Double-layer negative plate, preparation method thereof and lithium ion capacitor

By using a double-layer negative electrode sheet in lithium-ion capacitors and combining with lithium cobalt oxide positive electrode sheets, the rate performance and capacity are improved, and the problem of low efficiency and insufficient power density of hard carbon in lithium-ion batteries is solved. Meets the needs of high-power applications.

CN118942927AActive Publication Date: 2024-11-12GUIZHOU MEILING POWER SUPPLY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411361549.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-12
Estimated Expiration
2044-09-27

AI Technical Summary

Technical Problem

The first time hard carbon has low efficiency in lithium-ion batteries and insufficient power density in ultra-high-rate constant current discharge, which cannot meet the requirements of aerospace, military and high power.

Method used

By using the preparation method of a double-layer negative electrode sheet, two layers of negative electrode slurry A and negative electrode slurry B of different components are coated on the copper current collector, and dried and rolled to form a double-layer negative electrode sheet, combined with cobalt The lithium-earth positive electrode sheet is assembled into a lithium-ion capacitor to improve rate performance and capacity.

Benefits of technology

It significantly improves the rate performance and capacity of lithium-ion capacitors, solves the problems of low first-term efficiency and insufficient power density of hard carbon, and meets the usage requirements in aerospace, military and high power fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942927A_ABST
    Figure CN118942927A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a double-layer negative plate in the field of energy storage equipment. The preparation process comprises three main steps: firstly, preparing negative electrode slurry A, uniformly stirring and mixing hard carbon, conductive carbon black, natural graphite, single-walled carbon nanotube dispersion liquid and polyvinylidene fluoride according to a specific mass ratio in a drying room with the dew point of-30 to-40 DEG C, then adding 1-methyl-2-pyrrolidone, and uniformly stirring; secondly, negative electrode slurry B is prepared, the process is similar to that of A, but an HL mixture (hard carbon and lithium cobalt nitride are uniformly mixed according to a specific proportion) is used for replacing part of hard carbon; and finally, preparing a double-layer negative electrode plate, firstly coating a layer of negative electrode slurry A or B on two sides of a copper current collector, drying for the first time, then coating another layer of negative electrode slurry A or B, drying for the second time, and finally rolling and slitting to obtain the double-layer negative electrode plate. The design of the double-layer negative plate aims to solve the problems of low initial efficiency of hard carbon and insufficient power density during ultrahigh-rate constant-current discharge.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of energy storage equipment, and in particular relates to a double-layer negative electrode sheet and a preparation method thereof, and a lithium ion capacitor. Background Art

[0002] Lithium-ion capacitors have the advantages of high specific energy and power performance, good rate discharge capability, low self-discharge rate, wide operating temperature range and good cycle life, and have been widely used in the field of military equipment. For example, in high-power microwave weapons, lithium-ion capacitors have been used as the main power source for microwave weapon launch to maintain high energy density and power density. With the development of related military equipment technology, the energy storage power supply required to be configured has the characteristics of high specific energy, high power, high safety and reliability, and wide operating temperature range.

[0003] The negative electrode materials of commercial lithium-ion capacitors (such as automotive lithium-ion capacitors) are mainly hard carbon (HC) and graphite. Among them, the specific capacity of hard carbon in lithium-ion batteries can reach about 1000mAh / g, which is almost three times that of graphite. In addition, due to the 3D ion transfer path in the structure, the rate performance of hard carbon is much better than that of graphite. The negative electrode of hard carbon shows a low potential platform at ≤0.2V (relative to Li + / Li), which enables them to provide high power density in lithium-ion batteries. However, the first coulombic efficiency (ICE) of hard carbon is generally around 70%, and even lower for those with high specific surface area.

[0004] In view of the above technical problems, the patent with application publication number "CN 114899354 A" discloses a multilayer negative electrode sheet, its preparation method and secondary battery; the multilayer negative electrode sheet in the patent includes an ultra-thin bottom coating coated on the surface of the current collector, a first coating layer coated on the surface of the ultra-thin bottom coating layer and a second coating layer coated on the surface of the first coating layer, wherein the first coating layer includes a first active material, the first active material is graphite, soft carbon or hard carbon; the second coating layer includes a second active material, the second active material is graphite, soft carbon or hard carbon; the ultra-thin bottom coating layer includes a third active material, and the third active material is carbon nanotubes. The multilayer negative electrode sheet provided by the patent has both high energy load and fast ion transfer performance, which not only improves the energy density of the battery, but also effectively prevents the battery from lithium deposition, improves the battery safety performance, cycle performance and rate performance; however, the high rate discharge performance of the lithium ion battery based on the multilayer negative electrode sheet is poor and the first coulomb is low, which makes it impossible to meet the requirements of aerospace, military and high power. Summary of the invention

[0005] The present invention aims to provide a double-layer negative electrode sheet preparation method to solve the problems of low initial efficiency of hard carbon and insufficient power density under ultra-high rate constant current discharge.

