 14a of the second protective film 14. In addition, the first protective film 11 is peelably bonded to the first polarizer protective layer 12. Similarly, the second protective film 14 is also peelably bonded to the polarizer 13.

[0062] The dimension of the polarizing film laminate 10 in the width direction is, for example, 500 mm to 2000 mm, or preferably 1000 mm to 1500 mm. The length of the polarizing film laminate 10 is, for example, 50 m to 6000 m, or preferably 150 m to 4000 m.

[0063] exist Figure 1 In the example shown, a plurality of through holes 14a are provided in a predetermined pattern. The arrangement pattern of the through holes 14a can be appropriately set according to the purpose. The top view shape of the through holes 14a can be determined by adjusting the non-polarizing portion 13a (see Figure 4 ) The desired shape can be appropriately changed. The top view shape of the through hole 14a includes, for example, a circle, an ellipse, a rectangle, etc., preferably a circle. Figure 1 In the example shown, the polarizing film stack 10 is wound so that the through hole 14 a is arranged on the inner side, but the present invention is not limited to this, and the polarizing film stack 10 may be wound so that the through hole 14 a is arranged on the outer side.

[0064] The diameter of the opening of the through hole 14a can be determined by the non-polarizing portion 13a (see Figure 4 The diameter of the opening of the through hole 14a is, for example, 0.5 mm to 20 mm, preferably 1 mm to 10 mm.

[0065] exist Figure 2In the example shown, the opening edge of the through hole 14a on the second protective film 14 of the polarizing film stack 10 provided at the outermost circumference (first circumference) is in contact with the first protective film 11 of the polarizing film stack 10 located just below the outermost circumference (second circumference). Hereinafter, the through hole provided on the second protective film of the polarizing film stack of the first circumference is sometimes described as "the through hole of the first circumference". In addition, the through hole provided on the second protective film of the polarizing film stack of the nth circumference (n is an integer greater than 2) is sometimes described as "the through hole of the nth circumference".

[0066] In the state where the polarizing film laminate 10 is wound, there is a tendency for excessive pressure to be applied below (inwardly) the opening edge of the through hole 14a. Figure 2 In the example shown, there is a tendency that excessive pressure is applied to the X portion of the first polarizer protective layer 12 of the second polarizing film laminate 10 through the first protective film 11 below the opening edge of the through hole 14a of the first cycle. As a result, the hole mark 12b described later is easily generated on the first polarizer protective layer 12 of the second polarizing film laminate 10 (see Figure 5 ). Similarly, there is a tendency to apply excessive pressure to the X portion of the first polarizer protective layer 12 of the polarizing film stack 10 of the n+1th week through the first protective film 11 below the opening edge of the through hole 14a of the nth week. As a result, it is easy to produce a hole mark 12b on the first polarizer protective layer 12 of the polarizing film stack 10 of the n+1th week. In particular, when the diameter of the opening of the through hole 14a is 1mm to 10mm, there is a tendency to produce a hole mark 12b on the first polarizer protective layer 12 of the polarizing film stack 10 after the second week.

[0067] The winding preparation process may be a process of preparing a commercially available polarizing film laminate roll 100, or may include a process of winding up the obtained polarizing film laminate 10 after forming the polarizing film laminate 10. The method for forming the polarizing film laminate 10 is not particularly limited, and for example, a known method described in Japanese Patent Publication No. 2016-53645, Japanese Patent Publication No. 2022-182000, etc. may be used. In the process of winding up the polarizing film laminate 10, a winding device (not shown) is used to wind up the polarizing film laminate 10 with a winding tension of, for example, 130N / 1000mm width or more to obtain a polarizing film laminate roll 100. By winding up with a winding tension of 130N / 1000mm width or more, the occurrence of winding deviation of the polarizing film laminate 10 can be suppressed. In addition, when the polarizing film laminate 10 is wound up with a winding tension of 130 N / 1000 mm width or more, hole marks 12b are easily generated on the first polarizer protective layer 12 of the polarizing film laminate 10 after the second turn (see Figure 5). In order to suppress damage to the polarizing film laminate 10 caused by tight winding, the polarizing film laminate 10 is preferably wound up at a winding tension of 250 N / 1000 mm width or less.

[0068] Next, each layer included in the polarizing film laminate 10 will be described in detail.

[0069] (First Protective Film 11)

[0070] The first protective film 11 is, for example, a laminate of a substrate (not shown) and an adhesive layer (not shown). Figure 2 In the example shown, the first protective film 11 and the first polarizer protective layer 12 are bonded together via the adhesive layer of the first protective film 11 .

[0071] The substrate of the first protective film 11 is formed by any appropriate film. As the constituent material of the film, non-permeable materials can be cited, specifically, polyester resins such as polyethylene terephthalate resins, polycycloolefin resins such as polynorbornene resins, polyolefin resins such as polypropylene, polyamide resins, polycarbonate resins, and their copolymer resins. In addition, in this specification, "non-permeable material" refers to a material that is not easily penetrated by the processing liquid used in the non-polarizing portion formation process described later. In order to increase the hardness of the substrate of the first protective film 11, the constituent material of the substrate is preferably a polyester resin. The thickness of the substrate of the first protective film 11 is, for example, 10μm to 200μm, preferably 20μm to 150μm.

