Maintenance method based on concrete strength prediction model under freezing condition

By developing the accumulated temperature calculation equation under freezing conditions, the accumulated temperature discontinuity problem in the prediction of concrete strength below freezing point is solved, and the accurate prediction of concrete strength in low temperature environments and winter construction quality control is achieved, and the construction quality and safety are improved.

CN118942590APending Publication Date: 2024-11-12ZHEJIANG COMMUNICATIONS CONSTRUCTION NEW MATERIAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411001486.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

Smart Images

  • Figure CN118942590A_ABST
    Figure CN118942590A_ABST
Patent Text Reader

Abstract

The invention relates to a curing method based on a concrete strength prediction model under a freezing condition, which comprises the following steps: determining the mixing amount of each component in concrete according to the preset air content, water-cement ratio and slump of the concrete, mixing according to the mixing amount to obtain a concrete test piece, and further determining a compressive strength change curve; determining a concrete strength prediction model according to calculation rules of a concrete reaction rate equation and an equivalent age equation, and further determining apparent activation energy and related fitting constants according to a compressive strength change curve; and according to the chemical potential equation, the concrete reaction rate equation and the equivalent age equation, determining a related fitting constant and an accumulated temperature equation, and according to the compressive strength change curve, determining the related fitting constant. According to the method, the strength development of the concrete below the freezing point can be clearly expressed as the relationship between the accumulated temperature above 0 DEG C and the compressive strength, namely the phenomenon of discontinuous accumulated temperature at 0 DEG C is eliminated, and the maintenance work of the precast concrete component in winter can be effectively guided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of precast concrete component maintenance, and in particular to a maintenance method based on a concrete strength prediction model under freezing conditions. Background Art

[0002] Due to the growing demand for diversification in the current construction field, the performance requirements for cold-resistant concrete are also showing a trend of diversification. In view of the improvement of environmental awareness, reducing the carbon content in concrete has become a necessary direction for the development of the industry. For concrete construction under freezing conditions, it is particularly necessary to control the initial heating temperature of concrete at the lowest possible level to reduce carbon dioxide emissions. To this end, the possibility of introducing various innovative materials and technologies in winter concrete maintenance is currently being actively explored. In order to accurately predict the strength development of concrete below freezing point, special tests have been carried out to clarify the maturity of concrete below freezing point (0℃) and obtain an equation that matches the maturity equation used under temperature conditions above freezing point. This research result has significant guiding significance for guiding the maintenance of precast concrete components in winter.

[0003] The temperature dependence of concrete strength can be explicitly expressed using maturity, which expresses the effects of temperature and time in a complex way. One such maturity equation was proposed by Nurse et al. based on empirical rules: , Bergström later pointed out that the reference temperature T0 of general concrete is -10℃. Koh et al. introduced this technology in Japan and developed it into a concrete construction planning and management technology under cold conditions, which has been widely used. Another maturity equation shows that the reaction temperature dependence follows the following Arrehenius equation: , which takes the ratio of the reaction rate at a reference temperature to the reaction rate at different curing temperatures and converts it into an age at the reference temperature (equivalent age). Carino examined the equation for maturity and studied the calculation method of the base temperature T0 of the accumulated temperature and the apparent activation energy E of the equivalent age, which has been used in ASTM 2011.

[0004] Based on this, estimating strength through engineering maturity requires the relationship between maturity and strength to be derived in advance. Modeling the maturity-compressive strength relationship can summarize the temperature dependence and derive the estimated strength. As part of his maturity-strength relationship model, Plowman gave the relationship between accumulated temperature and strength: . Carino and Tank gave the following hyperbolic equation: , this equation is also applicable to setting the accumulated temperature as age, and is standardized as the basic equation in ASTM C1074. Katsura et al. gave the relationship for the Gompertz curve approximation: , substituting the accumulated temperature into the formula with the age, the result is almost exactly the same as the equivalent age formula used by Hansen and Pedersen. In CEB Model Code 90 (CEB 1993), maturity and compressive strength at any age are expressed as follows: .

[0005] Therefore, the typical models of the existing maturity-strength relationship expressions used in construction site engineering are shown above, including curves obtained by empirical approximation of their shapes and curves obtained by assuming the reaction rate equation of the basic cement reaction. However, since these are all empirical equations to express the relationship between maturity and strength, the application is limited to the scope of basic empirical data, and the strength development below the freezing point is completely different from the compressive strength development characteristics above the freezing point, and cannot be expressed by the same maturity equation used at and above the freezing point.

