Semiconductor device

By using a polycrystalline oxide semiconductor layer and an aluminum-based metal oxide layer in a semiconductor device, combined with a specific manufacturing process, the problem of abnormal characteristics caused by defects in oxide semiconductor devices was solved, achieving high mobility and stable electrical performance.

CN118943145APending Publication Date: 2024-11-12JAPAN DISPLAY INC +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410503778.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-04-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, semiconductor devices using oxide semiconductors as the channel contain many defects in the insulating layer, which cause electrons to be trapped by the defects, resulting in abnormal characteristics or changes in characteristics during reliability tests. At the same time, the oxide semiconductor layer cannot be effectively supplied to repair oxygen defects, affecting mobility.

Method used

An oxide semiconductor layer with a polycrystalline structure is used, and an aluminum-based metal oxide layer is formed on the gate insulating layer. Combined with specific manufacturing processes such as sputtering and atomic layer deposition, an insulating layer covering the oxide semiconductor layer is formed to reduce defects and provide oxygen, thereby improving mobility.

Benefits of technology

A semiconductor device with high mobility has been achieved, with linear mobility exceeding that of previous technologies under certain conditions, while maintaining high mobility performance at low voltages and reducing the impact of defects on mobility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943145A_ABST
    Figure CN118943145A_ABST
Patent Text Reader

Abstract

The invention relates to a semiconductor device. The present invention addresses the problem of achieving a semiconductor device having high mobility. The semiconductor device includes: a gate electrode; a gate insulating layer on the gate electrode; a metal oxide layer having aluminum as a main component on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; a source electrode and a drain electrode in contact with the oxide semiconductor layer from above the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode. When the voltage supplied to the gate electrode is Vg, the threshold voltage of the semiconductor device is Vth, and the capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is Cox, the linear mobility of the semiconductor device is greater than 20 cm2 / Vs when (Vg-Vth) * Cox = 5 * 10-7 C / cm2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a semiconductor device. In particular, one embodiment of the present invention relates to a semiconductor device using an oxide semiconductor as a channel. Background Art

[0002] In recent years, the development of semiconductor devices using oxide semiconductors for channels instead of amorphous silicon, low-temperature polycrystalline silicon, and single-crystal silicon has been continuously advanced (for example, Patent Documents 1 to 6). Semiconductor devices using oxide semiconductors for channels can be formed by simple structures and low-temperature processes, just like semiconductor devices using amorphous silicon for channels. Semiconductor devices using oxide semiconductors for channels are known to have higher mobility than semiconductor devices using amorphous silicon for channels.

[0003] In order to stably operate a semiconductor device using an oxide semiconductor for a channel, it is important to reduce oxygen vacancies formed in the oxide semiconductor layer by supplying oxygen to the oxide semiconductor layer in the manufacturing process of the semiconductor device. As one method of supplying oxygen to the oxide semiconductor layer, for example, a technique of forming an insulating layer covering the oxide semiconductor layer under the condition that the insulating layer contains more oxygen is disclosed.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-141338

[0007] Patent Document 2: Japanese Patent Application Publication No. 2014-099601

[0008] Patent Document 3: Japanese Patent Application Publication No. 2021-153196

[0009] Patent Document 4: Japanese Patent Application Publication No. 2018-006730

[0010] Patent Document 5: Japanese Patent Application Publication No. 2016-184771

[0011] Patent Document 6: Japanese Patent Application Publication No. 2021-108405 Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, the insulating layer formed under the condition of containing more oxygen contains more defects. Under its influence, the characteristic abnormality of the semiconductor device or the characteristic change in the reliability test occurs, which is believed to be caused by the electrons being captured by the defects. On the other hand, if an insulating layer with fewer defects is used, it is impossible to increase the oxygen contained in the insulating layer. Therefore, it is impossible to fully supply oxygen from the insulating layer to the oxide semiconductor layer. In this way, it is required to realize a structure that can repair the oxygen defects formed in the oxide semiconductor layer while reducing the defects in the insulating layer that cause the characteristic changes of the semiconductor device.

[0014] One object of one embodiment of the present invention is to realize a semiconductor device having high mobility.

[0015] Means for solving problems

[0016] A semiconductor device according to an embodiment of the present invention includes: a gate electrode; a gate insulating layer on the gate electrode; a metal oxide layer mainly composed of aluminum on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; a source electrode and a drain electrode connected to the oxide semiconductor layer from above the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode. When the voltage supplied to the gate electrode is set to Vg, the threshold voltage of the semiconductor device is set to Vth, and the electrostatic capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is set to Cox, the linear mobility is (Vg-Vth)×Cox=5×10 -7 C / cm 2 When greater than 20cm 2 / Vs.

[0017] A semiconductor device according to an embodiment of the present invention includes: a gate electrode; a gate insulating layer on the gate electrode; a metal oxide layer mainly composed of aluminum on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; a source electrode and a drain electrode connected to the oxide semiconductor layer from above the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode. When the voltage supplied to the gate electrode is set to Vg, the threshold voltage of the semiconductor device is set to Vth, and the electrostatic capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is set to Cox, the linear mobility of the semiconductor device is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When greater than 30cm 2 / Vs.

[0018] A semiconductor device according to an embodiment of the present invention includes: a gate electrode; a gate insulating layer on the gate electrode; a metal oxide layer mainly composed of aluminum on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; a source electrode and a drain electrode connected to the oxide semiconductor layer from above the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode. When the voltage supplied to the gate electrode is set to Vg, the threshold voltage of the semiconductor device is set to Vth, and the electrostatic capacitance of the gate insulating layer sandwiched by the gate electrode and the oxide semiconductor layer is set to Cox, the normalized linear mobility of the semiconductor device normalized by the linear mobility when Vg=Vth is (Vg-Vth)×Cox=5×10 -7 C / cm 2 When greater than 3.0.

[0019] A semiconductor device according to an embodiment of the present invention includes: a gate electrode; a gate insulating layer on the gate electrode; a metal oxide layer on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; a source electrode and a drain electrode connected to the oxide semiconductor layer from above the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode. When the voltage supplied to the gate electrode is set to Vg, the threshold voltage of the semiconductor device is set to Vth, and the electrostatic capacitance of the gate insulating layer sandwiched by the gate electrode and the oxide semiconductor layer is set to Cox, the normalized linear mobility of the semiconductor device normalized by the linear mobility when Vg=Vth is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When greater than 4.0. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a cross-sectional view schematically showing a semiconductor device according to an embodiment of the present invention.

[0021] Figure 2 It is a plan view schematically showing a semiconductor device according to an embodiment of the present invention.

[0022] Figure 3 1 is a flowchart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0023] Figure 4 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0024] Figure 5 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0025] Figure 6 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0026] Figure 7 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0027] Figure 8 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0028] Fig. 9 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0029] Fig.10 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0030] Fig.11 This is a plan view schematically showing a display device according to an embodiment of the present invention.

[0031] Fig.12 This is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention.

[0032] Fig.13 : is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention.

[0033] Fig.14 This is a cross-sectional view schematically showing a display device according to one embodiment of the present invention.

[0034] Fig.15 It is a plan view showing a pixel electrode and a common electrode of a display device according to an embodiment of the present invention.

[0035] Fig.16 : is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention.

[0036] Fig.17 This is a cross-sectional view schematically showing a display device according to one embodiment of the present invention.

[0037] Fig.18 This is a diagram showing electrical characteristics of a semiconductor device according to an embodiment of the present invention.

[0038] Fig.19 This is a graph showing the linear mobility of the semiconductor device according to one embodiment of the present invention.

[0039] Fig. 20This is a diagram showing the dependence of the electrical characteristics of the semiconductor device according to one embodiment of the present invention on the gate capacitance.

[0040] Fig.21 This is a diagram showing the dependence of the electrical characteristics of the semiconductor device according to one embodiment of the present invention on the gate capacitance.

[0041] Fig. 22 This is a diagram showing the dependence of the linear mobility of the semiconductor device according to one embodiment of the present invention on the gate capacitance.

[0042] Fig.23 For the general Fig. 20 The horizontal axis is normalized by the threshold voltage and gate capacitance.

[0043] Fig.24 For the general Fig.21 The horizontal axis is normalized by the threshold voltage and gate capacitance.

[0044] Fig.25 For the general Fig. 22 The horizontal axis is normalized by the threshold voltage and gate capacitance.

[0045] Fig.26 This is a diagram showing the dependence of the normalized linear mobility of the semiconductor device according to one embodiment of the present invention on the gate capacitance.

