Composite positive electrode material and preparation method thereof, positive plate and secondary battery

By using the composite structure of P63mc and Pmnb crystal positive electrode materials in lithium-ion batteries, the insufficient circulation and safety performance of lithium-ion batteries under high voltage is solved, and a higher electrode compaction density and energy density are achieved.

CN118943316APending Publication Date: 2024-11-12ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410858049.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion batteries lack cycling and safety performance at high voltages, especially under voltages of 4.50V and above, the irreversible phase change and structural collapse of lithium cobalt oxide materials lead to cycle attenuation and safety risks, and the extreme sheet compaction The risk of particle crushing increases after the density increases.

Method used

The composite positive electrode material, including P63mc crystal form and Pmnb crystal form positive electrode material, is used to form a composite structure of LiMnaFe1-a-bNbPO4@LixNayCo1-zMzO2 and LixNayCo1-zMzO2 through specific particle sizes and chemical compositions, and combines the high-temperature solid phase method and Preparation by ion exchange method ensures the particle size and structural stability of the material.

Benefits of technology

Maintain good cycling and safety performance at high voltages, avoid irreversible capacity loss, alleviate structural collapse, and improve the compaction density and energy density of the pole sheet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004918576580000141
    Figure BDA0004918576580000141
  • Figure BDA0004918576580000151
    Figure BDA0004918576580000151
  • Figure BDA0004918576580000152
    Figure BDA0004918576580000152
Patent Text Reader

Abstract

The invention provides a composite positive electrode material and a preparation method thereof, a positive plate and a secondary battery, the composite positive electrode material comprises a first positive electrode active material of a P63mc crystal form and a second positive electrode active material of a Pmnb crystal form, the first positive electrode active material comprises first active particles and second active particles, the particle size of the first active particles is R1, and the particle size of the second active particles is R2; the particle size of the second active particles is R2, and the average particle size of the second positive electrode active material is R3; wherein R1, R2 and R3 meet the following relational expressions: R2 / R1 is less than or equal to 0.414, R3 / R1 is less than or equal to 0.225, and R3 / R2 is less than or equal to 0.543; compared with the prior art, the composite positive electrode material provided by the invention has good cycle performance and safety performance under the condition of high voltage of 4.50 V and above, and meanwhile, three particles with different particle sizes form three-stage grading, so that the compaction density of a pole piece can be improved, and the energy density of the pole piece is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a composite positive electrode material and a preparation method thereof, a positive electrode sheet and a secondary battery Background Art

[0002] Since its commercialization in the 1990s, lithium batteries have been widely used because of their high energy density, high charge and discharge efficiency, low self-discharge, long service life and environmental friendliness. At present, they have been applied to consumer electronics, aerospace, military, power tools and electric vehicles. With the development of technology, people have higher and higher requirements for the endurance of lithium-ion batteries in both the consumer field and the power battery field, and the development of high energy density lithium batteries has become the key. The development of high energy density lithium batteries can start from two aspects. One is to develop new high-gram capacity positive and negative electrode materials; the other is to increase the charge and discharge voltage of lithium batteries. Increasing the charge and discharge voltage of lithium batteries can simultaneously increase the mass energy density and volume energy density of lithium batteries, and can also reduce the cost of lithium batteries, which has become a hot topic of research.

[0003] For positive electrode materials, the high amount of lithium removal caused by high voltage poses a great challenge to its structural stability. As a positive electrode material with high energy density, lithium cobalt oxide has a lithium removal amount of more than 73% at a voltage above 4.50V, which will cause an irreversible phase transition from O3 to H1-3 in lithium cobalt oxide, a sharp change in unit cell parameters, and structural collapse, bringing serious cycle attenuation and safety risks. At present, the commonly used modification methods of lithium cobalt oxide are mainly to delay the phase change voltage through bulk doping and surface coating, but for higher voltages of 4.55V and above, the degree of irreversible phase change is aggravated, and the effect of delaying the phase change by doping and coating is not good. In addition, due to the drastic shrinkage of the C-axis and the collapse of the crystal structure under high lithium removal, the safety risks caused by it are minimally improved by doping and coating. On the other hand, with the increase of the compaction density of the pole piece, the pressure on the positive electrode particles increases during rolling, which greatly increases the risk of particle breakage and cycle failure.