[0006] At present, Nykanen proposed a temperature-time equation to express the development of strength below freezing point: , , although the reference temperature of the accumulated temperature is -10℃, Nykanen pointed out that the test results can also be successfully obtained by setting the reference temperature to -15℃ and setting it to 0.2 times the accumulated temperature. However, this technique produces an accumulated temperature discontinuity at 0℃ and is not applicable to temperatures below -15℃. Similarly, Mimori et al. used -10℃ as the reference temperature and multiplied the calculated value by the reduction factor α below the solidification point. The value of the reduction factor α varies with the water-cement ratio and the type of concrete. It is not universal, and when the application range is -10℃ or higher, the formula cannot eliminate the discontinuity at 0℃. Sudo et al. measured the apparent reaction rate based on the bound water ratio of the solidified cement paste under dry and frozen conditions, and studied the changes in the chemical potential of the reaction water caused by drying and freezing under the reaction rate constant of the Arrehenius equation, and established a simple cement hydration model: , whose research successfully expressed the apparent response rate, but its application in strength development has not been studied. It can be seen that the application scope of the sub-zero temperature maturity equation currently proposed is limited to the experimental scope of the paper, and it is difficult to regard it as a practical equation. Summary of the invention

[0007] The problem to be solved by the present invention is to provide a maintenance method based on a concrete strength prediction model under freezing conditions in view of the above-mentioned deficiencies in the prior art. The research has obtained a calculation equation for accumulated temperature below freezing point that can express the influence of temperature-time effect on low-temperature strength development, and the applicability of the formula has been verified by conducting strength tests on premixed concrete cured under ambient conditions, thereby proving its effectiveness. Under freezing (below freezing point) conditions, using the accumulated temperature equation as a concrete strength prediction model can clearly express the strength development of concrete below freezing point as the relationship between accumulated temperature above 0°C and compressive strength, that is, eliminating the phenomenon of accumulated temperature discontinuity at 0°C, thereby effectively guiding the maintenance of precast concrete components in winter.

[0008] The above-mentioned object of the present invention is achieved through the following technical solutions:

[0009] A maintenance method based on a concrete strength prediction model under freezing conditions comprises the following steps:

[0010] S1 determines the dosage of cement, coarse aggregate, fine aggregate, water and admixture in concrete according to the predetermined air content, water-cement ratio and slump of concrete, mixes according to the dosage to obtain concrete specimens, and then determines the compressive strength variation curve of concrete specimens with different water-cement ratios at different curing temperatures;

[0011] S2 According to the concrete reaction rate equation and the equivalent age equation The calculation rules are used to determine the concrete strength prediction model when the fitting constant μ=0. , and according to the compressive strength change curve, the apparent activation energy E, fitting constants a and b are determined; wherein, k T is the concrete reaction rate, E is the apparent activation energy, μ is the chemical potential energy of water, R is the gas constant, T is the Kelvin temperature, T e is the equivalent age of concrete, k rf is the reaction rate constant at 0°C, Δt is the time interval, F is the compressive strength of concrete, and F inf is the maximum strength of concrete, A, β, a and b are fitting constants;

[0012] S3 According to the chemical potential equation , the concrete reaction rate equation and equivalent age equation, determine the fitting constant β and the accumulated temperature equation , and according to the compressive strength variation curve, the fitting constants A, c and d are determined; wherein, M μf is the cumulative temperature obtained after curing for one day at the Kelvin temperature T, c and d are fitting constants;

[0013] S4 predicts the strength of the concrete specimens cured under freezing conditions according to the accumulated temperature equation, and adjusts the curing strategy according to the actual curing conditions to ensure that the concrete specimens can meet the predetermined strength requirements during the winter curing process.

[0014] Further, in S1, the air content of the concrete is controlled to be 4.5% v / v, the water-cement ratio is 30-60wt%, the slump is 180-600mm, the cement is ordinary Portland cement and / or fly ash Portland cement, the coarse aggregate is Toma gravel, the fine aggregate is Toma river sand, and the admixture is polycarboxylate water reducer and / or lignin sulfonate water reducer.

[0015] Furthermore, in S1, the density of ordinary Portland cement is 3.17 g / m 3 , with a specific surface area of ​​3450cm 2 / g, C3S content is 59.6wt%, C2S content is 15.6wt%, C3A content is 8.5wt%, and C4AF content is 9.1wt%.

[0016] Alternatively, in S1, the density of cement in fly ash silicate cement is 3.16 g / m 3 , with a specific surface area of ​​3460cm 2 / g, C3S content is 59.3wt%, C2S content is 15.1wt%, C3A content is 9.6wt%, C4AF content is 8.6wt%; the fly ash content in fly ash silicate cement is 15wt%, the ignition loss is 1.7%, the SiO2 content is 68.6wt%, the water content is 0.15wt%, and the density is 2.11g / m 3 , with a specific surface area of ​​3890cm 2 / g.

[0017] Furthermore, in S1, the saturated surface dry density of the Toma River sand is 2.58 g / cm 3 , the water absorption coefficient is 2.50%.

[0018] Furthermore, in S1, the surface density of the Toma gravel in the dry saturated state is 2.88 g / cm 3 , the water absorption coefficient is 1.88%.

[0019] Furthermore, in S1, concrete specimens with different water-cement ratios are respectively subjected to constant temperature curing at 5~35°C and low temperature curing at -1~-10°C until a predetermined age, and the compressive strength of the cured concrete specimens is measured; wherein, the low temperature curing is pre-cured at 10°C to 5~10MPa for 2 days, and then cured at -1~-10°C.