[0046] Description of Reference Numerals

[0047] 10: semiconductor device, 11: driving transistor, 12: selecting transistor, 20: display device, 22: liquid crystal region, 24: sealing region, 26: terminal region, 100: substrate, 105: gate electrode, 109: wiring, 110, 120: gate insulating layer, 111: contact hole, 130: metal oxide layer, 140: oxide semiconductor layer, 150, 160: insulating layer, 190: metal oxide layer, 200: source-drain electrode, 201: source electrode, 203: drain electrode, 209: wiring, 210: storage capacitor, 211: signal line, 212: gate line, 213: anode power line, 214: cathode power line , 300: array substrate, 301: pixel circuit, 302: source driving circuit, 303: gate driving circuit, 304: source wiring, 305: gate wiring, 306: terminal portion, 307: connection wiring, 310: sealing portion, 311: liquid crystal element, 320: opposing substrate, 330: flexible printed circuit substrate, 340: IC chip, 350: holding capacitor element, 360: insulating layer, 362: insulating layer, 363: opening, 370: common electrode, 380: insulating layer, 381: opening, 382: opening, 390: pixel electrode, 392: light-emitting layer, 394: common electrode, 395: electrode, DO: light-emitting element DETAILED DESCRIPTION

[0048] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings. The following disclosure is only an example. The configuration that can be easily thought of by those skilled in the art by appropriately changing the configuration of the embodiment while maintaining the gist of the invention is of course included in the scope of the present invention. With respect to the accompanying drawings, in order to make the description clearer, the width, thickness, shape, etc. of each part are sometimes schematically indicated compared to the actual method. However, the shape shown in the figure is only an example and does not limit the interpretation of the present invention. In this specification and each figure, the same figure mark is marked for the same elements as those described before with respect to the figures that have appeared, and the detailed description is sometimes appropriately omitted.

[0049] In various embodiments of the present invention, the direction from the substrate toward the oxide semiconductor layer is referred to as up or above. Conversely, the direction from the oxide semiconductor layer toward the substrate is referred to as down or below. In this way, for the sake of convenience, the above or below phrases are used for description, but, for example, the up-and-down relationship between the substrate and the oxide semiconductor layer may be configured in a manner opposite to that shown in the figure. In the following description, for example, the oxide semiconductor layer on the substrate is only used to illustrate the up-and-down relationship between the substrate and the oxide semiconductor layer as described above, and other components may be configured between the substrate and the oxide semiconductor layer. Above or below refers to the stacking order in a structure having multiple layers stacked, and in the case of a pixel electrode described as above a transistor, it may also be a positional relationship in which the transistor and the pixel electrode do not overlap when viewed from above. On the other hand, in the case of a pixel electrode described as being vertically above a transistor, it refers to a positional relationship in which the transistor and the pixel electrode overlap when viewed from above.

[0050] In the present specification, the term "film" and the term "layer" can be used interchangeably according to circumstances.

[0051] A “display device” refers to a structure that uses an electro-optical layer to display an image. For example, a term such as a display device sometimes refers to a display panel that includes an electro-optical layer, or sometimes refers to a structure in which other optical components (for example, a polarizing component, a backlight source, a touch panel, etc.) are assembled on a display unit. As long as no technical contradiction arises, the “electro-optical layer” can include a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer. Therefore, for the embodiments described later, a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer are exemplified as display devices for explanation, but the structure in this embodiment can be applied to a display device including the above-mentioned other electro-optical layers.

[0052] In this specification, unless otherwise specified, expressions such as “α includes A, B, or C”, “α includes any one of A, B, and C”, and “α includes one selected from the group consisting of A, B, and C” do not exclude the case where α includes a combination of multiple elements of A to C. In addition, the above expressions do not exclude the case where α includes other elements.

[0053] It should be noted that the following embodiments can be combined with each other as long as no technical contradiction occurs.

[0054] [1. First embodiment]

[0055] Reference Figures 1 to 10 A semiconductor device 10 according to an embodiment of the present invention will be described.

[0056] [1-1. Configuration of Semiconductor Device 10]

[0057] use Figure 1 and Figure 2 Next, a configuration of a semiconductor device 10 according to an embodiment of the present invention will be described. Figure 1 It is a cross-sectional view schematically showing a semiconductor device 10 according to an embodiment of the present invention. Figure 2 It is a plan view schematically showing a semiconductor device 10 according to an embodiment of the present invention. Figure 1 The cross-sectional view shown is similar to that along Figure 2 The cross section shown corresponds to the cross section when the line A1-A2 is cut.

[0058] like Figure 1 As shown, the semiconductor device 10 is provided above the substrate 100. The semiconductor device 10 includes a gate electrode 105, gate insulating layers 110 and 120, a metal oxide layer 130, an oxide semiconductor layer 140, a source electrode 201, a drain electrode 203, and insulating layers 150 and 160. When the source electrode 201 and the drain electrode 203 are not particularly distinguished, they are sometimes collectively referred to as source-drain electrodes 200. In this embodiment, as the semiconductor device 10, a bottom-gate transistor in which the gate electrode 105 is provided below the oxide semiconductor layer 140 is described.

[0059] In this embodiment, a bottom-gate transistor is exemplified as the semiconductor device 10 , but the semiconductor device 10 is not limited to a bottom-gate transistor. For example, the semiconductor device 10 may be a dual-gate transistor in which gate electrodes are provided both above and below the oxide semiconductor layer 140 .

[0060] The gate electrode 105 is provided on the substrate 100. The gate insulating layers 110 and 120 are provided on the substrate 100 and the gate electrode 105. The gate insulating layers 110 and 120 have a stacked structure. The metal oxide layer 130 is provided on the gate insulating layer 120. The oxide semiconductor layer 140 is provided on the metal oxide layer 130. The source electrode 201 and the drain electrode 203 are provided on the oxide semiconductor layer 140. The source electrode 201 and the drain electrode 203 are in contact with the oxide semiconductor layer 140 from above. The insulating layers 150 and 160 are provided on the oxide semiconductor layer 140, the source electrode 201 and the drain electrode 203. The insulating layers 150 and 160 have a stacked structure. The insulating layer 160 is provided on the insulating layer 150. That is, the insulating layers 150 and 160 cover the source electrode 201 and the drain electrode 203. The insulating layer 150 is in contact with the oxide semiconductor layer 140.

[0061] The oxide semiconductor layer 140 is light-transmissive and has a polycrystalline structure including a plurality of crystal grains. The oxide semiconductor layer 140 having a polycrystalline structure can be formed by using the Poly-OS (Poly-crystalline Oxide Semiconductor) technology, which will be described in detail later. The composition of the oxide semiconductor layer 140 is described below, and an oxide semiconductor having a polycrystalline structure is sometimes referred to as Poly-OS.

[0062] The crystal grain size of the crystal grains contained in the Poly-OS is, for example, 0.1 μm or more, 0.3 μm or more, or 0.5 μm or more. The crystal grain size of the crystal grains can be obtained by, for example, cross-sectional SEM observation, cross-sectional TEM observation, or electron backscattered diffraction (EBSD) method.

[0063] As described above, the crystal grains included in the Poly-OS have a crystal grain size of 0.1 μm or more. Therefore, in the oxide semiconductor layer 140 having a film thickness of 10 nm to 30 nm, there is a region including only one crystal grain along the film thickness direction in cross-sectional observation.

[0064] The film thickness of the gate insulating layer 110 is, for example, 50 nm to 500 nm, 50 nm to 400 nm, 50 nm to 300 nm, 50 nm to 150 nm, or 50 nm to 100 nm. The film thickness of the gate insulating layer 120 is, for example, 10 nm to 200 nm, or 10 nm to 100 nm. The total film thickness of the gate insulating layers 110 and 120 is, for example, 100 nm to 700 nm, 100 nm to 500 nm, 100 nm to 400 nm, 100 nm to 250 nm, 100 nm to 200 nm, or 100 nm to 150 nm.

[0065] The thickness of the metal oxide layer 130 is, for example, not less than 1 nm and not more than 10 nm, or not less than 1 nm and not more than 5 nm. In the present embodiment, aluminum oxide is used as the metal oxide layer 130. Aluminum oxide has a high barrier property to gases such as oxygen and hydrogen. The so-called barrier property refers to the function of inhibiting the permeation of gases such as oxygen and hydrogen through aluminum oxide. That is, even if gases such as oxygen and hydrogen are released from a layer disposed under the aluminum oxide film, the gas will not move to the layer disposed above the aluminum oxide film. Alternatively, even if gases such as oxygen and hydrogen are released from a layer disposed above the aluminum oxide film, the gas will not move to the layer disposed under the aluminum oxide film.