[0072] The adhesive layer of the first protective film 11 is formed of any appropriate adhesive (pressure-sensitive adhesive). Examples of the adhesive include (meth) acrylic adhesives, urethane adhesives, silicone adhesives, etc. The thickness of the adhesive layer of the first protective film 11 is, for example, 1 μm to 20 μm, preferably 2 μm to 10 μm.

[0073] In order to increase the productivity of the circular polarizer by increasing the number of windings of the polarizing film laminate 10, the thickness of the first protective film 11 (for example, the total thickness of the substrate and the adhesive layer) is preferably 50 μm or less, and more preferably 40 μm or less. In addition, in order to suppress damage to the first polarizer protective layer 12, the thickness of the first protective film 11 (for example, the total thickness of the substrate and the adhesive layer) is preferably 10 μm or more, and more preferably 20 μm or more. In addition, when the thickness of the first protective film 11 is 50 μm or less, the hole marks 12b described later are easily generated (see Figure 5 ).

[0074] (Second Protective Film 14)

[0075] The second protective film 14 is, for example, a laminate of a substrate (not shown) and an adhesive layer (not shown). Figure 2 In the illustrated example, the second protective film 14 and the polarizer 13 are bonded together via the adhesive layer of the second protective film 14 .

[0076] As the constituent material of the substrate of the second protective film 14, for example, the materials listed as the constituent materials of the substrate of the first protective film 11 mentioned above can be cited. The preferred range of the thickness of the substrate of the second protective film 14 is also the same as the preferred range of the thickness of the substrate of the first protective film 11 mentioned above. The constituent material of the substrate of the first protective film 11 and the constituent material of the substrate of the second protective film 14 may be the same or different. In addition, the thickness of the substrate of the first protective film 11 and the thickness of the substrate of the second protective film 14 may be the same or different.

[0077] As the adhesive constituting the adhesive layer of the second protective film 14, for example, the adhesive listed as the adhesive constituting the adhesive layer of the above-mentioned first protective film 11 can be cited. The preferred range of the thickness of the adhesive layer of the second protective film 14 is also the same as the preferred range of the thickness of the adhesive layer of the above-mentioned first protective film 11. The adhesive constituting the adhesive layer of the first protective film 11 and the adhesive constituting the adhesive layer of the second protective film 14 may be the same or different. In addition, the thickness of the adhesive layer of the first protective film 11 and the thickness of the adhesive layer of the second protective film 14 may be the same or different.

[0078] Furthermore, through holes 14a are formed in the second protective film 14. The method for forming the through holes 14a is not particularly limited, and examples thereof include mechanical processing, laser processing, and etching processing by chemical reaction.

[0079] By increasing the number of windings of the polarizing film laminate 10, the productivity of the circular polarizer is improved, and the non-polarizing portion 13a (see FIG. 14 ) is formed in an appropriate size in the non-polarizing portion forming step described later. Figure 4 ), the thickness of the second protective film 14 (for example, the total thickness of the substrate and the adhesive layer) is preferably 20 μm to 150 μm, more preferably 25 μm to 150 μm, and further preferably 30 μm to 150 μm.

[0080] (Polarizer 13)

[0081] The polarizer 13 includes, for example, a resin film, preferably a polyvinyl alcohol-based resin film containing a dichroic substance. Hereinafter, the polyvinyl alcohol-based resin may be referred to as a "PVA-based resin." The polarizer 13 may be a single-layer resin film or a laminate of two or more layers.

[0082] As dichroic substances, for example, iodine, organic dyes, etc. can be cited. Dichroic substances can be used alone or in combination. As a preferred dichroic substance, iodine can be cited. If iodine is used as the dichroic substance, in the non-polarizing portion forming step described later, the portion exposed from the through hole 14a in the polarizer 13 is brought into contact with the treatment liquid, thereby appropriately reducing the iodine complex contained in the polarizer 13. In this way, the formed non-polarizing portion 13a (see Figure 4 ) to impart appropriate properties (light transmittance, etc.).

[0083] In the case where the polarizer 13 is composed of a single-layer resin film, as a specific example of the polarizer 13, a polarizer obtained by subjecting a PVA-based resin film to a dyeing treatment and a stretching treatment (representatively uniaxial stretching) using iodine can be cited. The above-mentioned dyeing using iodine is formed, for example, by immersing the PVA-based resin film in an iodine aqueous solution. The stretching ratio of the above-mentioned uniaxial stretching is preferably 3 to 7 times. Stretching can be performed after the dyeing treatment, or it can be performed while dyeing. In addition, dyeing can be performed after stretching. As needed, the PVA-based resin film is subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc. For example, by immersing the PVA-based resin film in water for washing before dyeing, the contamination and anti-blocking agent on the surface of the PVA-based resin film can be removed, and the PVA-based resin film is swelled to prevent uneven dyeing.