[0004] In view of this, it is indeed necessary to provide a technical solution to the above problems. Summary of the invention

[0005] One of the purposes of the present invention is to provide a composite positive electrode material to address the deficiencies of the prior art, so as to improve the cycle and safety performance of current lithium-ion batteries under high voltage and to increase the compaction density of the electrode sheet.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A composite positive electrode material includes a first positive electrode active material of a P63mc crystal form and a second positive electrode active material of a Pmnb crystal form, wherein the first positive electrode active material includes first active particles and second active particles, the particle size of the first active particles is R1, the particle size of the second active particles is R2, and the average particle size of the second positive electrode active material is R3; wherein R1, R2 and R3 satisfy the relationship: R2 / R1≤0.414, R3 / R1≤0.225, R3 / R2≤0.543.

[0008] Preferably, the XRD diffraction pattern of the composite positive electrode material contains at least three diffraction peaks in the range of 17.8° to 22°; wherein, there is a first diffraction peak in the range of 17.8° to 18.3°, with a peak intensity of I1; there is a second diffraction peak in the range of 18.3° to 19.0°, with a peak intensity of I2; there is a third diffraction peak in the range of 19.0° to 22°, with a peak intensity of I3; the peak intensities I1, I2 and I3 of the diffraction peaks satisfy the relationship: I2>I3>I1, and I2 / (I1+I3)≥2.

[0009] Preferably, the value range of R1 is: 10μm≤R1≤20μm; the value range of R2 is: 2μm≤R2≤6μm; the value range of R3 is: 0.2μm≤R3≤3μm.

[0010] Preferably, the chemical formula of the composite positive electrode material is: LiMn a Fe 1-a-b N b PO 4 @Li x Na y Co 1-z M z O 2 , wherein M and N include at least one of Al, Mg, Ti, La, Y, Zn, Ni, Mn, Co, V, and Si elements; wherein 0≤a<0.5, 0≤b<0.02; 0.7≤x<1, 0.01<y<0.1, 0≤z<0.02.

[0011] Preferably, the first positive electrode active material is Li x Na y Co 1-z M z O, the second positive electrode active material is LiMn a Fe 1-a-b N b PO 4 ; Among them, 0≤a<0.5, 0≤b<0.02; 0.7≤x<1, 0.01<y<0.1, 0≤z<0.02.

[0012] Preferably, the mass of the first active particles of the first positive electrode active material is m1, the mass of the second active particles is m2, and the mass of the second positive electrode active material is m3, wherein m1, m2 and m3 satisfy the relationship: m1>m2>m3, m1 / m2≥4, m1 / m3≥15.

[0013] The second object of the present invention is to provide a method for preparing a positive electrode material, comprising the following steps:

[0014] S1: Mix the cobalt salt solution and the salt solution of the doping element M in a molar ratio of Co to M of (1-z):z, add an excess of the precipitant solution, stir, and filter to obtain a precipitate; sinter the precipitate at 400°C to 600°C for 6 to 12 hours to obtain (Co 1-z M z ) 3 O 4 Powder, where 0≤z<0.02;

[0015] S2:Co 1-z M z ) 3 O 4 The mixture is uniformly mixed with sodium salt in a molar ratio of Na to Co of (0.5-0.7): (1-1.2); sintered at 800-1100°C for 45-52h to obtain Na with P63mc crystal structure. n Co 1-z M z O 2 , where 0.5≤n≤0.7;

[0016] S3: Put Na n Co 1-z M z O 2 Dispersed in lithium salt solution, mixed evenly in a ratio of Li to Na molar ratio ≥5, reacted in a reactor at 140-160°C for 22-26h, filtered, rinsed with deionized water, dried, and crushed to obtain Li x Na y Co 1- z M z O 2 first active particles;

[0017] S4: Put Na n Co 1-z M z O 2 Dispersed in lithium salt solution, mixed evenly in a ratio of Li to Na molar ratio ≥5, reacted in a reactor at 140-160°C for 10-14h, filtered, rinsed with deionized water, dried, and crushed to obtain Li xNa y Co 1- z M z O 2 second active particles;

[0018] S5: The +3-valent iron salt solution, manganese salt solution, and salt solution doped with element N are mixed evenly according to the molar ratio of Mn, Fe, and N being a: (1-ab): b to form a mixed solution, and then the mixed solution is mixed with the phosphate solution according to the molar ratio of (Fe+N+Mn) to P being 1:1, and Mn is obtained by filtering. a Fe 1-a-b N b PO 4 Precipitation; then Mn a Fe 1-a-b N b PO 4 The precipitate is mixed evenly with the lithium salt so that the molar ratio of P to Li is (0.8-1):(1.2-1.4), sintered at 700-1000°C in an oxygen atmosphere for 8-12 hours, and crushed to obtain LiMn a Fe 1-a-b N b PO 4 Positive electrode active material;

[0019] S6: After mixing the materials prepared in steps S3, S4 and S5 according to a certain proportion, sintering at 700-800° C. for 5-8 hours, the composite positive electrode material is obtained.