[0066] The oxide semiconductor layer 140 has a thickness of 10 nm to 50 nm, 10 nm to 40 nm, or 10 nm to 30 nm. The insulating layer 150 has a thickness of 50 nm to 300 nm, 60 nm to 200 nm, or 70 nm to 150 nm.

[0067] The wiring 109 is formed in the same layer as the gate electrode 105. That is, the wiring 109 is in contact with the substrate 100 and the gate insulating layer 110 in the same manner as the gate electrode 105. The wiring 209 is formed in the same layer as the source electrode 201 and the drain electrode 203. That is, the wiring 209 is in contact with the insulating layer 150 in the same manner as the source electrode 201 and the drain electrode 203. In the region overlapping with the wiring 109, a contact hole 111 is provided in the gate insulating layers 110 and 120. The wiring 209 is connected to the wiring 109 via the contact hole 111. The wiring 109 and the wiring 209 function as gate wirings.

[0068] like Figure 2 As shown, in a plan view, the oxide semiconductor layer 140 overlaps with the gate electrode 105. The D1 direction is a direction connecting the source electrode 201 and the drain electrode 203. The D2 direction is a direction orthogonal to the D1 direction. In the semiconductor device 10, the channel region is a region where the gate electrode 105 overlaps with the oxide semiconductor layer 140, and is a region sandwiched by the source electrode 201 and the drain electrode 203. The channel length L is the length of the channel region in the D1 direction, corresponding to the length between the source electrode 201 and the drain electrode 203 in the D1 direction. The channel width W is the width of the channel region in the D2 direction, corresponding to the width of the oxide semiconductor layer 140 in the D2 direction. In a plan view, the region of the oxide semiconductor layer 140 overlapping with the source electrode 201 is the source region, and the region of the oxide semiconductor layer 140 overlapping with the drain electrode 203 is the drain region. That is, the channel region is located between the source region and the drain region.

[0069] In a plan view, the planar pattern of the metal oxide layer 130 is substantially the same as the planar pattern of the oxide semiconductor layer 140. In other words, the end of the metal oxide layer 130 is substantially consistent with the end of the oxide semiconductor layer 140. Figure 1 and Figure 2 The lower surface of the oxide semiconductor layer 140 is covered by the metal oxide layer 130 . In particular, in the semiconductor device 10 according to the present embodiment, the entire lower surface of the oxide semiconductor layer 140 is covered by the metal oxide layer 130 .

[0070] The wirings 109 and 209 extend in the direction D1. In the direction D2, the width of the wiring 109 is greater than the width of the wiring 209. A contact hole 111 is provided at the end of the wiring 209 on the opposite side of the direction D1. Figure 2, the wiring 109 and the wiring 209 are extended in the D1 direction together, but the present invention is not limited to this configuration. The wiring 209 may extend in the D1 direction across the end of the wiring 109 in the D1 direction. The width of the wiring 109 in the D2 direction may be the same as the width of the wiring 209, or may be smaller than the width of the wiring 209.

[0071] [1-2. Electrical Characteristics of Semiconductor Device 10]

[0072] The gate capacitance Cox is the electrostatic capacitance of the dielectric (gate insulating layers 110, 120 and metal oxide layer 130) provided between the oxide semiconductor layer 140 and the gate electrode 105 in a state where carriers are generated when a voltage for controlling the semiconductor device 10 to be in an on state is supplied to the gate electrode 105. Specifically, the gate capacitance Cox is calculated based on the film thickness and dielectric constant of the gate insulating layers 110, 120 and the metal oxide layer 130 in the channel region.

[0073] The semiconductor device 10 involved in this embodiment has the above-mentioned structure, so that it can obtain high linear mobility compared with the semiconductor device (conventional semiconductor device) using the oxide semiconductor (for example, an oxide semiconductor having a composition ratio of In:Ga:Zn:O=1:1:1:4 and having an amorphous structure). The so-called linear mobility refers to the mobility in the linear region in the electrical characteristics (Id-Vg characteristics) of the transistor. The linear mobility in this embodiment is the mobility calculated based on the Id-Vg characteristics of the semiconductor device 10 when the voltage between the source electrode 201 and the drain electrode 203 is 0.1V. The voltage supplied to the drain electrode 203 when 0V is supplied to the source electrode 201 is called the drain voltage Vd.

[0074] In the semiconductor device 10, the defects in the film of the oxide semiconductor layer 140 that functions as a channel are less than the defects in the film of the conventional oxide semiconductor. As a result, the mobility calculated based on the electrical characteristics of the semiconductor device 10 according to the present embodiment is higher than the mobility calculated based on the electrical characteristics of the conventional semiconductor device. In particular, in the conventional semiconductor device, high mobility cannot be obtained when the drain voltage Vd and the gate voltage Vg are low, whereas in the semiconductor device 10 according to the present embodiment, high mobility can be obtained even when the drain voltage Vd and the gate voltage Vg are low. The gate voltage Vg is a voltage supplied to the gate electrode 105.

[0075] When calculating mobility based on the electrical characteristics (Id-Vg characteristics) of a semiconductor device, the amount of defects formed in the oxide semiconductor layer and the difference in gate capacitance Cox affect the value of mobility. Therefore, it is difficult to evaluate the difference in mobility caused by the physical properties and structure of the oxide semiconductor layer.

[0076] For example, when a defect is formed in an oxide semiconductor layer of a semiconductor device, the amount of the defect affects the threshold voltage Vth in the Id-Vg characteristic of the semiconductor device. Specifically, if a voltage is supplied to the gate electrode of the semiconductor device, the defect is filled with charges excited by the channel in a small range of the gate voltage Vg. Therefore, the charge does not contribute to the drain current Id, and the rising voltage of the Id-Vg characteristic shifts to the higher voltage side compared to the original rising voltage.

[0077] The threshold voltage Vth is the gate voltage Vg when a current of “channel width W / channel length L×10 nA” flows through the semiconductor device in the Id-Vg characteristic when the drain voltage Vd is 0.1 V.

[0078] In addition, the gate capacitance Cox depends on the film thickness of the gate insulating layer and the dielectric constant of the material used as the gate insulating layer. Therefore, even when the same gate voltage Vg is supplied, the larger the gate capacitance Cox, the higher the carrier concentration generated in the channel. Therefore, when comparing the mobility under the same gate voltage, the larger the gate capacitance Cox, the more carriers are generated in the channel. Therefore, the larger the gate capacitance Cox, the higher the mobility. That is, the amount of charge accumulated in the channel changes depending on the thickness of the gate insulating layer, so there is a possibility that the mobility cannot be correctly evaluated.

[0079] As described above, in order to reduce the influence of defects formed in the oxide semiconductor layer and the influence on mobility caused by the gate capacitance Cox, in this embodiment, the measured Id-Vg characteristics are normalized based on the threshold voltage Vth and the gate capacitance Cox. Specifically, in the Id-Vg characteristics, the normalization is performed by converting the horizontal axis from "gate voltage Vg" to "(gate voltage Vg-threshold voltage Vth)×gate capacitance Cox". The gate voltage Vg×gate capacitance Cox is equivalent to the amount of charge excited by the channel.

[0080] The linear mobility in the Id-Vg characteristic standardized as described above is (Vg-Vth)×Cox=5×10 -7 C / cm 2 When greater than 20cm 2 / Vs, details will be given later. In addition, (Vg-Vth)×Cox=1×10 -6 C / cm 2 When the linear mobility is greater than 30 cm 2 / Vs.

[0081] In addition, the normalized linear mobility obtained by normalizing the linear mobility when Vg=Vth by setting (Vg-Vth)×Cox as the horizontal axis is (Vg-Vth)×Cox=5×10 -7 C / cm 2 In addition, the normalized linear mobility is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When greater than 4.0.

[0082] [1-3. Materials of Components of Semiconductor Device 10]

[0083] As the substrate 100, a glass substrate, a quartz substrate, a sapphire substrate and other rigid substrates with light transmission can be used. When the substrate 100 needs to be flexible, a substrate containing resin such as a polyimide substrate, an acrylic resin substrate, a siloxane-based substrate, a fluororesin substrate and the like can be used as the substrate 100. When a substrate containing resin is used as the substrate 100, impurities can be introduced into the above-mentioned resin in order to improve the heat resistance of the substrate 100. In particular, when the semiconductor device 10 is a top-emitting display, since the substrate 100 does not need to be transparent, impurities that deteriorate the transparency of the substrate 100 can also be used. When the semiconductor device 10 is used in an integrated circuit that is not a display device, a semiconductor substrate such as a silicon substrate, a silicon carbide substrate, a compound semiconductor substrate, or a conductive substrate such as a stainless steel substrate that is not light-transmitting can be used as the substrate 100.