[0006] A method for preparing a double-layer negative electrode sheet in this scheme comprises the following steps:

[0007] Step 1, preparation of negative electrode slurry A: hard carbon (HC), conductive carbon black (SP), natural graphite (KS-6), single-walled carbon nanotube dispersion and polyvinylidene fluoride (PVDF) are mixed in a drying room with a dew point of -30 to -40°C according to a mass ratio of (92 to 96): (2.0 to 0.82): (2.18 to 1.05): (0.18 to 0.13): (3.64 to 2.0) to obtain a kneaded material A; then 1-methyl-2-pyrrolidone (NMP) is added and stirred evenly, and the viscosity is adjusted to 3000-6000 mPa·s to obtain a negative electrode slurry A;

[0008] Step 2, preparation of negative electrode slurry B: HL mixture, conductive carbon black (SP), natural graphite (KS-6), single-walled carbon nanotube dispersion and polyvinylidene fluoride (PVDF) are stirred and mixed in a drying room with a dew point of -30 to -40 ° C according to a mass ratio of (92 to 96): (2.0 to 0.82): (2.18 to 1.05): (0.18 to 0.13): (3.64 to 2.0) to obtain a kneaded material B; then 1-methyl-2-pyrrolidone (NMP) is added and stirred evenly, and the viscosity is adjusted to 3000-6000 mPa·s to obtain a negative electrode slurry B; the HL mixture is composed of HC (hard carbon) and LCN (lithium cobalt nitride) according to m LCN / m (HC+LCN) =0~10% mass ratio and mixed evenly;

[0009] Step 3, preparation of double-layer negative electrode sheet: two layers of negative electrode slurry are coated on both sides of the copper current collector, the two layers of negative electrode slurry are negative electrode slurry A and negative electrode slurry B respectively, and the two layers of negative electrode slurry are different. If the first layer is negative electrode slurry A, the second layer is negative electrode slurry B, and vice versa; specifically: first, a layer of negative electrode slurry A or negative electrode slurry B is coated on both sides of the copper current collector, and dried for the first time at a temperature of 80-120°C; then, another layer of negative electrode slurry is coated on both sides of the copper current collector, and then dried for a second time to obtain a negative electrode coating; finally, the negative electrode coating is rolled and cut to obtain a double-layer negative electrode sheet.

[0010] Furthermore, in step one and / or step two, a vacuum mixer is used to stir and mix the materials.

[0011] Furthermore, in step three, a coating machine is used to coat the negative electrode slurry on the copper current collector.

[0012] Furthermore, in step three, the first drying time is 30 to 60 minutes.

[0013] Furthermore, in step three, vacuum drying is used during the secondary drying. Specifically, after coating another layer of negative electrode slurry on both sides of the copper current collector, vacuum drying is continuously performed in a vacuum dryer for 18 to 24 hours, and the vacuum degree is ≤-0.095Mpa.

[0014] Furthermore, in step three, a double-roller machine is used to roll the negative electrode coating.

[0015] Furthermore, in step three, a slitting machine is used to slit the negative electrode coating after rolling.

[0016] Through experimental verification, the double-layer negative electrode sheet obtained by the above preparation method is assembled into a lithium-ion capacitor with a lithium cobalt oxide positive electrode sheet, which has high rate performance and capacity, and solves the problems of low initial efficiency of hard carbon and insufficient power density under ultra-high rate constant current discharge. Therefore, this application also requests protection of the double-layer negative electrode sheet prepared by the above preparation method, and the lithium-ion capacitor containing the double-layer negative electrode sheet. The lithium-ion capacitor of this application can effectively meet the use requirements of aerospace, military and high power, and can also be used in commercial fields such as automobiles. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Scanning electron microscopy of the single-layer A electrode and the single-layer B electrode prepared in Examples 3 to 4;

[0018] Figure 2 A comparison chart of the resistivity of the lithium ion capacitor electrodes prepared in Examples 1 to 4;