[0020] Furthermore, in S2, the cement is ordinary Portland cement, the apparent activation energy E is 44350 J / mol, the fitting constant a is -11.91, and the fitting constant b is -1.01.

[0021] Alternatively, in S2, the cement is fly ash silicate cement, the apparent activation energy E is 40319 J / mol, the fitting constant a is -7.91, and the fitting constant b is -1.30.

[0022] Furthermore, in S3, the cement is ordinary Portland cement, the fitting constant A is 43.1, the fitting constant β is 10.0, the fitting constant c is -0.60, and the fitting constant d is 0.74.

[0023] Alternatively, in S3, the cement is fly ash silicate cement, the fitting constant A is 39.5, the fitting constant β is 9.1, the fitting constant c is -0.60, and the fitting constant d is 0.74.

[0024] In summary, the beneficial technical effects of the present invention are:

[0025] 1. By adopting the above-mentioned maintenance method based on the concrete strength prediction model under freezing conditions, not only can the strength of concrete specimens be accurately predicted in low temperature environments such as winter, but the maintenance strategy can also be flexibly adjusted according to actual maintenance conditions to ensure that the concrete specimens meet the predetermined strength requirements during winter maintenance. This maintenance method significantly improves the quality control level of precast concrete components in winter construction and reduces engineering risks caused by substandard strength.

[0026] 2. In addition, the method of the present invention also considers the influence of different cement types (such as ordinary Portland cement and fly ash Portland cement) on the strength of concrete, and determines the corresponding fitting constants through experiments, making the prediction model more accurate and reliable; at the same time, the present invention also considers the change of compressive strength of concrete specimens at different curing temperatures, providing a scientific basis for the curing of precast concrete components under different environments;

[0027] 3. In practical applications, the method of the present invention can realize automatic control through programming software or electronic equipment, which greatly simplifies the operation process in the maintenance process and improves work efficiency; at the same time, the method can also be combined with other intelligent technologies, such as Internet of Things technology, big data technology, etc., to realize real-time monitoring and data analysis of the maintenance process of precast concrete components, and provide more comprehensive and efficient support for engineering quality management;

[0028] 4. In summary, the maintenance method based on the concrete strength prediction model under freezing conditions of the present invention has significant technical advantages and application prospects, and will play an important role in the winter maintenance of precast concrete components. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a curve diagram between the age and compressive strength of concrete specimens Ⅰ-1~Ⅰ4 of Example 2 of the present invention.

[0030] Figure 2 It is a curve diagram between the age and concrete strength of concrete specimens II-1 to II-4 of Example 2 of the present invention.

[0031] Figure 3 It is a curve diagram between the age and concrete strength of concrete specimens Ⅰ-5~Ⅰ8 of Example 2 of the present invention.

[0032] Figure 4 It is a curve diagram between the age and concrete strength of concrete specimens II-5 to II-8 of Example 2 of the present invention.

[0033] Figure 5 (Left) is a graph showing the measured compressive strength and the estimated compressive strength of concrete specimens II-1 to II-4 of Example 3 of the present invention.

[0034] Figure 5 (Right) is a graph showing the measured compressive strength and the estimated compressive strength of concrete specimens II-5 to II-8 of Example 3 of the present invention.

[0035] Figure 6 It is a curve diagram between the accumulated temperature and the compressive strength of the concrete specimens II-1 to II-4 of Example 4 of the present invention.

[0036] Figure 7 It is a curve diagram between the accumulated temperature and the compressive strength of the concrete specimens II-5 to II-8 of Example 4 of the present invention.

[0037] Figure 8 This is a temperature change diagram of the concrete component after outdoor sealing and curing in Example 5 of the present invention.

[0038] Fig. 9 This is a graph showing the compressive strength of concrete components according to Example 5 of the present invention.

[0039] Fig.10 4 is a relationship diagram between the accumulated temperature and the compressive strength of the concrete member of Example 5 of the present invention.

[0040] Fig.11 4 is a relationship diagram between the temperature measurement interval and the calculated accumulated temperature of the concrete component in Example 5 of the present invention. DETAILED DESCRIPTION

[0041] In order to make the technical means, creative features, objectives and functions achieved by the present invention clearer and easier to understand, the present invention is further explained below in conjunction with the accompanying drawings and specific implementation methods.