[0084] As the gate electrode 105, the source-drain electrode 200, and the wirings 109 and 209, a common metal material can be used. For example, as the above-mentioned members, for example, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys or compounds thereof can be used. As the gate electrode 105, the source-drain electrode 200, and the wirings 109 and 209, the above-mentioned materials can be used as a single layer or as a stacked layer.

[0085] As the gate insulating layers 110, 120 and the insulating layers 150, 160, a common insulating material can be used. For example, as the gate insulating layer 120 and the insulating layer 150, silicon oxide (SiO x ), silicon oxide nitride (SiO x N y ), aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y) or other inorganic insulating layer containing oxygen. As the gate insulating layer 110 and the insulating layer 160, silicon nitride (SiN x ), silicon oxide nitride (SiN x O y ), aluminum nitride (AlN x ), aluminum nitride (AlN x O y ) or the like. Among them, the gate insulating layer 110 and the insulating layer 160 may use the above-mentioned inorganic insulating layer containing oxygen. The gate insulating layer 120 and the insulating layer 150 may use the above-mentioned inorganic insulating layer containing nitrogen.

[0086] As the insulating layer 150, an insulating layer having a function of releasing oxygen by heat treatment is used. That is, as the insulating layer 150, an oxide insulating layer containing excessive oxygen is used. The temperature of the heat treatment for releasing oxygen from the insulating layer 150 is, for example, 600° C. or less, 500° C. or less, 450° C. or less, or 400° C. or less. That is, the insulating layer 150 releases oxygen under the heat treatment temperature conditions performed in the manufacturing process of the semiconductor device 10 when a glass substrate is used as the substrate 100, for example.

[0087] As the gate insulating layer 120, an insulating layer with few defects can be used. For example, when the composition ratio of oxygen in the gate insulating layer 120 is compared with the composition ratio of oxygen in an insulating layer (hereinafter referred to as "another insulating layer") having the same composition as the gate insulating layer 120, the composition ratio of oxygen in the gate insulating layer 120 is closer to the stoichiometric ratio for the insulating layer than the composition ratio of oxygen in the other insulating layer. Specifically, silicon oxide (SiO x ), the composition ratio of oxygen in the silicon oxide used as the gate insulating layer 120 is closer to the stoichiometric ratio of silicon oxide than the composition ratio of oxygen in the silicon oxide used as the insulating layer 150. For example, as the gate insulating layer 120, a layer in which no defects are observed when evaluated by an electron spin resonance method (ESR) can be used.

[0088] The above SiO x N y and AlO x N y A silicon compound or an aluminum compound containing nitrogen (N) at a ratio (x>y) less than oxygen (O). SiN x O y and AlN x O y These are silicon compounds and aluminum compounds containing oxygen at a ratio smaller than that of nitrogen (x>y).

[0089] As the metal oxide layer 130, a metal oxide containing aluminum as a main component can be used. For example, aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y ) or the like. The so-called "metal oxide layer 130 mainly composed of aluminum" means that the ratio of aluminum contained in the metal oxide layer 130 is 1% or more of the entire metal oxide layer. The ratio of aluminum contained in the metal oxide layer 130 may be 5% or more and 70% or more, 10% or more and 60% or more, or 30% or more and 50% or less of the entire metal oxide layer. The above ratio may be a mass ratio or a weight ratio.

[0090] A metal oxide having semiconductor characteristics can be used as the oxide semiconductor layer 140. The oxide semiconductor layer 140 has a polycrystalline structure. The oxide semiconductor layer 140 having a polycrystalline structure can be manufactured using a Poly-OS technique.

[0091] For example, as the oxide semiconductor layer 140, an oxide semiconductor containing indium (In), gallium (Ga), zinc (Zn) and oxygen (O) can be used. For example, as the oxide semiconductor layer 140, an oxide semiconductor having a composition ratio of In:Ga:Zn:O=1:1:1:4 can be used. Among them, the oxide semiconductor containing In, Ga, Zn and O used in this embodiment is not limited to the above composition. As the oxide semiconductor, an oxide semiconductor having a composition different from that described above can also be used. For example, in order to improve mobility, an oxide semiconductor layer having an In ratio greater than that described above can be used. On the other hand, in order to increase the energy gap and reduce the influence of light irradiation, an oxide semiconductor layer having a Ga ratio greater than that described above can also be used.

[0092] For example, as an oxide semiconductor layer 140 having an In ratio greater than the above, an oxide semiconductor containing two or more metals including indium (In) may be used. In this case, in the oxide semiconductor layer 140, the ratio of the indium element to all metal elements may be 50% or more in terms of atomic ratio. As the oxide semiconductor layer 140, in addition to indium, gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconium dioxide (Zr), and lanthanide elements may be used. As the oxide semiconductor layer 140, elements other than the above may also be used.

[0093] As the oxide semiconductor layer 140, other elements may be added to the oxide semiconductor containing In, Ga, Zn and O, for example, metal elements such as Al and Sn may be added. In addition to the above-mentioned oxide semiconductors, an oxide semiconductor containing In and Ga (IGO), an oxide semiconductor containing In and Zn (IZO), an oxide semiconductor containing In, Sn and Zn (ITZO), and an oxide semiconductor containing In and W may also be used as the oxide semiconductor layer 140.

[0094] When the ratio of the indium element is large, the oxide semiconductor layer 140 is easy to crystallize. As described above, in the oxide semiconductor layer 140, by using a material in which the ratio of the indium element to all metal elements is 50% or more, the oxide semiconductor layer 140 having a polycrystalline structure can be easily obtained. As a metal element other than indium, the oxide semiconductor layer 140 preferably contains gallium. Gallium belongs to the same Group 13 element as indium. Therefore, the crystallinity of the oxide semiconductor layer 140 is not hindered by gallium, and the oxide semiconductor layer 140 has a polycrystalline structure.

[0095] The oxide semiconductor layer 140 can be formed using a sputtering method, and a detailed method for manufacturing the oxide semiconductor layer 140 will be described later. The composition of the oxide semiconductor layer 140 formed by the sputtering method depends on the composition of the sputtering target. In the case where the oxide semiconductor layer 140 has a polycrystalline structure, the composition of the sputtering target is also substantially consistent with the composition of the oxide semiconductor layer 140. In this case, the composition of the metal element of the oxide semiconductor layer 140 can be determined based on the composition of the metal element of the sputtering target.

[0096] In the case where the oxide semiconductor layer 140 has a polycrystalline structure, the composition of the oxide semiconductor layer can be determined using an X-ray diffraction (XRD) method. Specifically, based on the crystal structure and lattice constant of the oxide semiconductor layer obtained by the XRD method, the composition of the metal elements of the oxide semiconductor layer can be determined. In addition, the composition of the metal elements of the oxide semiconductor layer 140 can also be determined using fluorescent X-ray analysis or electron probe microanalyzer (EPMA) analysis. Among them, the oxygen element contained in the oxide semiconductor layer 140 will change depending on the sputtering processing conditions, etc., and therefore sometimes cannot be determined by the above method.

[0097] [1-4. Method for Manufacturing Semiconductor Device 10]

[0098] use Figures 3 to 10 A method for manufacturing the semiconductor device 10 according to an embodiment of the present invention will be described. Figure 3It is a flowchart for explaining a method for manufacturing the semiconductor device 10 according to one embodiment of the present invention. Figures 4 to 10 1 is a schematic cross-sectional view showing a method for manufacturing a semiconductor device 10 according to an embodiment of the present invention. Figure 3 The steps of the flowchart shown.

[0099] Figure 3 In step S1001 (“GE formation”), a gate electrode 105 is formed on the substrate 100 (see Figure 4 ). The wiring 109 is formed in the same step together with the gate electrode 105. The gate electrode 105 and the wiring 109 are formed by a PVD (Physical Vapor Deposition) method such as a sputtering method or a vacuum evaporation method.

[0100] Figure 3 In step S1002 (“GI formation”), gate insulating layers 110 and 120 are formed on the gate electrode 105 and the wiring 109 (see Figure 4 ). The gate insulating layers 110 and 120 are formed by CVD (Chemical Vapor Deposition) or sputtering. For example, an insulating material containing nitrogen can be used as the gate insulating layer 110. With this structure, impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140 can be blocked. An insulating material containing oxygen can be used as the gate insulating layer 120.