[0019] Figure 3 AC impedance test diagram of the lithium ion capacitor electrode prepared in Examples 1 to 4;

[0020] Figure 4 Rate performance test diagram of lithium ion capacitors prepared in Examples 1 to 4;

[0021] Figure 5 The lithium ion capacitor prepared in Example 1 is discharged at 1600A pulse;

[0022] Figure 6 for Figure 5 A partial enlarged view of . DETAILED DESCRIPTION

[0023] The following is further described in detail through specific implementation methods:

[0024] Embodiment 1:

[0025] (1) 85.707 g of HC (hard carbon), SP (conductive carbon black), KS-6 (natural graphite), single-walled carbon nanotube dispersion, and PVDF (polyvinylidene fluoride) were weighed according to a mass ratio of 94:1.7:1.85:0.15:2.3, and the materials were stirred at 1000 r / min for 10 min in a planetary vacuum mixer in a drying room with a dew point of -35°C. 137 g of 1-methyl-2-pyrrolidone (NMP) organic solvent was added, and the mixture was stirred at 1000 r / min and 1200 r / min for 15 min and 10 min in the planetary vacuum mixer to obtain a uniform and stable negative electrode slurry A. Then, a small coating machine was used to coat the negative electrode slurry A on both sides of the copper current collector with a coating thickness of 15 μm, and the mixture was placed in an oven at 80°C and dried for 30 min to obtain an A electrode sheet;

[0026] (2) HC (hard carbon) and LCN are divided into LCN / m (HC+LCN) =5% by mass ratio, and fully mixed at 800r / min for 8min in a dry powder mixer to obtain a mixed powder material of HC and LCN (hereinafter referred to as HL mixture); 85.707g of HL mixture, SP, KS-6, single-walled carbon nanotube dispersion, and PVDF were weighed according to a mass ratio of 94:1.7:1.85:0.15:2.3, and the materials were stirred at 1000r / min for 10min in a planetary vacuum mixer in a drying room with a dew point of -35°C, and 137g of 1-Methyl-2-pyrrolidone (NMP) organic solvent, first stir at 1000r / min speed for 15min in a planetary vacuum mixer, then stir at 1200r / min speed for 10min, so as to obtain a uniform and stable negative electrode slurry B, and then use a small coating machine to coat the negative electrode slurry B on both sides of the A electrode sheet, with a coating thickness of 15μm, and place it in a 120℃ vacuum drying oven (vacuum degree -0.095Mpa, the same below) to dry for 12h to obtain the AB electrode sheet, with a total coating thickness of 30μm. Finally, use a roller machine to roll the AB negative electrode sheet to a certain thickness, and then use a slitting machine to cut the AB negative electrode coating into 300*57mm rectangular electrode sheets, that is, double-layer AB negative electrode sheets, that is, AB electrodes.

[0027] (3) Assemble the AB electrode prepared in (2) with the corresponding lithium cobalt oxide positive electrode into a soft-pack lithium ion capacitor. The entire assembly process is carried out in a dry room and the humidity is strictly controlled (dew point is -35°C, the same below). Use an electrolyte system with a volume ratio of EC:DMC:EMC of 1:1:1 containing 1 mol / L LiPF6, and an isolation membrane of NKK ceramic membrane. The lithium ion capacitor is assembled in a winding manner. After assembly, it is packaged with an 80μm aluminum-plastic mold and placed in a vacuum oven for baking at 80°C for 12 hours to remove the injection. During the assembly of the lithium ion capacitor, it is necessary to ensure that there are no operational errors, the positive and negative electrodes do not contact to cause a short circuit, and there are no bubbles between the diaphragm and the electrode. The seal is tight and the air is isolated to avoid affecting the performance of the lithium ion capacitor.

[0028] Embodiment 2:

[0029] The only difference between Example 2 and Example 1 is that during coating, the negative electrode slurry B is first coated and dried to obtain the B electrode sheet, and then the negative electrode slurry A is coated on the B electrode sheet and dried, rolled and cut to obtain a double-layer BA negative electrode sheet, i.e., a BA electrode.