[0042] Embodiment 1: A maintenance method based on a concrete strength prediction model under freezing conditions disclosed in the present invention comprises the following steps:

[0043] S1 determines the dosage of cement, coarse aggregate, fine aggregate, water and admixture in concrete according to the predetermined air content, water-cement ratio and slump of concrete, and mixes them according to the dosage to obtain concrete specimens, and then determines the compressive strength variation curve of concrete specimens with different water-cement ratios at different curing temperatures;

[0044] S2 According to the concrete reaction rate equation and the equivalent age equation The calculation rules are used to determine the concrete strength prediction model when the fitting constant μ=0. , and according to the compressive strength change curve, the apparent activation energy E, fitting constants a and b are determined; where k T is the concrete reaction rate, E is the apparent activation energy, μ is the chemical potential energy of water, R is the gas constant, T is the Kelvin temperature, T e is the equivalent age of concrete, k rf is the reaction rate constant at 0°C, Δt is the time interval, F is the compressive strength of concrete, and F inf is the maximum strength of concrete, A, β, a and b are fitting constants;

[0045] S3 According to the chemical potential equation , concrete reaction rate equation and equivalent age equation, determine the fitting constant β and accumulated temperature equation , and according to the compressive strength change curve, the fitting constants A, c and d are determined; among them, M μf is the cumulative temperature obtained after curing for one day at the Kelvin temperature T, c and d are fitting constants;

[0046] S4 predicts the strength of concrete specimens cured under freezing conditions based on the accumulated temperature equation, and adjusts the curing strategy according to the actual curing conditions to ensure that the concrete specimens can meet the predetermined strength requirements during the winter curing process.

[0047] Embodiment 2: A maintenance method based on a concrete strength prediction model under freezing conditions disclosed in the present invention, which is different from Embodiment 1 in that the specific implementation of S1 is:

[0048] S11 determines the air content, water-cement ratio and slump of concrete; wherein, when the air content of concrete is 4.5% v / v and the water-cement ratio is 30wt%, the slump is 600mm, and when the water-cement ratio is 40, 50 or 60wt%, the slump is 180mm;

[0049] S12 prepares concrete raw materials, which include cement, coarse aggregate, fine aggregate, water and admixtures; wherein the cement is ordinary Portland cement and / or fly ash Portland cement; the density of ordinary Portland cement is 3.17 g / m 3 , with a specific surface area of ​​3450cm 2 / g, C3S content is 59.6wt%, C2S content is 15.6wt%, C3A content is 8.5wt%, C4AF content is 9.1wt%; the density of cement in fly ash silicate cement (Portland cement) is 3.16g / m 3 , with a specific surface area of ​​3460cm 2 / g, C3S content is 59.3wt%, C2S content is 15.1wt%, C3A content is 9.6wt%, C4AF content is 8.6wt%; the coarse aggregate is Toma gravel, and the saturated surface dry density of Toma river sand is 2.58 g / cm 3 The water absorption coefficient is 2.50%; the fine aggregate is Toma River sand, and the surface dry saturated density of Toma gravel is 2.88g / cm 3 , the water absorption coefficient is 1.88%; when the water-cement ratio is 30 or 40wt%, the admixture is a polycarboxylate water reducer, and when the water-cement ratio is 50 or 60wt%, the admixture is a lignin sulfonate water reducer;

[0050] S12 determines the dosage of each component in the concrete raw material, as shown in Table 1 below; the concrete is stirred by a 100L mixer, and the stirring temperature is controlled to be stable at 15°C; for cement with a water-cement ratio of 40-60wt%, all of it is added at one time, and the stirring time is 3min; for cement with a water-cement ratio of 30wt%, the mortar is premixed for 3min, coarse aggregate is added, and it is stirred again for 1.5min; the cement is allowed to stand for 5min, then stirred for another 30s, and finally sprayed out, and the slump or fluidity value is measured immediately after stirring, and the gas volume is measured by the pressure method, and concrete is poured in a φ10×20cm mold to obtain a concrete specimen;

[0051] Table 1

[0052] Group Cement Type Water-cement ratio / % s / a / % <![CDATA[Cement consumption / kg / m 3 > <![CDATA[Fine aggregate dosage / kg / m 3 > <![CDATA[Coarse aggregate dosage / kg / m 3 > <![CDATA[Water consumption / kg / m 3 > <![CDATA[Water reducing agent dosage / kg / m 3 > Ⅰ-1 Ordinary Portland Cement 60 45.9 293 812 1070 176 1.00 Ⅰ-2 Ordinary Portland Cement 50 44.4 352 764 1070 176 1.00 Ⅰ-3 Ordinary Portland Cement 40 42.9 425 720 1070 170 0.70 Ⅰ-4 Ordinary Portland Cement 30 48.0 583 737 892 175 1.60 Ⅰ-5 Fly ash silicate cement 60 45.9 287 812 1070 172 0.87 Ⅰ-6 Fly ash silicate cement 50 44.3 344 763 1070 172 0.87 Ⅰ-7 Fly ash silicate cement 40 42.8 415 717 1070 166 0.87 Ⅰ-8 Fly ash silicate cement 30 47.7 570 729 892 171 1.67 Ⅱ-1 Ordinary Portland Cement 60 45.5 298 800 1070 179 1.00 Ⅱ-2 Ordinary Portland Cement 50 43.9 358 751 1070 179 1.00 Ⅱ-3 Ordinary Portland Cement 40 42.9 425 720 1070 170 0.80 Ⅱ-4 Ordinary Portland Cement 30 48.0 583 737 892 175 2.13 Ⅱ-5 Fly ash silicate cement 60 45.4 293 796 1070 176 1.00 Ⅱ-6 Fly ash silicate cement 50 43.7 352 745 1070 176 1.00 Ⅱ-7 Fly ash silicate cement 40 42.8 415 717 1070 166 0.90 Ⅱ-8 Fly ash silicate cement 30 47.7 570 729 892 171 2.00