[0101] An oxidized insulating layer with few defects can be used as the gate insulating layer 120. In order to form an oxidized insulating layer with few defects as the insulating layer 120, the insulating layer 120 can be formed at a film forming temperature of 350°C or higher.

[0102] Figure 3 In step S1003 (“MO film formation”), a metal oxide layer 130 is formed on the gate insulating layers 110 and 120 (see Figure 5 The metal oxide layer 130 is formed by sputtering or atomic layer deposition (ALD: Atomic Layer Deposition).

[0103] As the metal oxide layer 130, a metal oxide containing aluminum as a main component is used. For example, aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y ) and other inorganic insulating layers.

[0104] Figure 3In step S1004 (“OS film formation”), an oxide semiconductor layer 140 is formed on the metal oxide layer 130 (see Figure 5 ). The oxide semiconductor layer 140 is formed by a sputtering method or an atomic layer deposition (ALD) method.

[0105] When the oxide semiconductor layer 140 is crystallized by OS annealing described later, the oxide semiconductor layer 140 after film formation and before OS annealing is preferably amorphous (a state in which the oxide semiconductor has a small amount of crystal components). That is, the film formation conditions of the oxide semiconductor layer 140 are preferably conditions under which the oxide semiconductor layer 140 immediately after film formation is not crystallized as much as possible. For example, when the oxide semiconductor layer 140 is formed by sputtering, the oxide semiconductor layer 140 is formed while controlling the temperature of the film formation object (substrate 100 and the structure formed thereon).

[0106] When a film is formed on an object to be formed by sputtering, ions generated in the plasma and atoms rebounded by the sputtering target collide with the object to be formed, so the temperature of the object to be formed rises along with the film forming process. If the temperature of the object to be formed rises during the film forming process, the oxide semiconductor layer 140 will contain crystalline components in the state just after the film is formed. If the oxide semiconductor layer 140 contains crystalline components, the crystal grain size cannot be increased by subsequent OS annealing. In order to control the temperature of the object to be formed as described above, for example, by cooling the object to be formed while forming the film, the crystalline components contained in the oxide semiconductor layer 140 can be reduced.

[0107] For example, the object to be film-formed can be cooled from the side opposite to the film-formed surface in such a manner that the temperature of the film-formed surface of the object to be film-formed (hereinafter referred to as "film-formed temperature") becomes 100°C or less, 70°C or less, 50°C or less, or 30°C or less. In particular, the film-formed temperature of the oxide semiconductor layer 140 of the present embodiment is preferably 50°C or less. By forming the oxide semiconductor layer 140 while cooling the substrate 100, an oxide semiconductor layer 140 having a small crystal component in the state just after film formation can be obtained. In the present embodiment, the oxide semiconductor layer 140 is formed at a film-formed temperature of 50°C or less, and the OS annealing described later is performed at a heating temperature of 400°C or more.

[0108] During the sputtering process, the oxide semiconductor layer 140 having an amorphous structure is formed under the condition that the oxygen partial pressure is 10% or less. If the oxygen partial pressure is high, the oxide semiconductor layer 140 immediately after the film formation will contain crystalline components due to the excess oxygen contained in the oxide semiconductor layer 140. Therefore, it is preferred to form the oxide semiconductor layer 140 under the condition of low oxygen partial pressure. The oxygen partial pressure is, for example, 1% to 5% or 2% to 4%. Under the condition that the oxygen partial pressure is less than 1%, the distribution of oxygen in the film forming device tends to become uneven. As a result, the composition of oxygen in the oxide semiconductor layer also becomes uneven, and an oxide semiconductor layer containing more crystalline components is formed, or an oxide semiconductor layer that will not crystallize even if an OS annealing process is performed later is formed.

[0109] Figure 3 In step S1005 (“OS pattern formation”), a pattern of the oxide semiconductor layer 140 is formed (see Figure 6 ). A resist mask (not shown) is formed on the oxide semiconductor layer 140, and the oxide semiconductor layer 140 is etched using the resist mask to form the pattern. As the etching of the oxide semiconductor layer 140, wet etching or dry etching can be used. As wet etching, an acidic etchant can be used for etching. As an etchant, for example, oxalic acid, PAN, sulfuric acid, hydrogen peroxide or hydrofluoric acid can be used. Using this step, a patterned oxide semiconductor layer 140 can be formed. Then, the resist mask is removed.

[0110] The formation of the patterned oxide semiconductor layer 140 (ie, patterning of the oxide semiconductor layer 140) is preferably performed before OS annealing. The oxide semiconductor layer 140 after OS annealing has high etching resistance and is therefore difficult to process by etching.

[0111] Figure 3 In step S1006 ("OS annealing"), after the patterned oxide semiconductor layer 140 is formed, the oxide semiconductor layer 140 is subjected to a heat treatment (OS annealing). In the OS annealing, the substrate 100 formed with the oxide semiconductor layer 140 is maintained at a predetermined reaching temperature for a predetermined time. The predetermined reaching temperature is between 300°C and 500°C, or between 350°C and 450°C. The holding time at the reaching temperature is between 15 minutes and 120 minutes, or between 30 minutes and 60 minutes. By performing the OS annealing, the oxide semiconductor layer 140 having an amorphous structure is crystallized to form an oxide semiconductor layer 140 having a polycrystalline structure (Poly-OS).

[0112] Figure 3In step S1007 (“MO pattern formation”), the metal oxide layer 130 formed on the entire surface of the substrate 100 is patterned (see Figure 7 ). The oxide semiconductor layer 140 that is fully crystallized by heat treatment has high etching resistance. Therefore, the metal oxide layer 130 can be etched using the crystallized oxide semiconductor layer 140 as a mask. As the etching of the metal oxide layer 130, wet etching can be used, or dry etching can be used. As wet etching, for example, diluted hydrofluoric acid (DHF) can be used. By etching the metal oxide layer 130 using the oxide semiconductor layer 140 as a mask, the photolithography process can be omitted. The process of etching the metal oxide layer 130 using the oxide semiconductor layer 140 as a mask can also be omitted.

[0113] Figure 3 In step S1008 (“contact formation”), a contact hole 111 is formed in the gate insulating layer 110, 120 (see Figure 7 ). By forming the contact hole, the upper surface of the wiring 109 is exposed. When it is not necessary to connect the wiring 209 and the wiring 109, the process of step S1008 can be omitted.

[0114] Figure 3 In step S1009 ("SD formation"), the source electrode 201, the drain electrode 203 and the wiring 209 are formed (see Figure 8 The source electrode 201 , the drain electrode 203 , and the wiring 209 are formed by sputtering, and by photolithography and etching. The wiring 209 is connected to the wiring 109 via the contact hole 111 .

[0115] As the etching of the source electrode 201, the drain electrode 203 and the wiring 209, wet etching or dry etching can be used. As wet etching, a mixed acid aluminum solution or a mixed solution of hydrogen peroxide and ammonia water (H2O2 / NH3 solution) can be used. As dry etching, a gas containing fluorine such as sulfur hexafluoride gas (SF6) or a gas containing chlorine such as chlorine gas (Cl2) can be used.

[0116] Poly-OS is excellent in etching resistance. Specifically, the etching rate of Poly-OS in the etching solution or etching gas used in the formation of the source electrode 201 and the drain electrode 203 is very small. This means that Poly-OS is hardly etched by the etching solution or etching gas. Therefore, in the semiconductor device 10, even if a conductive film is directly formed on the oxide semiconductor layer 140 and the conductive film is patterned to form the source electrode 201 and the drain electrode 203, the channel region of the oxide semiconductor layer 140 is hardly etched. As a result, the options for conductive materials that can be used as the source electrode 201, the drain electrode 203 and the wiring 209 increase. For example, even in the case where a conductive film of a stacked structure using MoW, Al, MoW or a single-layer structure of a MoW alloy is processed by wet etching in order to form the source electrode 201 and the drain electrode 203, the oxide semiconductor layer 140 can be suppressed from being reduced.

[0117] Figure 3 In step S1010 (“SiOx formation”), the insulating layer 150 is formed on the oxide semiconductor layer 140, the source electrode 201, and the drain electrode 203 (see Fig. 9 As the insulating layer 150, an insulating material containing oxygen is preferably used. For example, as the insulating layer 150, silicon oxide (SiO x ) or silicon oxide nitride (SiO x N y )wait.

[0118] The insulating layer 150 can be formed by the same film forming method as the gate insulating layers 110 and 120. In order to increase the oxygen composition ratio in the insulating layer 150, the film can be formed at a relatively low temperature (for example, a film forming temperature lower than 350° C.). In addition, after the insulating layer 150 is formed, a process of injecting oxygen into a portion of the insulating layer 150 can be performed.