[0084] When the polarizer 13 is a laminate of two or more layers, a laminate of a resin substrate and a PVA resin layer (PVA resin film) laminated on the resin substrate can be cited as a specific example of the polarizer 13. When the polarizer 13 is a laminate of a resin substrate and a PVA resin layer laminated on the resin substrate, the PVA resin layer is arranged on the second protective film 14 side.

[0085] The polarizer 13 formed by a laminate of two or more layers can be made, for example, through the following steps: a step of applying a PVA-based resin solution to a resin substrate, drying it, forming a PVA-based resin layer on the resin substrate, and obtaining a laminate of the resin substrate and the PVA-based resin layer; and a step of stretching and dyeing the laminate. When stretching, for example, the laminate is immersed in an aqueous boric acid solution for stretching. The obtained laminate of the resin substrate / PVA-based resin layer can be used directly, or the resin substrate can be peeled off from the laminate of the resin substrate / PVA-based resin layer, and any appropriate protective layer corresponding to the purpose can be stacked on the peeled surface for use. The details of the method for manufacturing such a polarizer are recorded in, for example, Japanese Patent Gazette No. 2012-73580 and Japanese Patent No. 6470455.

[0086] The thickness of the polarizer 13 is preferably 15 μm or less, more preferably 12 μm or less, further preferably 10 μm or less, and particularly preferably 8 μm or less. The thickness of the polarizer 13 is, for example, 1 μm or more, and preferably 3 μm or more.

[0087] The polarizer 13 preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer 13 is, for example, 41.5% to 46.0%, preferably 43.0% to 46.0%, and more preferably 44.5% to 46.0%. The polarization degree of the polarizer 13 is preferably 97.0% or more, more preferably 99.0% or more, and further preferably 99.9% or more.

[0088] (First polarizer protective layer 12)

[0089] The first polarizer protective layer 12 is composed of any appropriate film that can be used as a protective layer of the polarizer 13. The film can be a laminate of more than two layers. As specific examples of the constituent materials of the film, cellulose resins such as triacetyl cellulose (TAC), polyester resins, polyvinyl alcohol resins, polycarbonate resins, polyamide resins, polyimide resins, polyether sulfone resins, polysulfone resins, polystyrene resins, polycycloolefin resins, polyolefin resins, (meth) acrylic resins, acetate resins, urethane resins, (meth) acrylic urethane resins, epoxy resins, silicone resins, etc. can be cited.

[0090] In order to reliably protect the polarizer 13, the surface 12a (see Figure 2 ) is preferably 4B or more, more preferably 3B or more, and further preferably 2B or more. In order to improve the handleability of the polarizing film laminate 10, the pencil hardness of the surface 12a of the first polarizer protective layer 12 on the first protective film 11 side is preferably H or less. The pencil hardness of the surface 12a can be adjusted, for example, by changing the type of constituent material of the first polarizer protective layer 12. In order to adjust the pencil hardness of the surface 12a to 4B or more, the constituent material of the first polarizer protective layer 12 is preferably a polyolefin resin such as a polyethylene resin, a polycycloolefin resin such as a polynorbornene resin, a polyester resin such as a polyethylene terephthalate resin, a polyamide resin, or a polycarbonate resin, and more preferably a polycycloolefin resin such as a polynorbornene resin. In addition, when the pencil hardness of the surface 12a is 4B or more, the hole marks 12b described later are likely to occur (see Figure 5 ).

[0091] The thickness of the first polarizer protection layer 12 is, for example, 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm.

[0092] (Adhesive layer 15)

[0093] The adhesive constituting the adhesive layer 15 is not particularly limited, and examples thereof include thermosetting adhesives and active energy ray-curing adhesives. From the viewpoint of improving productivity, active energy ray-curing adhesives are preferred. Specific examples of the adhesive constituting the adhesive layer 15 include epoxy resin adhesives, silicone resin adhesives, acrylic resin adhesives, polyurethane adhesives, polyamide adhesives, polyether adhesives, and the like.

[0094] The thickness of the adhesive layer 15 is, for example, 0.1 μm to 3.0 μm, or preferably 0.5 μm to 2.8 μm.

[0095] [Non-polarization portion forming step]

[0096] Next, refer to Figure 3 and Figure 4 The non-polarization portion forming step will be described. Figure 3 This is a process diagram showing an example of a process of forming a non-polarizing portion. Figure 4 This is a partial cross-sectional view showing an example of a polarizing film laminate after the non-polarizing portion is formed.

[0097] In the non-polarization portion forming step, Figure 3 As shown, the polarizing film laminate 10 is unwound from the polarizing film laminate roll 100 in the direction of the arrow in the figure, and the exposed portion from the through hole 14a in the polarizer 13 is contacted with the treatment liquid 21, thereby decolorizing to form a non-polarizing portion 13a (see Figure 4 ) Hereinafter, the portion exposed from the through hole 14a in the polarizer 13 may be simply referred to as an "exposed portion".