[0053] After S13 casting is completed, the upper surface of the specimen is sealed with a polyethylene film, and then it is cured in a constant temperature box at a set temperature until the specified age (1 or 2, 3, 7, 14, 28, 56, 91, 119*, 182 days) is reached. Then, after curing the specimen in water for 1 day, it is taken out of the mold and immediately placed in 20°C water for curing to the specified age (3, 7, 28 days). Among them, in the curing process of concrete specimens Ⅰ-1~Ⅰ8, the cast concrete specimens are immediately sealed and cured in a constant temperature room after forming to the specified age, and the curing temperatures are 5°C, 20°C and 35°C respectively; when concrete construction is carried out under cold conditions, it should be avoided that the concrete is exposed to temperatures below zero immediately after casting to prevent early frost damage. Therefore, after completing the pre-curing equivalent to the initial curing, it is cured at sub-zero temperatures in series II; in the curing process of concrete specimens Ⅱ-1~Ⅱ-8, the concrete specimens are first cured in a constant temperature room at 10°C. , until the compressive strength reaches 5~10MPa. After confirming the strength development, the concrete is moved to a constant temperature chamber set at a temperature below freezing (-1℃, -5℃ and -10℃), and continues to be cured in a sealed state until the specified age is reached; for concrete cured at -1℃, it is believed that the water in the concrete pores will not freeze when the concrete pre-cured at 10℃ is moved; therefore, based on the preliminary research results, it was decided to move the concrete to a constant temperature chamber of -1℃ after being placed in a constant temperature chamber of -5℃ for one day to ensure that the core temperature is reduced to -5℃; in the actual experiment, an embedded thermocouple was used for temperature measurement; after confirming that the core temperature has stably reached -1℃, the compressive strength is measured 2 days after the pre-curing is completed; for all concrete cured under sub-freezing temperature conditions, the compressive strength is measured 2 days after the pre-curing is completed, and it is used as the starting point for the development of strength below freezing; then it is cured until the specified age is reached;

[0054] After S14 curing, the end face of each specimen was ground and the compressive strength was measured according to JIS A 1108. After the specimens cured at a temperature below freezing were taken out of the mold in the laboratory, they were immersed in 20°C water for about 30 minutes to melt the internal ice and then measured. The melting time was obtained from preliminary experiments based on the temperature measurement in the cylinder embedded with the thermocouple. Therefore, at a temperature of -10°C, the melting time takes about 30 minutes, and at a lower temperature it takes about 1 hour. The compressive strength test results are shown in Figures 1 to 4 shown.

[0055] Embodiment 3 is a maintenance method based on a concrete strength prediction model under freezing conditions disclosed by the present invention. The difference from Embodiment 1 is that the specific implementation of S2 is:

[0056] S21 established a simple cement hydration model based on the apparent hydration rate measurement of the proportion of bound water in cement paste and examined the reaction rate. The researchers found that in hardened cement under dry or frozen conditions, the chemical potential of water reacting with cement decreased and the reaction rate slowed down. The researchers described the reaction rate constant equation by the following equation (1), which includes the effect of the reduced chemical potential in the Arrehenius equation;

[0057] (1) ;

[0058] Among them, k T is the concrete reaction rate, E is the apparent activation energy, μ is the chemical potential energy of water, R is the gas constant, and T is the Kelvin temperature;

[0059] The S22 equivalent age is the temperature-time equation that represents the development of concrete strength, expressed by the reaction rate constant of the Arrehenius equation, as shown in the following equation (2);

[0060] (2) ;

[0061] Among them, T e is the equivalent age of concrete, k rf is the reaction rate constant at the reference temperature, Δt is the time interval;

[0062] S23 Obtain the apparent activation energy according to the above equations (1) and (2) to match the strength development approximated by the Gompertz curve with the test results. In order to make the strength development below the freezing point consistent with the range of 0°C and above, the reference temperature in the above equation (2) is set to 0°C (273.15K) during the calculation; Since the curing of concrete specimens Ⅰ-1 to Ⅰ8 is based on sealed specimens, the change in internal moisture caused by hydration can be regarded as the decrease in the chemical potential of water. However, as mentioned above, since there is almost no difference in the strength development observed between concrete cured at 20°C water and concrete cured at 20°C sealed, this effect is very small and can be ignored, that is, μ = 0, and the following equation (1') is obtained;

[0063] (1') ;

[0064] The strength development of S24 concrete is modeled using equation expressions, which can be approximated by the Logistic curve and the Gompertz curve when the cumulative temperature is used. In this study, the strength development is expressed as an equation of the equivalent age formula (1') and (2), and is approximated by the Gompertz curve as the concrete strength prediction model shown in the following formula (3);