[0119] Figure 3 In step S1011 (“MO film formation”), a metal oxide layer 190 is formed on the insulating layer 150 (see Fig. 9 ). The metal oxide layer 190 is formed by sputtering or atomic layer deposition (ALD).

[0120] As the metal oxide layer 190, a metal oxide containing aluminum as a main component can be used. For example, as the metal oxide layer 190, aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y) or the like. The so-called metal oxide layer with aluminum as the main component means that the ratio of aluminum contained in the metal oxide layer is more than 1% of the entire metal oxide layer 190. The ratio of aluminum contained in the metal oxide layer 190 can be more than 5% and less than 70%, more than 10% and less than 60%, or more than 30% and less than 50% of the entire metal oxide layer 190. The above ratio can be a mass ratio or a weight ratio.

[0121] The thickness of the metal oxide layer 190 is not less than 1 nm and not more than 50 nm, preferably not less than 1 nm and not more than 30 nm. As the metal oxide layer 190, aluminum oxide is preferably used. Aluminum oxide has a high barrier property against gases such as oxygen or hydrogen. Here, barrier property refers to the function of inhibiting the permeation of gases such as oxygen or hydrogen through aluminum oxide. That is, aluminum oxide has a high barrier property against gases such as oxygen or hydrogen, which means that aluminum oxide prevents gases such as oxygen or hydrogen in a layer below the aluminum oxide film from moving to a layer above the aluminum oxide film. Alternatively, aluminum oxide prevents gases such as oxygen or hydrogen in a layer above the aluminum oxide film from moving to a layer below the aluminum oxide film.

[0122] Figure 3 In step S1012 ("oxidation annealing"), a heat treatment is performed on the oxide semiconductor layer 140 while the insulating layer 150 and the metal oxide layer 190 are formed. Here, the oxidation annealing can be performed at, for example, 300° C. to 450° C. By this step, oxygen released from the insulating layer 150 is supplied to the oxide semiconductor layer 140. By providing the metal oxide layer 190 in a manner covering the substrate 100, it is possible to suppress the oxygen released from the insulating layer 150 from being released to the outside of the metal oxide layer 190.

[0123] In the process from when the oxide semiconductor layer 140 is formed to when the insulating layer 150 is formed on the oxide semiconductor layer 140, many oxygen defects are generated in the oxide semiconductor layer 140. However, by the oxidation annealing in step S1012, oxygen released from the insulating layer 150 is supplied to the oxide semiconductor layer 140, and the oxygen defects are repaired.

[0124] Figure 3 In step S1013 ("MO removal"), the metal oxide layer 190 (see Fig.10 ). The metal oxide layer 190 can be removed using, for example, diluted hydrofluoric acid (DHF).

[0125] Figure 3 In step S1014 (“SiNx film formation”), an insulating layer 160 is formed on the insulating layer 150 (see Figure 1 As the insulating layer 160, an insulating material containing nitrogen is preferably used. For example, as the insulating layer 160, silicon nitride (SiNx ) or silicon oxide nitride (SiN x O y ) etc. The insulating layer 160 can be formed by using the same film forming method as that of the gate insulating layer 110 .

[0126] Through the above steps, it is possible to produce Figure 1 A semiconductor device 10 is shown.

[0127] [2. Second embodiment]

[0128] use Figure 11 to Figure 15 A display device using a semiconductor device according to an embodiment of the present invention will be described. In the following embodiment, a circuit configuration in which the semiconductor device 10 described in the first embodiment is applied to a liquid crystal display device will be described.

[0129] [2-1. Overview of Display Device 20]

[0130] Fig.11 1 is a top view showing an overview of a display device according to an embodiment of the present invention. Fig.11 As shown, the display device 20 includes an array substrate 300, a sealing portion 310, an opposing substrate 320, a flexible printed circuit substrate 330 (FPC330), and an IC chip 340. The array substrate 300 and the opposing substrate 320 are bonded together by the sealing portion 310. In the liquid crystal region 22 surrounded by the sealing portion 310, a plurality of pixel circuits 301 are arranged in a matrix. The liquid crystal region 22 is a region that overlaps with a liquid crystal element 311 described later in a plan view.

[0131] The sealing region 24 provided with the sealing portion 310 is the region around the liquid crystal region 22. The FPC 330 is provided in the terminal region 26. The terminal region 26 is the region where the array substrate 300 is exposed from the counter substrate 320 and is provided outside the sealing region 24. The outside of the sealing region 24 refers to the region provided with the sealing portion 310 and the outside of the region surrounded by the sealing portion 310. The IC chip 340 is provided on the FPC 330. The IC chip 340 supplies a signal for driving each pixel circuit 301.

[0132] [2-2. Circuit Configuration of Display Device 20]

[0133] Fig.12 1 is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention. Fig.12As shown, a source driving circuit 302 is provided at a position adjacent to the liquid crystal region 22 in the opposite direction (column direction) of the D3 direction, and a gate driving circuit 303 is provided at a position adjacent to the liquid crystal region 22 in the D4 direction and the opposite direction (row direction). The source driving circuit 302 and the gate driving circuit 303 are provided in the above-mentioned sealing region 24. However, the region where the source driving circuit 302 and the gate driving circuit 303 are provided is not limited to the sealing region 24, and may be any region as long as it is outside the region where the pixel circuit 301 is provided.

[0134] The source wiring 304 extends from the source driver circuit 302 in the direction D3 and is connected to the plurality of pixel circuits 301 arranged in the direction D3. The gate wiring 305 extends from the gate driver circuit 303 in the direction D4 and is connected to the plurality of pixel circuits 301 arranged in the direction D4.

[0135] The terminal region 26 is provided with a terminal portion 306. The terminal portion 306 is connected to the source driver circuit 302 via a connection wiring 307. Similarly, the terminal portion 306 is connected to the gate driver circuit 303 via a connection wiring 307. By connecting the FPC 330 to the terminal portion 306, an external device connected to the FPC 330 is connected to the display device 20, and each pixel circuit 301 provided in the display device 20 is driven by a signal from the external device.

[0136] The semiconductor device 10 described in the first embodiment is used as a transistor included in the pixel circuit 301 , the source driver circuit 302 , and the gate driver circuit 303 .

[0137] [2-3. Pixel Circuit 301 of Display Device 20]

[0138] Fig.13 FIG. 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. Fig.13 As shown, the pixel circuit 301 includes a semiconductor device 10, a storage capacitor element 350, a liquid crystal element 311 and other elements. The semiconductor device 10 has a gate electrode 105, a source electrode 201 and a drain electrode 203. The gate electrode 105 is connected to the gate wiring 305. The source electrode 201 is connected to the source wiring 304. The drain electrode 203 is connected to the storage capacitor element 350 and the liquid crystal element 311. In this embodiment, for the sake of convenience of description, the electrode shown by the reference numeral "201" is called a source electrode, and the electrode shown by the reference numeral "203" is called a drain electrode, but the electrode shown by the reference numeral "201" can also function as a drain electrode, and the electrode shown by the reference numeral "203" can also function as a source electrode.

[0139] [2-4. Cross-sectional structure of display device 20]

[0140] Fig.14 FIG. 1 is a cross-sectional view of a display device according to an embodiment of the present invention. Fig.14 As shown in FIG. 1 , the display device 20 is a display device using the semiconductor device 10. In this embodiment, the semiconductor device 10 is used in the pixel circuit 301, but the semiconductor device 10 can also be used in peripheral circuits including the source driver circuit 302 and the gate driver circuit 303. In the following description, the semiconductor device 10 is used in the pixel circuit 301. Figure 1 The semiconductor device 10 shown is the same, and therefore the description thereof is omitted.

[0141] An insulating layer 360 is provided on the source electrode 201 and the drain electrode 203. A common electrode 370 provided for a plurality of pixels is provided on the insulating layer 360. An insulating layer 380 is provided on the common electrode 370. Openings 381 and 382 are provided on the insulating layers 360 and 380. A pixel electrode 390 is provided on the insulating layer 380 and inside the opening 381. The pixel electrode 390 is connected to the drain electrode 203. An electrode 395 is provided on the insulating layer 380 and inside the opening 382. The electrode 395 constitutes a holding capacitor element 350 together with the common electrode 370.