[0098] As the treatment liquid 21, for example, an alkaline solution can be cited. As a method for bringing the treatment liquid 21 into contact with the exposed portion, there is no particular limitation, for example, Figure 3 As shown in FIG. 1 , a method of immersing the polarizing film laminate 10 in the treatment liquid 21 while conveying the polarizing film laminate 10 can be mentioned. In addition, after immersing the polarizing film laminate 10 in the treatment liquid 21, as shown in FIG. Figure 3 As shown, the polarizing film laminate 10 is washed by being immersed in a washing liquid 22 (for example, water, alcohol, or a mixed liquid thereof) while being conveyed.

[0099] When the polarizer 13 contains iodine as a dichromatic substance, if an alkaline solution is brought into contact with the exposed portion, the iodine content of the exposed portion decreases, thereby decolorizing the exposed portion and forming a plurality of non-polarizing portions 13 a in the polarizer 13 .

[0100] The content of the dichroic substance (specifically, iodine, etc.) in the non-polarizing portion 13a is preferably less than 1.0 weight %, more preferably less than 0.5 weight %, and further preferably less than 0.2 weight %. If the content of the dichroic substance in the non-polarizing portion 13a is within such a range, the desired transparency can be fully imparted to the non-polarizing portion 13a. As a result, when the non-polarizing portion 13a corresponds to the camera portion of the image display device, excellent shooting performance can be achieved from the perspectives of both brightness and hue. On the other hand, the lower limit value of the content of the dichroic substance in the non-polarizing portion 13a is generally below the detection limit value. In addition, when iodine is used as the dichroic substance, the iodine content is obtained, for example, based on the X-ray intensity measured by fluorescent X-ray analysis and based on a calibration curve prepared in advance using a standard sample.

[0101] The difference between the content of the dichroic substance in the portion other than the non-polarizing portion 13a of the polarizer 13 and the content of the dichroic substance in the non-polarizing portion 13a is preferably 0.5 wt % or more, more preferably 1 wt % or more. If the difference in content is within such a range, a highly transparent non-polarizing portion 13a can be formed.

[0102] The light transmittance of the non-polarizing portion 13a (for example, the light transmittance measured by light of a wavelength of 550nm at 23°C) is preferably 50% or more, more preferably 60% or more, further preferably 75% or more, and particularly preferably 90% or more. With such a light transmittance, the transparency of the non-polarizing portion 13a becomes high. As a result, when the non-polarizing portion 13a is made to correspond to the camera portion of the image display device, excellent shooting performance can be achieved from the viewpoints of both brightness and color tone.

[0103] The alkaline solution contains an alkaline compound and a solvent that disperses and / or dissolves the alkaline compound. As the alkaline compound, any appropriate alkaline compound can be used. As the alkaline compound, there can be mentioned alkali metal hydroxides such as sodium hydroxide, potassium hydroxide, lithium hydroxide; alkaline earth metal hydroxides such as calcium hydroxide; inorganic alkali metal salts such as sodium carbonate; organic alkali metal salts such as sodium acetate; ammonia, etc. These alkaline compounds can be used alone or in combination. As preferred alkaline compounds, there can be mentioned alkali metal and / or alkaline earth metal hydroxides. As more preferred alkaline compounds, there can be mentioned sodium hydroxide, potassium hydroxide, lithium hydroxide. If the alkaline compound contains alkali metal and / or alkaline earth metal hydroxides, the iodine complex can be ionized with good efficiency, and the non-polarized portion 13a can be formed more easily.

[0104] As the solvent of the alkaline solution, any appropriate solvent can be used. As the solvent, water; alcohols such as ethanol and methanol; ether; benzene; chloroform; and mixed solvents thereof can be cited. As preferred solvents, water and alcohol can be cited. If the solvent contains water and / or alcohol, iodine ions can be smoothly moved from the polarizer 13 to the solvent, and iodine ions can be easily removed as the alkaline solution is removed.

[0105] The concentration (normality) of the alkaline compound in the alkaline solution is, for example, 0.01N to 5N, preferably 0.05N to 3N, and more preferably 0.1N to 2.5N. If the concentration of the alkaline compound is within such a range, the iodine concentration of the exposed portion can be reduced with good efficiency, and the ionization of the iodine complex in the polarizer 13 other than the exposed portion can be suppressed.

[0106] In the non-polarizing portion forming step, after the treatment liquid 21 is brought into contact with the exposed portion, the polarizing film laminate 10 may be immersed in a post-treatment liquid 23 (for example, an acidic solution). Figure 3 In the example shown, after the treatment liquid 21 is brought into contact with the exposed portion, the polarizing film laminate 10 is immersed in the cleaning liquid 22 while being conveyed, and then immersed in the post-treatment liquid 23. In addition, after the polarizing film laminate 10 is immersed in the post-treatment liquid 23, as shown in FIG. Figure 3 As shown, the polarizing film laminate 10 may be washed by being immersed in a washing liquid 24 (for example, water, alcohol, or a mixed liquid thereof) while being conveyed.