[0020] A third object of the present invention is to provide a positive electrode sheet comprising any of the composite positive electrode materials described above.

[0021] Preferably, the compaction density of the positive electrode sheet is P≥4.25g / cm 3 .

[0022] A fourth object of the present invention is to provide a secondary battery, comprising a positive electrode sheet, a negative electrode sheet and a separator between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet described above.

[0023] Compared with the prior art, the present invention has the following beneficial effects: the composite positive electrode material provided by the present invention has good cycle performance and safety performance under the condition of high voltage of 4.50V and above, wherein the P63mc crystalline positive electrode material in the composite material has a unique LiO 6 Octahedron and CoO 6 Octahedrons are connected in the same plane, and only CoO appears at high voltage 2The slip of the layers and the arrangement of Li vacancies are highly reversible, avoiding the cycle attenuation caused by irreversible capacity loss; the Pmnb crystalline positive electrode material in the composite material can maintain a complete crystal skeleton under high lithium removal, alleviate the large volume expansion of the P63mc crystalline positive electrode material during the lithium deintercalation process, avoid structural collapse, and improve the safety performance of the composite material; then combine the two particle sizes of P63mc crystalline phase structure positive electrode material with the Pmnb crystalline phase structure positive electrode material, and the combination of three particle sizes of particles to improve the compaction density of the electrode sheet and further improve the energy density. DETAILED DESCRIPTION

[0024] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be described in further detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.

[0025] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0026] 1. Cathode materials

[0027] The first aspect of the present invention aims to provide a composite positive electrode material comprising a first positive electrode active material and a second positive electrode active material, wherein the first positive electrode active material is a P63mc crystal type, and the second positive electrode active material is a Pmnb crystal type; the first positive electrode active material comprises first active particles and second active particles, the particle size of the first active particles is R1, the particle size of the second active particles is R2, and the average particle size of the second positive electrode active material is R3; wherein R1, R2 and R3 satisfy the relationship: R2 / R1≤0.414, R3 / R1≤0.225, R3 / R2≤0.543.

[0028] Among them, the XRD diffraction spectrum of the composite positive electrode material contains at least three diffraction peaks in the range of 17.8° to 22°; among them, there is a first diffraction peak in the range of 17.8° to 18.3°, and the peak intensity is I1; there is a second diffraction peak in the range of 18.3° to 19.0°, and the peak intensity is I2; there is a third diffraction peak in the range of 19.0° to 22°, and the peak intensity is I3; the diffraction peak peak intensities I1, I2 and I3 satisfy the relationship: I2>I3>I1, and I2 / (I1+I3)≥2.

[0029] In some embodiments, the value range of R1 is: 10 μm≤R1≤20 μm; the value range of R2 is: 2 μm≤R2≤6 μm; the value range of R3 is: 0.2 μm≤R3≤3 μm.

[0030] In some embodiments, the chemical formula of the composite cathode material is: LiMn a Fe 1-a-b N b PO 4 @Li x Na y Co 1- z M z O 2 , wherein M and N include at least one of Al, Mg, Ti, La, Y, Zn, Ni, Mn, Co, V, and Si elements; wherein 0≤a<0.5, 0≤b<0.02; 0.7≤x<1, 0.01<y<0.1, 0≤z<0.02.

[0031] Wherein, the first positive electrode active material is Li x Na y Co 1-z M z O 2 , the second positive electrode active material is LiMn a Fe 1-a-b N b PO 4 ; Among them, 0≤a<0.5, 0≤b<0.02; 0.7≤x<1, 0.01<y<0.1, 0≤z<0.02.

[0032] In some embodiments, the mass of the first active particles of the first positive electrode active material is m1, the mass of the second active particles is m2, and the mass of the second positive electrode active material is m3, wherein m1, m2 and m3 satisfy the relationship: m1>m2>m3, m1 / m2≥4, m1 / m3≥15.