[0065] (3) ;

[0066] Where F is the compressive strength of concrete, F inf is the maximum strength of concrete, A, β, a and b are fitting constants;

[0067] Applying this equation to the test results of Series I, using the nonlinear least squares method, we obtain E for each cement, a and b for each concrete; since the expected F inf It will change with the change of initial age temperature conditions, so it is determined for each concrete and each curing temperature; the apparent activation energy E obtained is: 44350 J / mol for ordinary Portland cement and 40319 J / mol for fly ash Portland cement;

[0068] S25 is to further verify the correlation between the measured strength values ​​of ordinary Portland cement concrete and fly ash Portland cement concrete and the strength calculated by formula (3). The results are as follows Figure 5 As shown, for these two cements, the correlation between the measured strength and the calculated strength is very strong, with a correlation coefficient of 0.99 or higher. Therefore, the obtained empirical equation can successfully represent the strength development. On this basis, the values ​​obtained here will be used as the values ​​of the apparent activation energy of the cement for subsequent tests.

[0069] Embodiment 4 is a maintenance method based on a concrete strength prediction model under freezing conditions disclosed by the present invention. The difference from Embodiment 1 is that the specific implementation of S3 is as follows:

[0070] The chemical potential energy μ of S31 water is obtained from the empirical equation based on the decrease of chemical potential energy during the melting process of ice from -70℃, as shown in the following equation (4);

[0071] (4) ;

[0072] S32 The experimental constant β in formula (1) is the optimal value derived from the test results below the freezing point and the test results at various water-cement ratios at and above 0°C, the strength development curve approximated by the Gompertz curve, and the nonlinear least squares method. In addition to the freezing effect of water, the chemical potential of water will also decrease due to the reduction of water in the concrete caused by hydration. However, since no difference in strength development was observed between concrete cured at 20°C water and concrete cured at 20°C sealed, the effect of internal moisture changes caused by hydration was ignored as secondary. The β of each cement was determined by the calculation formula for each chemical potential shown in formula (4), and the β values ​​were: 10.0 for ordinary Portland cement and 9.1 for fly ash Portland cement;

[0073] S33 By substituting equation (1) into equation (4) and then into equation (2) to calculate the equivalent age, it is found that the equivalent age can be expressed as an equation of temperature; wherein equation (4) can be considered as a calculation equation that includes the effect of melting point depression and the effect related to pore size from its derivation process. However, it is an equation obtained during the melting process at -60°C or lower, and does not include the effect caused by supercooled water, and the existing equation cannot properly describe the reduction of the chemical potential of water in the pores of concrete;

[0074] S34 If a line can be obtained that can connect the value of equation (4) in the range of -1 to -5 °C with the Radjy equation at a lower temperature and the volume equation The curve connecting the values ​​of can be obtained to obtain an equation to explain the strength development below the freezing point. Therefore, assuming the strength development, the relationship between the logarithmic value of the equivalent age and the temperature can be expressed by the following equation (5);

[0075] (5) ;

[0076] S36 By applying the above equation (5) to the test results to determine the empirical constant, the equation becomes an empirical equation for calculating the equivalent age below freezing point; however, in concrete engineering under cold conditions, the cumulative temperature is generally used for the temperature-time equation at 0°C or higher, which is difficult to be regarded as continuous; modify the following equation (6) so that 1 day of curing at 0°C becomes 10°C cumulative temperature days, which can continuously handle 0°C or higher cumulative temperatures;

[0077] (6) ;

[0078] Among them, M μf is the cumulative temperature obtained after curing for one day at the Kelvin temperature T, c and d are fitting constants;

[0079] The values ​​of S37 coefficients c and d are determined by nonlinear least squares method to make the relationship between the strength and the accumulated temperature below the solidification point calculated by equation (6) above consistent with the empirical value; for the influence of cement type, by comparing the calculation results of equation (4), it is determined that there is no significant difference. Regardless of the cement type, the calculated values ​​are the same. Through this, the accumulated temperature equation for the temperature range below the solidification point is obtained, as shown in equation (6') below;

[0080] (6') ;

[0081] S38 The calculation results of equation (6') and equation (4) are transformed. The shape of the obtained equation is almost connected with the values ​​of equation (4) in the range of -1℃ to -5℃ and the values ​​of Radjy equation and volume equation below this temperature, which is consistent with expectations. At the same time, combined with Figure 6 and Figure 7 Calculated compressive strength versus accumulated temperature. Although there are some variations, it can be confirmed that the strength development of all concretes is almost unambiguously expressed within the sub-zero curing temperature range.