[0142] Fig.15 FIG. 1 is a top view showing a pixel electrode and a common electrode of a display device according to an embodiment of the present invention. Fig.15 As shown, the common electrode 370 has an overlapping region that overlaps with the pixel electrode 390 when viewed from above, and a non-overlapping region that does not overlap with the pixel electrode 390. When a voltage is supplied between the pixel electrode 390 and the common electrode 370, a transverse electric field is formed from the pixel electrode 390 in the overlapping region toward the common electrode 370 in the non-overlapping region. The liquid crystal molecules contained in the liquid crystal element 311 are moved by the transverse electric field, thereby determining the grayscale of the pixel.

[0143] [3. Third embodiment]

[0144] use Fig.16 and Fig.17 A display device using a semiconductor device according to an embodiment of the present invention will be described. In this embodiment, a circuit configuration in which the semiconductor device 10 described in the first embodiment is applied to an organic EL display device will be described. Fig.11 and Fig.12 The contents shown are the same, so the description is omitted.

[0145] [3-1. Pixel Circuit 301 of Display Device 20]

[0146] Fig.16 FIG. 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. Fig.16 As shown, the pixel circuit 301 includes elements such as a driving transistor 11, a selection transistor 12, a holding capacitor element 210, and a light-emitting element DO. The driving transistor 11 and the selection transistor 12 have the same structure as the semiconductor device 10. The source electrode of the selection transistor 12 is connected to the signal line 211, and the gate electrode of the selection transistor 12 is connected to the gate line 212. The source electrode of the driving transistor 11 is connected to the anode power line 213, and the drain electrode of the driving transistor 11 is connected to one end of the light-emitting element DO. The other end of the light-emitting element DO is connected to the cathode power line 214. The gate electrode of the driving transistor 11 is connected to the drain electrode of the selection transistor 12. The holding capacitor element 210 is connected to the gate electrode and the drain electrode of the driving transistor 11. A grayscale signal that determines the light intensity of the light-emitting element DO is supplied to the signal line 211. A signal for selecting a pixel row to which the grayscale signal is to be written is supplied to the gate line 212.

[0147] [3-2. Cross-sectional structure of display device 20]

[0148] Fig.17 This is a cross-sectional view of a display device according to one embodiment of the present invention. Fig.17 The display device 20 shown in FIG. Fig.14 The display device 20 shown is similar, but Fig.17 The structure above the insulating layer 360 in the display device 20 is Fig.14 The display device 20 has a different structure than the insulating layer 360. Fig.17 The display device 20 is not provided with Fig.14 The display device 20 of FIG. 1 is different in that the structure of the capacitor element 350 is different. Fig.17 The display device 20 is configured as follows: Fig.14 The description of the same structure as the display device 20 is omitted, and the differences between the two are described.

[0149] like Fig.17As shown, the display device 20 has a pixel electrode 390, a light-emitting layer 392 and a common electrode 394 included in the light-emitting element DO above the insulating layer 360. The pixel electrode 390 is arranged on the insulating layer 360 and inside the opening 381. An insulating layer 362 is arranged on the pixel electrode 390. An opening 363 is arranged in the insulating layer 362. The opening 363 corresponds to the light-emitting area. That is, the insulating layer 362 divides the pixel. The light-emitting layer 392 and the common electrode 394 are arranged on the pixel electrode 390 exposed through the opening 363. The pixel electrode 390 and the light-emitting layer 392 are arranged separately with respect to each pixel. On the other hand, the common electrode 394 is arranged in common for a plurality of pixels. The light-emitting layer 392 uses different materials corresponding to the display color of the pixel.

[0150] In the second and third embodiments, the semiconductor device described in the first embodiment is applied to a liquid crystal display device and an organic EL display device, but the semiconductor device can also be applied to display devices other than these (for example, a self-luminous display device or an electronic paper display device other than an organic EL display device). In addition, the semiconductor device can be applied to display devices ranging from small and medium-sized to large display devices without particular limitation.

[0151] Example

[0152] [Electrical Characteristics of Semiconductor Device 10]

[0153] use Figures 18 to 26 The electrical characteristics of the semiconductor device 10 according to the above-described embodiment will be described. Fig.18 It is a diagram showing the electrical characteristics (Id-Vg characteristics) of the semiconductor device according to one embodiment of the present invention. Fig.18 Each Id-Vg characteristic shown is a semi-logarithmic graph in which Id as the vertical axis is logarithmically displayed. The measurement conditions of the electrical characteristics are as follows. Fig.18 In the figure, it is shown that Figure 1 The electrical characteristics of the semiconductor device 10 shown are those in which the film thicknesses of the gate insulating layers 110 and 120 of the semiconductor device 10 are different.

[0154] [Measurement conditions]

[0155] ·Size of channel region CH: W / L=6.0 μm / 6.0 μm

[0156] Source-drain voltage: 0.1V, 10V

[0157] ·Gate voltage: -40V~+40V (Gate voltage of characteristic F is -30V~+30V)

[0158] ·Measurement environment: room temperature, dark room

[0159] Fig.18 The six electrical characteristics shown are electrical characteristics of semiconductor devices 10 having different film thicknesses of gate insulating layers 110 and 120. That is, semiconductor devices 10 showing these electrical characteristics have different gate capacitances Cox. In this embodiment, silicon nitride is used as the gate insulating layer 110, and silicon oxide is used as the gate insulating layer 120. The film thicknesses of silicon oxide / silicon nitride are indicated in the figure. Fig.18 From the upper left to the right, the film thickness is silicon oxide / silicon nitride = 100 / 400nm (characteristic A), 100 / 300nm (characteristic B), 100 / 150nm (characteristic C). Fig.18 From the lower left to the right, the film thickness is silicon oxide / silicon nitride = 50 / 150nm (characteristic D), 50 / 100nm (characteristic E), and 50 / 50nm (characteristic F).

[0160] Fig.18 The gate capacitance Cox under various film thickness conditions is indicated in . Fig.18 From the upper left to the right, the gate capacitance Cox is 1.0e-8[F / cm 2 ](Characteristic A), 1.3e-8[F / cm 2 ](Characteristic B), 1.9e-8[F / cm 2 ](Characteristic C). Similarly, from Fig.18 From the lower left to the right, the gate capacitance Cox is 2.5e-8[F / cm 2 ](Characteristic D), 3.2e-8[F / cm 2 ](Characteristic E), 4.5e-8[F / cm 2 ](Characteristic F). The gate capacitance Cox was calculated using 6.5 as the relative dielectric constant of silicon nitride and 4.1 as the relative dielectric constant of silicon oxide.

[0161] Fig.18 The solid horizontal line shown in each figure is shown in the leakage current Id of 10 -7 [A], mobility is 50 [cm 2 / Vs] scale position. For the leakage current Id, the current value changes by 1 order of magnitude for each scale. For the mobility, the value changes by 10 [cm 2 / Vs]. Fig.18 The solid vertical line shown in each figure is displayed at the position of the scale where the gate voltage is 0 [V]. The gate voltage changes in value by 10 [V] per scale.

[0162] exist Fig.18In each figure, the electrical characteristics with a leftward arrow indicate the Id-Vg characteristics of the semiconductor device 10. There are two types of Id-Vg characteristics shown in each figure. Of the two types of Id-Vg characteristics, the Id-Vg characteristic with a relatively large current (solid line) is the characteristic when the drain voltage Vd is 10V, and the Id-Vg characteristic with a relatively small current (dashed line) is the characteristic when the drain voltage Vd is 0.1V. Fig.18 In each of the figures, the characteristic with a rightward arrow indicates the mobility (linear mobility) of the semiconductor device 10 calculated from the Id-Vg characteristic when the drain voltage Vd is 0.1 V. Fig.18 As shown, good electrical properties with no particular abnormalities were obtained under almost all conditions, and the linear mobility was 30 [cm 2 / Vs] or above.

[0163] It should be noted that in the semiconductor device 10 under the condition of silicon oxide / silicon nitride = 50 / 50nm, if a voltage higher than +30V or a voltage lower than -30V is applied to the gate electrode 105, the semiconductor device 10 will be broken down. Therefore, the voltage applied to the gate electrode 105 is -30V to +30V.

[0164] Fig.19 This is a graph showing the linear mobility of a semiconductor device according to an embodiment of the present invention. Fig.19 The linear mobility shown is given by Fig.18 The maximum value of mobility obtained from the Id-Vg characteristic when the drain voltage Vd is 0.1V is shown. Fig.19 The plot indicated by "○" in the figure shows the mobility of the semiconductor device 10 according to the first embodiment. The plot indicated by "×" shows the mobility of a conventional semiconductor device as reference data.