[0107] If the treatment liquid 21 is brought into contact with the exposed portion to form a non-polarized portion 13a, a metal salt of an alkali metal and / or an alkaline earth metal can be generated in the non-polarized portion 13a. Hydroxide ions can be generated from these metal salts. The generated hydroxide ions act on (decompose / reduce) the dichroic substance (e.g., iodine complex) present around the non-polarized portion 13a, and the non-polarized region (low-concentration region) can be expanded. If a post-treatment step of reducing the metal salt of an alkali metal and / or an alkaline earth metal is implemented, the expansion of the non-polarized region can be suppressed, and therefore, the dimensional change of the non-polarized portion 13a can be suppressed.

[0108] Representative examples of metal salts that can generate the hydroxide ions include borates, which can be generated, for example, by neutralizing the boric acid used in the stretching treatment with an alkaline solution (typically, a solution of an alkali metal hydroxide and / or an alkaline earth metal hydroxide).

[0109] If the post-treatment liquid 23 (typically an acidic solution) is brought into contact with the non-polarizing portion 13a, the metal salt of the alkali metal and / or alkaline earth metal can be moved to the post-treatment liquid 23, and the content of the metal salt of the alkali metal and / or alkaline earth metal in the non-polarizing portion 13a can be reduced. In particular, if the post-treatment liquid 23 is an acidic solution, the hydroxide of the alkali metal and / or alkaline earth metal remaining in the non-polarizing portion 13a can be neutralized, and the alkali metal and / or alkaline earth metal can be chemically removed.

[0110] The content of the metal salt of the alkali metal and / or alkaline earth metal in the non-polarizing portion 13 a after the post-treatment step is preferably 3.6 wt % or less, more preferably 2.5 wt % or less, further preferably 1.0 wt % or less, and particularly preferably 0.5 wt % or less.

[0111] The acidic solution contains an acidic compound and a solvent for dispersing and / or dissolving the acidic compound. As the acidic compound, any appropriate acidic compound can be used. Examples of the acidic compound include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, and boric acid; and organic acids such as formic acid, oxalic acid, citric acid, acetic acid, and benzoic acid. The acidic compound can be used alone or in combination. Preferred acidic compounds include inorganic acids, and more preferred acidic compounds include hydrochloric acid, sulfuric acid, and nitric acid.

[0112] Any appropriate solvent may be used as the solvent of the acidic solution. Examples of the solvent include the solvents listed as the solvents of the alkaline solution.

[0113] The concentration (normality) of the acidic compound in the acidic solution is, for example, 0.01N to 5N, preferably 0.05N to 3N, and more preferably 0.1N to 2.5N.

[0114] exist Figure 3 In the example shown, after the polarizing film laminate 10 is immersed in the cleaning liquid 24, for example, after a drying process not shown in the figure, the polarizing film laminate 10 is rolled up. The preferred range of the winding tension when the polarizing film laminate 10 is rolled up is, for example, the same as the preferred range of the winding tension when the polarizing film laminate 10 is rolled up in the above-mentioned winding material preparation process. In addition, when the polarizing film laminate 10 is rolled up, the first protective film 11 and the second protective film 14 can be peeled off from the polarizing film laminate 10 while being rolled up. That is, Figure 3 The step of winding up the polarizing film laminate 10 shown may also serve as a protective film peeling step described later.

[0115] [Protective film peeling process]

[0116] Next, the protective film stripping step is described. In the protective film stripping step, the first protective film 11 and the second protective film 14 are stripped from the polarizing film laminate 10. In addition, in the following description, the polarizing film laminate after the first protective film and the second protective film are stripped is sometimes described as a "polarizer with a protective layer on one side".

[0117] The method for peeling the first protective film 11 and the second protective film 14 from the polarizing film laminate 10 is not particularly limited, and for example, a roll-to-roll peeling device (not shown) can be used to peel the first protective film 11 and the second protective film 14 from the polarizing film laminate 10 while conveying the polarizing film laminate 10. By performing the protective film peeling step, the Figure 5 The polarizing plate 30 with a single-sided protective layer is shown. In the polarizing plate 30 with a single-sided protective layer, the polarizer 13 having a non-polarizing portion 13a and the first polarizer protective layer 12 are laminated via an adhesive layer 15. Figure 2 The polarizing film laminate 10 obtained after the second week of the single-sided protective layer polarizing plate 30 is as follows Figure 5 As shown, in the first polarizer protective layer 12, the X portion (refer to Figure 2 ) portion to form a hole mark 12b.