[0082] Embodiment 5 is a maintenance method based on a concrete strength prediction model under freezing conditions disclosed by the present invention. The difference from Embodiment 1 is that the specific implementation of S4 is as follows:

[0083] S31 determines the technical parameters of concrete components. The concrete used is premixed concrete with a nominal strength of 24 MPa, the cement is ordinary Portland cement, and the fine aggregate is Toma River sand (density 2.59 g / cm in saturated surface dry state). 3 ; water absorption coefficient 2.66%), the coarse aggregate is Tomah gravel (density 2.60g / cm2 in saturated surface dry state) 3 ; Water absorption coefficient 1.94%), concrete mix ratio is shown in Table 2;

[0084] Table 2

[0085] Group Cement Type Water-cement ratio / % s / a / % <![CDATA[Cement consumption / kg / m 3 > <![CDATA[Fine aggregate dosage / kg / m 3 > <![CDATA[Coarse aggregate dosage / kg / m 3 > <![CDATA[Water consumption / kg / m 3 > <![CDATA[Dosage of water reducer / kg / m 3 > Ⅲ Ordinary Portland Cement 60 45.9 293 812 1070 176 1.00

[0086] S32 curing conditions are shown in Table 3;

[0087] Table 3

[0088] Group Maintenance conditions Age / day 1~2 Curing in water at 20℃ 28,91 3~9 20℃ sealed maintenance 2,4,7,14,28,56,91 10~13 5℃ sealed maintenance 14,28,56,91 14~25 -2℃, -5℃, -10℃ sealed maintenance 28,56,91,182 26~29 Outdoor sealing maintenance 14,28,56,91

[0089] S33 After the concrete arrives, the slump and air content are measured immediately, and the concrete is poured in a φ10×20cm mold. After pouring, the upper surface of the specimen is sealed with a polyethylene film and cured in a constant temperature chamber at 20°C for 2 days; after that, it continues to cure in a sealed state outdoors or in a constant temperature chamber set to a specific temperature until it reaches the specified age; for each set of curing conditions, a TC thermocouple is buried in the center of the specimen, and the concrete temperature is measured and recorded every 15 minutes until the specified age is reached;

[0090] After the specified curing of S34 is completed, the compressive strength is measured according to JISA 1108. The specimens cured at a temperature below freezing are measured after being immersed in 20℃ water for about 1 hour in the laboratory to melt the internal ice. The test results are as follows Figures 8 to 11 shown.

[0091] from Figure 8 and Fig. 9 It can be seen that the strength development was observed under constant temperature and exposure conditions below freezing. Under constant temperature curing conditions, the strength development varies with the curing temperature, and at lower temperatures, the strength development tends to be slower.

[0092] from Fig.10 It can be seen that for concrete cured at a constant temperature below freezing and for concrete exposed outdoors, the relationship between accumulated temperature and compressive strength at temperatures close to 0°C or higher can be clearly expressed. Based on this, the accumulated temperature equation proposed in this study can be considered to be applicable even to ready-mixed concrete made from different cements and is a temperature-time equation that can clearly express strength development even in the presence of temperature and time fluctuations.

[0093] Meanwhile, during concrete working under cold conditions, especially during extended age without heating, temperature fluctuations occur every day, and concrete temperature fluctuates accordingly. However, there are no clear guidelines on how to record concrete temperature data and predict strength when strength management is performed. The temperature measurement intervals for strength management were checked using the concrete specific temperature measurement records of the exposed specimens in this study. Based on the measurement results of this study, the degree of difference in accumulated temperature calculated using the daily average temperature, seasonal average temperature, and data at intervals of 15 min, 1 h, 2 h, 4 h, and 6 h was calculated.

[0094] from Fig.11 It can be seen that there is no significant difference in the accumulated temperature obtained when the measurement interval is set between 15min and 6h. However, when the daily average temperature is used, the accumulated temperature value decreases by about 15% compared to the interval of up to 6h; when the seasonal average temperature is used, the value decreases by about 35%. When the temperature of the concrete fluctuates around the 0℃ mark throughout the day, the accumulated temperature values ​​obtained at temperatures below 0℃ drop sharply. Therefore, when the measurement interval is wide enough and the fluctuation within a day is not obvious, the average temperature may always be 0℃ or lower, and the temperature above 0℃ may not be calculated as accumulated temperature. In contrast, if the measurement interval is shortened and the daily variation is clear, the time spent at 0℃ or higher can be calculated. Therefore, it is expected that the accumulated temperature values ​​will differ depending on the temperature measurement interval, so it can be managed according to the temperature data, and the measurement interval is set as short as possible, with 6h as the upper limit.

[0095] Therefore, the present invention obtains the calculation equation of cumulative temperature below freezing point based on the empirical results of preparing concrete with ordinary Portland cement and fly ash Portland cement, and verifies its effectiveness through demonstration tests of ordinary Portland cement ready-mixed concrete. Although it has not yet been confirmed in other types of cement, it can be inferred that it can be used within the range of strength development below freezing point, and the cumulative temperature can be used as a maturity equation. However, verification using concrete made from other cements is still necessary and is a problem that needs to be solved in the future.