[0165] In the semiconductor device 10 according to the first embodiment, the linear mobility tends to increase as the gate capacitance Cox increases. Under any conditions, the linear mobility of the semiconductor device 10 is greater than that of a conventional semiconductor device.

[0166] Fig. 20 and Fig.21 This is a diagram showing the dependence of the electrical characteristics of the semiconductor device according to one embodiment of the present invention on the gate capacitance. Fig. 20 This is a linear graph in which the leakage current Id (vertical axis) is linearly displayed. Fig.21 This is a semi-logarithmic graph in which the leakage current Id (vertical axis) is displayed logarithmically. Fig. 20 and Fig.21 Among the Id-Vg characteristics shown in FIG. 1 , characteristics A to F indicated by solid lines are characteristics of the semiconductor device 10 according to the first embodiment. Fig. 20 and Fig.21 In FIG. 1 , the characteristic shown by the dotted line (which roughly overlaps with the characteristic A) is the characteristic of the conventional semiconductor device (conventional characteristic) used as reference data. Fig. 20 and Fig.21 As shown, the smaller the film thickness of the gate insulating layers 110 and 120 is (the larger the gate capacitance Cox is), the steeper the rise of the Id-Vg characteristic is and the larger the current that flows is.

[0167] Fig. 22 FIG. 4 is a diagram showing the dependence of the linear mobility of a semiconductor device according to an embodiment of the present invention on the gate capacitance. Fig. 22 As shown, the linear mobility shows the same tendency as the leakage current Id in the Id-Vg characteristic, and has a tendency that the larger the film thickness of the gate insulating layers 110 and 120, the smaller the linear mobility, and the smaller the film thickness of the gate insulating layers 110 and 120, the larger the linear mobility. Under any condition, the linear mobility of the semiconductor device 10 is greater than that of a conventional semiconductor device using an oxide semiconductor.

[0168] However, as described in the first embodiment, the above-mentioned Id-Vg characteristics are affected by defects formed in the oxide semiconductor layer and the influence on mobility caused by the gate capacitance Cox. Therefore, in order to reduce these influences, the above-mentioned Id-Vg characteristics are normalized based on the threshold voltage Vth and the gate capacitance Cox. The results are shown in Figure 23 to Figure 25 Specifically, for Figure 20 to Figure 22 By converting the horizontal axis from "gate voltage Vg" to "(gate voltage Vg-threshold voltage Vth)×gate capacitance Cox [(Vg-Vth)×Cox (C / cm2)]", we get Figure 23 to Figure 25 Id-Vg characteristics and linear mobility are shown. Figure 23 to Figure 25 The characteristics A'~F' in correspond to Figure 20 to Figure 22 Characteristics A to F in.

[0169] like Figure 23 to Figure 25 As shown in FIG. 1 , by performing the standardization as described above, the influence caused by the gate capacitance Cox becomes smaller, the difference between the characteristics A' to F' in the Id-Vg characteristics and the linear mobility becomes smaller, and the difference between the characteristics A' to F' and the conventional characteristics becomes significant. Fig.25 As shown, in any case of characteristics A' to F', the linear mobility in the standardized Id-Vg characteristic is (Vg-Vth)×Cox=5×10 -7 C / cm 2 More than 20cm 2 / Vs, 25cm 2 / Vs, or 30cm 2 / Vs. In addition, the linear mobility is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When greater than 30cm 2 / Vs or 35cm 2 / Vs. The above-mentioned linear mobility value is a value that cannot be achieved by conventional characteristics.

[0170] Fig.26 This is a diagram showing the dependence of the normalized linear mobility of a semiconductor device according to one embodiment of the present invention on the gate capacitance. As described above, the normalized linear mobility is the mobility obtained by normalizing the linear mobility with (Vg-Vth)×Cox as the horizontal axis by the linear mobility when Vg=Vth. Fig.26 The normalized linear mobility shown is shown with Fig.25 The linear mobility shown in Figure 1 behaves in the same manner. In any case of characteristics A' to F', the normalized linear mobility is (Vg-Vth)×Cox=5×10 -7 C / cm 2 In addition, the normalized linear mobility is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When the value is greater than 4.0 or 4.5. The above-mentioned value of normalized linear mobility is a value that cannot be achieved by conventional characteristics.

[0171] As described above, in the semiconductor device 10 according to the first embodiment, it is possible to obtain linear mobility and normalized linear mobility that cannot be achieved in conventional semiconductor devices, regardless of the gate capacitance Cox associated with the film thickness of the gate insulating layers 110 and 120 .

[0172] As the embodiments of the present invention, the above-mentioned embodiments can be appropriately combined and implemented as long as they do not contradict each other. In addition, based on the embodiments, the scheme obtained by the technicians in this field by appropriately adding, deleting, or changing the design of the components, or the scheme obtained by adding, omitting, or changing the conditions of the process is also included in the scope of the present invention as long as it has the gist of the present invention.

[0173] Even if there are other effects different from the effects brought about by the above-mentioned embodiments, it is understood that the effects that can be clearly seen from the description of this specification or the effects that can be easily predicted by those skilled in the art are also brought about by the present invention.

Claims

1. A semiconductor device comprising: a gate electrode; a gate insulating layer on the gate electrode; A metal oxide layer mainly composed of aluminum on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; A source electrode and a drain electrode extending from above the oxide semiconductor layer and in contact with the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode, Here, when the voltage supplied to the gate electrode is Vg, The threshold voltage of the semiconductor device is Vth, When the electrostatic capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is represented by Cox, The linear mobility of the semiconductor device is (Vg-Vth)×Cox=5×10 -7 C / cm 2 When greater than 20cm 2 / Vs.

2. The semiconductor device according to claim 1, wherein: The linear mobility is (Vg-Vth)×Cox=1×10 - 6 C / cm 2 When greater than 30cm 2 / Vs.

3. A semiconductor device comprising: a gate electrode; a gate insulating layer on the gate electrode; A metal oxide layer mainly composed of aluminum on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; A source electrode and a drain electrode extending from above the oxide semiconductor layer and in contact with the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode, Here, when the voltage supplied to the gate electrode is Vg, The threshold voltage of the semiconductor device is Vth, When the electrostatic capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is represented by Cox, The linear mobility of the semiconductor device is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When greater than 30cm 2 / Vs.

4. A semiconductor device comprising: a gate electrode; a gate insulating layer on the gate electrode; A metal oxide layer mainly composed of aluminum on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; A source electrode and a drain electrode extending from above the oxide semiconductor layer and in contact with the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode, Here, when the voltage supplied to the gate electrode is Vg, The threshold voltage of the semiconductor device is Vth, When the electrostatic capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is represented by Cox, The normalized linear mobility of the semiconductor device normalized by the linear mobility when Vg=Vth is (Vg-Vth)×Cox=5×10 -7 C / cm 2 When greater than 3.

0.

5. The semiconductor device according to claim 4, wherein: The normalized linear mobility is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When greater than 4.

0.

6. A semiconductor device comprising: a gate electrode; a gate insulating layer on the gate electrode; A metal oxide layer mainly composed of aluminum on the gate insulating layer; an oxide semiconductor layer having a polycrystalline structure on the metal oxide layer; A source electrode and a drain electrode extending from above the oxide semiconductor layer and in contact with the oxide semiconductor layer; and an insulating layer on the source electrode and the drain electrode, Here, when the voltage supplied to the gate electrode is Vg, The threshold voltage of the semiconductor device is Vth, When the electrostatic capacitance of the gate insulating layer sandwiched between the gate electrode and the oxide semiconductor layer is represented by Cox, The normalized linear mobility of the semiconductor device when Vg=Vth is (Vg-Vth)×Cox=1×10 -6 C / cm 2 When greater than 4.

0.

7. The semiconductor device according to any one of claims 1 to 6, wherein: For a channel region that is a region where the gate electrode overlaps with the oxide semiconductor layer and is sandwiched by the source electrode and the drain electrode, when a length of the channel region in a first direction connecting the source electrode and the drain electrode is set to L and a width of the channel region in a second direction orthogonal to the first direction is set to W, Vth is Vg when a current of W / L×10 nA flows through the semiconductor device when the voltage between the source electrode and the drain electrode is 0.1 V.

8. The semiconductor device according to any one of claims 1 to 6, wherein: The linear mobility is obtained based on Id-Vg characteristics of the semiconductor device when the voltage between the source electrode and the drain electrode is 0.1V.

9. The semiconductor device according to any one of claims 1 to 6, wherein: The metal oxide layer includes aluminum oxide.

Citation Information

Cited By

  • Semiconductor device and semiconductor storage device

    US12349358B2