[0118] In order to improve the productivity of the circular polarizer by increasing the number of windings of the polarizer 30 with a single-sided protective layer, the thickness of the polarizer 30 with a single-sided protective layer is preferably 50 μm or less, and more preferably 40 μm or less. In addition, in order to improve the handling of the polarizer 30 with a single-sided protective layer, the thickness of the polarizer 30 with a single-sided protective layer is preferably 10 μm or more, and more preferably 15 μm or more. In addition, when the thickness of the polarizer 30 with a single-sided protective layer is 50 μm or less, when forming an image display device, if the surface 12a of the first polarizer protective layer 12 having a hole mark 12b is arranged closer to the visible side than the polarizer 13, the hole mark 12b becomes obvious, and there is a tendency to easily cause poor appearance. As described later, in the circular polarizer obtained in this embodiment, when forming an image display device, the polarizer 13 is arranged closer to the visible side than the hole mark 12b. Thus, in this embodiment, even if the thickness of the polarizer 30 with a single-sided protective layer is 50 μm or less, the occurrence of poor appearance can be suppressed.

[0119] [Second Polarizer Protective Layer Lamination Step]

[0120] Next, refer to Figure 5 and Figure 6 The second polarizer protective layer lamination step will be described. Figure 61 is a partial cross-sectional view showing an example of a polarizing film laminate after laminating the second polarizer protective layer. In the second polarizer protective layer lamination step, on the surface 13b (refer to Figure 5 ) is stacked on the second polarizer protective layer 42. Figure 6 In the example shown, the second polarizer protective layer 42 is laminated on the surface 13b via the adhesive layer 41. In the second polarizer protective layer laminating step, the second polarizer protective layer 42 may be laminated on the surface 13b via an adhesive layer (not shown).

[0121] The method for laminating the second polarizer protective layer 42 on the surface 13b via the adhesive layer 41 is not particularly limited. For example, there can be mentioned a method in which the second polarizer protective layer 42 is laminated (laminated) on the surface 13b via the adhesive layer 41 using a roll-to-roll laminating device (not shown) to convey the polarizing plate 30 with a protective layer on one side.

[0122] As the constituent material of the second polarizer protective layer 42, for example, the materials listed as the constituent materials of the first polarizer protective layer 12 mentioned above can be cited. The preferred range of the thickness of the second polarizer protective layer 42 is also the same as the preferred range of the thickness of the first polarizer protective layer 12 mentioned above. The constituent material of the first polarizer protective layer 12 and the constituent material of the second polarizer protective layer 42 can be the same or different. In addition, the thickness of the first polarizer protective layer 12 and the thickness of the second polarizer protective layer 42 can be the same or different.

[0123] As the adhesive constituting the adhesive layer 41, for example, there can be mentioned the adhesives listed as the adhesive constituting the above-mentioned adhesive layer 15. The preferred range of the thickness of the adhesive layer 41 is also the same as the preferred range of the thickness of the above-mentioned adhesive layer 15. The adhesive constituting the adhesive layer 15 and the adhesive constituting the adhesive layer 41 may be the same or different. In addition, the thickness of the adhesive layer 15 and the thickness of the adhesive layer 41 may be the same or different.

[0124] The second polarizer protection layer lamination step may be performed before or after the phase difference layer lamination step described below.

[0125] [Phase difference layer lamination process]

[0126] Next, refer to Figure 7 The phase difference layer lamination process will be described. Figure 7 1 is a partial cross-sectional view showing an example of a circular polarizing plate obtained by the manufacturing method of this embodiment. In the phase difference layer lamination step, the phase difference layer is laminated on the side of the first polarizer protective layer 12 opposite to the polarizer 13 side. Figure 7In the example shown, after the first phase difference layer 52 is bonded to the surface 12a of the first polarizer protective layer 12 on the opposite side to the polarizer 13 side via the adhesive layer 51, the second phase difference layer 54 is bonded to the surface 52a of the first phase difference layer 52 on the opposite side to the adhesive layer 51 side via the adhesive layer 53. Thus, the circular polarizing plate 200 is obtained. In addition, after the first phase difference layer 52 and the second phase difference layer 54 are bonded to each other via the adhesive layer 53, the first phase difference layer 52 may be bonded to the surface 12a of the first polarizer protective layer 12 on the opposite side to the polarizer 13 side via the adhesive layer 51.

[0127] The lamination method of the phase difference layer in the phase difference layer lamination process is not particularly limited as long as it is a method of laminating the phase difference layer on the side opposite to the polarizer 13 side of the first polarizer protective layer 12. As a specific example of the lamination method of the phase difference layer, a method of laminating the phase difference layer on the side opposite to the polarizer 13 side of the first polarizer protective layer 12 by the lamination method described in Japanese Patent Publication No. 2021-18354 can be cited.

[0128] On the other hand, as Figure 7 Different from the lamination method shown in the example, it is also possible to consider the surface 42a (see Figure 6 ) on the surface 42a of the second polarizer protective layer 42 opposite to the adhesive layer 41, when the obtained circular polarizer is used in an image display device, the hole mark 12b is arranged closer to the visible side than the polarizer 13, and therefore, the hole mark 12b is obvious. As a result, poor appearance is likely to occur. In contrast, in the present embodiment, a phase difference layer is stacked on the side of the first polarizer protective layer 12 opposite to the polarizer 13 (on the surface 42a of the second polarizer protective layer 42 opposite to the adhesive layer 41). Figure 7 In the example of the first phase difference layer 52 and the second phase difference layer 54), when the obtained circular polarizing plate 200 is used in an image display device, the polarizer 13 is arranged closer to the visible side than the hole mark 12b. As a result, the hole mark 12b becomes less noticeable in appearance, so according to this embodiment, the occurrence of poor appearance caused by the hole mark 12b can be suppressed.