[0030] Embodiment 3:

[0031] (1) 85.707 g of HC (hard carbon), SP (conductive carbon black), KS-6 (natural graphite), single-walled carbon nanotube dispersion, and PVDF (polyvinylidene fluoride) were weighed according to a mass ratio of 94:1.7:1.85:0.15:2.3, and the materials were stirred at 1000 r / min for 10 min in a planetary vacuum mixer in a drying room with a dew point of -35°C. 137 g of 1-methyl-2-pyrrolidone (NMP) organic solvent was added, and the mixture was stirred at 1000 r / min in a planetary vacuum mixer. r / min speed for 15 min, and then stir at 1200r / min speed for 10 min to obtain a uniform and stable negative electrode slurry A, and then use a small coating machine to coat the negative electrode slurry A on both sides of the copper current collector with a total coating thickness of 30μm, and place it in a 120℃ vacuum drying oven to dry for 12h to obtain a single-layer A electrode sheet, and finally use a double-roller machine to roll the single-layer A electrode sheet to a certain thickness, and then use a slitting machine to cut the single-layer electrode sheet into 300*57mm rectangular electrode sheets, i.e., single-layer A electrodes.

[0032] (2) The single-layer A electrode prepared in (1) is assembled with the corresponding lithium cobalt oxide positive electrode sheet into a soft-pack lithium ion capacitor. The entire assembly process is carried out in a dry room and the humidity is strictly controlled. An electrolyte system with a volume ratio of EC:DMC:EMC of 1:1:1 containing 1 mol / L LiPF6 is used. The isolation membrane is an NKK ceramic diaphragm. The lithium ion capacitor is assembled in a winding manner. After the assembly is completed, it is packaged with an aluminum plastic mold and placed in a vacuum oven and baked at 80°C for 12 hours to remove the injection. During the assembly of the lithium ion capacitor, it is necessary to ensure that there are no operational errors, the positive and negative electrodes do not contact to cause a short circuit, and there are no bubbles between the diaphragm and the electrode. The seal is tight and the air is isolated to avoid affecting the performance of the lithium ion capacitor.

[0033] Embodiment 4:

[0034] (1) HC (hard carbon) and LCN are divided into LCN / m (HC+LCN) =5% by mass ratio, and fully mixed at 800r / min for 8min in a dry powder mixer to obtain a mixed powder material of HC and LCN (hereinafter referred to as HL mixture); 85.707g of HL mixture, SP, KS-6, single-walled carbon nanotube dispersion, and PVDF were weighed according to a mass ratio of 94:1.7:1.85:0.15:2.3, and the materials were stirred at 1000r / min for 10min in a planetary vacuum mixer in a drying room with a dew point of -35°C, and 137g of 1-methyl-2-pyrrolidone (NMP) organic solvent was added. The agent is first stirred at a planetary vacuum mixer at a speed of 1000r / min for 15min, and then stirred at a speed of 1200r / min for 10min to obtain a uniform and stable negative electrode slurry B, and then a small coating machine is used to coat the negative electrode slurry B on both sides of the copper current collector with a total coating thickness of 30μm, and it is placed in a vacuum drying oven at 120℃ and dried for 12h to obtain a single-layer B electrode sheet, and finally a double-roll machine is used to roll the single-layer B electrode sheet to a certain thickness, and then a slitting machine is used to cut the single-layer B electrode sheet into 300*57mm rectangular electrode sheets, i.e., single-layer B electrodes.

[0035] (2) Assemble the single-layer B electrode sheet prepared in (1) and the corresponding lithium cobalt oxide positive electrode sheet into a soft-pack lithium ion capacitor. The entire assembly process is carried out in a dry room and the humidity is strictly controlled. Use an electrolyte system with a volume ratio of EC:DMC:EMC of 1:1:1 containing 1 mol / L LiPF6. The isolation membrane is an NKK ceramic diaphragm. The lithium ion capacitor is assembled in a winding manner. After assembly, it is packaged with an aluminum plastic mold and placed in a vacuum oven at 80°C for 12 hours to remove and inject liquid. During the assembly of the lithium ion capacitor, it is necessary to ensure that there are no operational errors, the positive and negative electrodes do not contact to cause a short circuit, and there are no bubbles between the diaphragm and the electrode. The seal is tight and the air is isolated to avoid affecting the performance of the lithium ion capacitor.

[0036] In Examples 1, 2 and 4, LCN is Li 2.6 Co 0.4 N.

[0037] Electrochemical performance test

[0038] The capacity of soft-pack lithium-ion capacitors was tested at a rate of 0.2C, and the charge and discharge voltage was limited to 2.5-4.2V.