[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A maintenance method based on a concrete strength prediction model under freezing conditions, characterized in that: The following steps are included: S1 determines the dosage of cement, coarse aggregate, fine aggregate, water and admixture in concrete according to the predetermined air content, water-cement ratio and slump of concrete, mixes according to the dosage to obtain concrete specimens, and then determines the compressive strength variation curve of concrete specimens with different water-cement ratios at different curing temperatures; S2 According to the concrete reaction rate equation and the equivalent age equation The calculation rules are used to determine the concrete strength prediction model when the fitting constant μ=0. , and according to the compressive strength change curve, the apparent activation energy E, fitting constants a and b are determined; wherein, k T is the concrete reaction rate, E is the apparent activation energy, μ is the chemical potential energy of water, R is the gas constant, T is the Kelvin temperature, T e is the equivalent age of concrete, k rf is the reaction rate constant at 0°C, Δt is the time interval, F is the compressive strength of concrete, and F inf is the maximum strength of concrete, A, β, a and b are fitting constants; S3 According to the chemical potential equation , the concrete reaction rate equation and equivalent age equation, determine the fitting constant β and the accumulated temperature equation , and according to the compressive strength variation curve, the fitting constants A, c and d are determined; wherein, M μf is the cumulative temperature obtained after curing for one day at the Kelvin temperature T, c and d are fitting constants; S4 predicts the strength of the concrete specimens cured under freezing conditions according to the accumulated temperature equation, and adjusts the curing strategy according to the actual curing conditions to ensure that the concrete specimens can meet the predetermined strength requirements during the winter curing process.

2. A curing method based on a concrete strength prediction model under freezing conditions according to claim 1, characterized in that: In S1, the air content of the concrete is controlled to be 4.5% v / v, the water-cement ratio is 30-60wt%, the slump is 180-600mm, the cement is ordinary Portland cement and / or fly ash Portland cement, the coarse aggregate is Toma gravel, the fine aggregate is Toma river sand, and the admixture is polycarboxylate water reducer and / or lignin sulfonate water reducer.

3. The curing method based on the concrete strength prediction model under freezing conditions according to claim 2 is characterized in that: In S1, the density of ordinary Portland cement is 3.17 g / m 3 , with a specific surface area of ​​3450cm 2 / g, C3S content is 59.6wt%, C2S content is 15.6wt%, C3A content is 8.5wt%, and C4AF content is 9.1wt%.

4. The curing method based on the concrete strength prediction model under freezing conditions according to claim 2 is characterized in that: In S1, the density of cement in fly ash silicate cement is 3.16 g / m 3 , with a specific surface area of ​​3460cm 2 / g, C3S content is 59.3wt%, C2S content is 15.1wt%, C3A content is 9.6wt%, C4AF content is 8.6wt%; the fly ash content in fly ash silicate cement is 15wt%, the ignition loss is 1.7%, the SiO2 content is 68.6wt%, the water content is 0.15wt%, and the density is 2.11g / m 3 , with a specific surface area of ​​3890cm 2 / g.

5. The curing method based on the concrete strength prediction model under freezing conditions according to claim 2 is characterized in that: In S1, the saturated surface dry density of the Toma River sand is 2.58 g / cm 3 The water absorption coefficient is 2.50%; the surface density of Toma gravel in dry saturated state is 2.88g / cm 3 , the water absorption coefficient is 1.88%.

6. The curing method based on the concrete strength prediction model under freezing conditions according to claim 2 is characterized in that: In S1, concrete specimens with different water-cement ratios are respectively subjected to constant temperature curing at 5-35°C and low temperature curing at -1-10°C until a predetermined age, and the compressive strength of the cured concrete specimens is measured; wherein, the low temperature curing is performed by pre-curing at 10°C to 5-10 MPa for 2 days, and then curing at -1-10°C.

7. The curing method based on the concrete strength prediction model under freezing conditions according to claim 6 is characterized in that: In S2, cement is ordinary Portland cement, the apparent activation energy E is 44350 J / mol, the fitting constant a is -11.91, and the fitting constant b is -1.

01.

8. The curing method based on the concrete strength prediction model under freezing conditions according to claim 6 is characterized in that: In S2, the cement is fly ash silicate cement, the apparent activation energy E is 40319 J / mol, the fitting constant a is -7.91, and the fitting constant b is -1.

30.

9. The curing method based on the concrete strength prediction model under freezing conditions according to claim 6, characterized in that: In S3, cement is ordinary Portland cement, the fitting constant A is 43.1, the fitting constant β is 10.0, the fitting constant c is -0.60, and the fitting constant d is 0.

74.

10. The curing method based on the concrete strength prediction model under freezing conditions according to claim 6, characterized in that: In S3, the cement is fly ash silicate cement, the fitting constant A is 39.5, the fitting constant β is 9.1, the fitting constant c is -0.60, and the fitting constant d is 0.74.

Citation Information

Cited By

  • Intelligent concrete curing method based on electrical impedance

    CN120839919A

  • Intelligent concrete curing method based on electrical impedance

    CN120839919B