[0129] As the first phase difference layer 52, for example, a liquid crystal orientation solidification layer can be cited. In addition, "liquid crystal orientation solidification layer" refers to an orientation solidification layer of a liquid crystal compound. In addition, "orientation solidification layer" refers to a layer in which a compound is oriented in a specified direction in a layer and the orientation state is fixed. By using a liquid crystal compound in the orientation solidification layer, the difference between nx and ny of the obtained liquid crystal orientation solidification layer can be made much larger than that of a non-liquid crystal material, and therefore, the thickness of the liquid crystal orientation solidification layer used to obtain the desired in-plane phase difference can be significantly reduced. As a result, the thinning and lightweight of the circular polarizer can be achieved. In addition, in the case of using a thin circular polarizer for an image display device, if the surface 12a of the first polarizer protective layer 12 having a hole mark 12b is arranged closer to the visible side than the polarizer 13, the hole mark 12b is obvious, and there is a tendency to easily have a poor appearance. In the circular polarizer obtained in this embodiment, when an image display device is formed, the polarizer 13 is arranged closer to the visible side than the hole mark 12b. Therefore, according to the present embodiment, even with a thin circular polarizing plate (circular polarizing plate having a thin retardation layer), the occurrence of poor appearance can be suppressed.

[0130] When the first phase difference layer 52 is a liquid crystal orientation solidification layer, there is no particular limitation as the liquid crystal orientation solidification layer, and for example, a liquid crystal orientation solidification layer described in Japanese Patent Publication No. 2021-18354 can be used. The liquid crystal orientation solidification layer is preferably a liquid crystal orientation solidification layer that functions as a quarter wave plate. When the first phase difference layer 52 is a liquid crystal orientation solidification layer that functions as a quarter wave plate, the thickness of the first phase difference layer 52 is, for example, 0.2 μm to 10 μm, preferably 0.5 μm to 7 μm.

[0131] When the first phase difference layer 52 is a liquid crystal orientation solidification layer that functions as a quarter wave plate, the second phase difference layer 54 is preferably a positive C plate. In the case of such a configuration, a circular polarizer that can also shield reflected light from external light from an oblique direction can be formed. When the second phase difference layer 54 is a positive C plate, the thickness of the second phase difference layer 54 is, for example, 0.2 μm to 10 μm, preferably 0.5 μm to 7 μm.

[0132] Alternatively, the first retardation layer 52 may be a liquid crystal alignment solidified layer functioning as a half wavelength plate. When the first retardation layer 52 is a liquid crystal alignment solidified layer functioning as a half wavelength plate, the thickness of the first retardation layer 52 is, for example, 0.2 μm to 10 μm, preferably 0.5 μm to 7 μm.

[0133] In the case where the first phase difference layer 52 is a liquid crystal orientation solidified layer that functions as a 1 / 2 wavelength plate, the second phase difference layer 54 is preferably a liquid crystal orientation solidified layer that functions as a 1 / 4 wavelength plate. In this case, it is preferably configured in such a manner that the angle formed by the slow axis direction of the 1 / 2 wavelength plate and the absorption axis direction of the polarizer 13 is 75°±5°, and the angle formed by the slow axis direction of the 1 / 4 wavelength plate and the absorption axis direction of the polarizer 13 is 15°±5°. The circular polarizer having such a layer structure functions as a circular polarizer in a wide wavelength range of visible light, and therefore, can reduce the coloring of reflected light.

[0134] As the adhesive constituting the adhesive layer 51, for example, there can be mentioned the adhesives listed as the adhesive constituting the above-mentioned adhesive layer 15. The preferred range of the thickness of the adhesive layer 51 is also the same as the preferred range of the thickness of the above-mentioned adhesive layer 15. The adhesive constituting the adhesive layer 15 and the adhesive constituting the adhesive layer 51 may be the same or different. In addition, the thickness of the adhesive layer 15 and the thickness of the adhesive layer 51 may be the same or different.

[0135] As the adhesive constituting the adhesive layer 53, for example, there can be mentioned the adhesives listed as the adhesive constituting the above-mentioned adhesive layer 15. The preferred range of the thickness of the adhesive layer 53 is also the same as the preferred range of the thickness of the above-mentioned adhesive layer 15. The adhesive constituting the adhesive layer 15 and the adhesive constituting the adhesive layer 53 may be the same or different. In addition, the thickness of the adhesive layer 15 and the thickness of the adhesive layer 53 may be the same or different.