[0039] The first coulombic efficiency of the lithium ion capacitors prepared in Examples 1 to 4 is shown in the following table:

[0040]

[0041] Principle: Using a multi-layer coating process, lithium supplement agents are added to the double-layer structure to form a lithium supplement layer in the vertical direction of the electrode, which not only improves the conductivity of the positive electrode, but also alleviates the serious gas production and exhaust difficulties of the lithium supplement agent. At the same time, it also constructs a thick electrode with a porosity gradient distribution and has higher conductivity. The assembled lithium-ion capacitor has a higher first efficiency and excellent electrochemical performance.

[0042] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing a double-layer negative electrode sheet, characterized in that: The following steps are involved: Step 1, preparation of negative electrode slurry A: hard carbon, conductive carbon black, natural graphite, single-walled carbon nanotube dispersion and polyvinylidene fluoride are mixed in a mass ratio of (92-96): (2.0-0.82): (2.18-1.05): (0.18-0.13): (3.64-2.0) in a drying room with a dew point of -30 to -40°C, and stirred to obtain kneaded material A; then 1-methyl-2-pyrrolidone is added and stirred evenly, and the viscosity is adjusted to 3000-6000 mPa·s to obtain negative electrode slurry A; Step 2, preparation of negative electrode slurry B: HL mixture, conductive carbon black, natural graphite, single-walled carbon nanotube dispersion and polyvinylidene fluoride are stirred and mixed in a drying room with a dew point of -30 to -40 ° C in a mass ratio of (92 to 96): (2.0 to 0.82): (2.18 to 1.05): (0.18 to 0.13): (3.64 to 2.0) to obtain kneaded material B; then 1-methyl-2-pyrrolidone (NMP) is added and stirred evenly, and the viscosity is adjusted to 3000-6000 mPa·s to obtain negative electrode slurry B; HL mixture is composed of HC and LCN according to m LCN / m (HC+LCN) =0-10% by mass ratio, LCN refers to lithium cobalt nitride, HC refers to hard carbon; Step 3, preparation of double-layer negative electrode sheet: two layers of negative electrode slurry are coated on both sides of the copper current collector, the two layers of negative electrode slurry are negative electrode slurry A and negative electrode slurry B respectively, and the two layers of negative electrode slurry are different. If the first layer is negative electrode slurry A, the second layer is negative electrode slurry B, and vice versa; specifically: first, a layer of negative electrode slurry A or negative electrode slurry B is coated on both sides of the copper current collector, and dried for the first time at a temperature of 80-120°C; then, another layer of negative electrode slurry is coated on both sides of the copper current collector, and then dried for a second time to obtain a negative electrode coating; finally, the negative electrode coating is rolled and cut to obtain a double-layer negative electrode sheet.

2. The method for preparing a double-layer negative electrode sheet according to claim 1, characterized in that: In step 1 and / or step 2, a vacuum mixer is used to stir and mix the materials.

3. The method for preparing a double-layer negative electrode sheet according to claim 2, characterized in that: In step three, a coating machine is used to coat the negative electrode slurry on the copper current collector.

4. The method for preparing a double-layer negative electrode sheet according to claim 3, characterized in that: In step 3, the first drying time is 30 to 60 minutes.

5. The method for preparing a double-layer negative electrode sheet according to claim 4, characterized in that: In step three, vacuum drying is used for secondary drying. Specifically, after coating another layer of negative electrode slurry on both sides of the copper current collector, vacuum drying is continuously performed in a vacuum dryer for 18 to 24 hours, and the vacuum degree is ≤-0.095Mpa.

6. The method for preparing a double-layer negative electrode sheet according to claim 5, characterized in that: In step three, the negative electrode coating is rolled using a double-roller machine.

7. The method for preparing a double-layer negative electrode sheet according to claim 6, characterized in that: In step three, a slitting machine is used to slit the negative electrode coating after rolling.

8. A double-layer negative electrode sheet, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.

9. A lithium ion capacitor, characterized in that: A double-layer negative electrode sheet comprising the method of claim 8.

Citation Information

Patent Citations

  • Lithium ion capacitor negative electrode material and preparation method thereof

    CN110517902A

  • Negative electrode, and electrochemical device and electronic device including same

    CN113437252A

  • Negative plate and lithium ion battery

    CN114649505A

  • Lithium supplementing method for hard carbon negative electrode of battery type capacitor and application of lithium supplementing method

    CN118299195A

  • Hard carbon-metal lithium nitride composite cathode materials and method for preparing same

    CN1877888A