[0136] The above describes the phase difference layer lamination process, but in the present invention, only one phase difference layer (e.g., a quarter wave plate) can be laminated on the side opposite to the polarizer side of the first polarizer protective layer. In addition, in the present invention, the phase difference layer can be laminated via an adhesive layer on the side opposite to the polarizer side of the first polarizer protective layer.

[0137] [Conditions for effectively exerting the effects of the present embodiment]

[0138] As described above, according to the manufacturing method of the circular polarizer of the present embodiment, the occurrence of poor appearance caused by hole marks can be suppressed. In the present embodiment, by satisfying the following condition 1, the effect of the present embodiment is more effectively exerted. In addition, in the present embodiment, by satisfying the following condition 2, the effect of the present embodiment is further effectively exerted. In addition, in the present embodiment, by satisfying the following condition 3, the effect of the present embodiment is particularly effectively exerted.

[0139] Condition 1: The thickness of the first protective film is 50 μm or less, and the thickness of the polarizing plate with a protective layer on one side is 50 μm or less.

[0140] Condition 2: The above-mentioned condition 1 is satisfied, and the pencil hardness of the surface on the first protective film side of the first polarizer protective layer is 4B or more.

[0141] Condition 3: The above condition 2 is satisfied, and the diameter of the opening of the through hole of the second protective film is 1 mm to 10 mm.

[0142] The above is a description of the method for manufacturing a circular polarizer of the present embodiment, but the method for manufacturing a circular polarizer of the present invention is not limited to the above embodiment. For example, the method for manufacturing a circular polarizer of the present invention may further include a step of laminating an adhesive layer (hereinafter referred to as an "outer adhesive layer") on the opposite side of the phase difference layer to the first polarizer protective layer after the phase difference layer lamination step. An image display device is formed by laminating the phase difference layer to an image display unit (for example, a liquid crystal unit, an organic EL unit, etc.) via the outer adhesive layer. The adhesive constituting the outer adhesive layer is not particularly limited, and for example, a transparent adhesive having a base polymer such as an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyvinyl ether, a vinyl acetate-vinyl chloride copolymer, a modified polyolefin, an epoxy resin, a fluorine resin, a natural rubber, a synthetic rubber, etc. can be appropriately selected. The thickness of the outer adhesive layer is not particularly limited, and is preferably 5μm to 100μm from the viewpoint of both thin layer and adhesion.

[0143] In addition, the method for manufacturing a circular polarizer of the present invention may further include a step of simultaneously pasting a release liner on the main surface of the outer adhesive layer on the opposite side of the phase difference layer. The release liner protects the surface of the outer adhesive layer, for example, until the phase difference layer is attached to the image display unit. As the constituent material of the release liner, a plastic film formed of acrylic acid, polyolefin, cyclic polyolefin, polyester, etc. can be suitably used. The thickness of the release liner is, for example, 5μm to 200μm. It is preferred that a release treatment is applied to the surface of the release liner. As materials for the release agent used for the release treatment, silicone-based materials, fluorine-based materials, long-chain alkyl-based materials, fatty acid amide-based materials, etc. can be cited.

[0144] In the method for producing a circularly polarizing plate of the present invention, the second polarizer protective layer lamination step is not an essential step. For example, an adhesive layer and a release liner may be sequentially laminated on the polarizer instead of the second polarizer protective layer.

Claims

1. A method for manufacturing a circular polarizer, comprising: Step Sa of preparing a roll of a polarizing film laminate that sequentially includes a first protective film, a first polarizer protective layer, a polarizer, and a second protective film having a through hole; Step Sb, wherein the polarizing film laminate is unwound from the roll while contacting the portion exposed from the through hole in the polarizer with a treatment liquid to thereby decolorize and form a non-polarizing portion; Step Sc of peeling the first protective film and the second protective film from the polarizing film laminate; and Step Sd of laminating a phase difference layer on the side of the first polarizer protective layer opposite to the polarizer side.

2. The method for manufacturing a circular polarizing plate according to claim 1, wherein: After the step Sc, a step Se is further provided of laminating a second polarizer protective layer on the surface of the polarizer from which the second protective film is peeled off.

3. The method for manufacturing a circular polarizing plate according to claim 1, wherein: The thickness of the first protective film is less than 50 μm.

4. The method for manufacturing a circular polarizing plate according to claim 1, wherein: In the step Sc, the polarizing film laminate has a thickness of 50 μm or less after the first protective film and the second protective film are peeled off.

5. The method for manufacturing a circular polarizing plate according to claim 1, wherein: The first polarizer protection layer is bonded to the polarizer by an adhesive.

6. The method for manufacturing a circular polarizing plate according to claim 1, wherein: The pencil hardness of the surface of the first polarizer protective layer on the first protective film side is 4B or more.

7. The method for manufacturing a circular polarizing plate according to claim 1, wherein: The second protective film has a thickness of 20 μm to 150 μm.

8. The method for manufacturing a circular polarizing plate according to claim 1, wherein: The diameter of the opening of the through hole is 1 mm to 10 mm.