[0033] The second aspect of the present invention is to provide a method for preparing a positive electrode material, comprising the following steps:

[0034] S1: Mix the cobalt salt solution and the salt solution of the doping element M in a molar ratio of Co to M of (1-z):z, add an excess of the precipitant solution, stir, and filter to obtain a precipitate; sinter the precipitate at 400°C to 600°C for 6 to 12 hours to obtain (Co 1-z M z ) 3 O 4 Powder, where 0≤z<0.02;

[0035] S2:Co 1-z M z ) 3 O 4 The mixture is uniformly mixed with sodium salt in a molar ratio of Na to Co of (0.5-0.7): (1-1.2); sintered at 800-1100°C for 45-52h to obtain Na with P63mc crystal structure. n Co 1-z M z O 2 , where 0.5≤n≤0.7;

[0036] S3: Put Na n Co 1-z M z O 2 Dispersed in lithium salt solution, mixed evenly in a ratio of Li to Na molar ratio ≥5, reacted in a reactor at 140-160°C for 22-26h, filtered, rinsed with deionized water, dried, and crushed to obtain Li x Na y Co 1- z M z O 2 first active particles;

[0037] S4: Put Na n Co 1-z M z O 2 Dispersed in lithium salt solution, mixed evenly in a ratio of Li to Na molar ratio ≥5, reacted in a reactor at 140-160°C for 10-14h, filtered, rinsed with deionized water, dried, and crushed to obtain Li x Na y Co 1- z M z O 2 second active particles;

[0038] S5: The +3-valent iron salt solution, manganese salt solution, and salt solution doped with element N are mixed evenly according to the molar ratio of Mn, Fe, and N being a: (1-ab): b to form a mixed solution, and then the mixed solution is mixed with the phosphate solution according to the molar ratio of (Fe+N+Mn) to P being 1:1, and Mn is obtained by filtering. a Fe 1-a-b N b PO 4 Precipitation; then Mn a Fe 1-a-b N b PO 4The precipitate is mixed evenly with the lithium salt so that the molar ratio of P to Li is (0.8-1):(1.2-1.4), sintered at 700-1000°C in an oxygen atmosphere for 8-12 hours, and crushed to obtain LiMn a Fe 1-a-b N b PO 4 Positive electrode active material;

[0039] S6: After mixing the materials prepared in steps S3, S4 and S5 according to a certain proportion, sintering at 700-800° C. for 5-8 hours, the composite positive electrode material is obtained.

[0040] Wherein, the steps S1 and S2 adopt a high temperature solid phase method to prepare (Co 1-z M z ) 3 O 4 Precursor and Na n Co 1- z M z O 2 Steps S3 and S4 use an ion exchange method to prepare Li with a P63mc crystal structure. x Na y Co 1-z M z O 2 The first active particles and the second active particles are prepared by a high temperature solid phase method with a Pmnb crystal form of LiMn a Fe 1-a- b N b PO 4 Positive electrode active materials. Among them, the powder particles prepared by the high temperature solid phase method have no agglomeration and good filling properties, and the high temperature solid phase method has the advantages of low cost, large output, simple preparation process, etc. The ion exchange method is used to prepare the first active particles and the second active particles, which can control the particle size of the prepared materials and facilitate the formation of active particles of different particle sizes.

[0041] In some embodiments, the sintering temperature of step S1 is 400-600°C, specifically 400°C, 450°C, 500°C, 550°C, 600°C, and may include but are not limited to the temperature values ​​exemplified above; the sintering time is 6-12h, specifically 6h, 7h, 8h, 9h, 10h, 11h, 12h, and may include but are not limited to the sintering times listed above, preferably 10h.

[0042] In some embodiments, the sintering temperature of step S2 is 800℃~1100℃, specifically 800℃, 850℃, 900℃, 950℃, 1000℃, 1050℃, 1100℃, and may include but are not limited to the sintering temperatures listed above. The sintering time is 45~52h, specifically 45h, 46h, 47h, 48h, 49h, 50h, 51h, 52h, and may include but are not limited to the sintering times listed above, and is preferably 48h.

[0043] In some embodiments, the reactor temperature in step S3 is 140-160°C, specifically 140°C, 145°C, 150°C, 155°C, 160°C, and may include but is not limited to the reactor temperatures listed above, and is preferably 150°C; the reaction in the reactor is 22-26h, specifically 22h, 23h, 24h, 25h, 26h, and may include but is not limited to the reaction time listed above, and is preferably 24h.

[0044] In some embodiments, the reactor temperature in step S4 is 140-160°C, specifically 140°C, 145°C, 150°C, 155°C, 160°C, and may include but is not limited to the reactor temperatures listed above, preferably 150°C; the reaction in the reactor is 10-14h, specifically 10h, 11h, 12h, 13h, 14h, and may include but is not limited to the reaction time listed above, preferably 12h.

[0045] In some embodiments, the step S5 is sintered at 700-1000°C oxygen atmosphere for 8-12 hours, and the sintering temperature can be specifically 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, and can include but are not limited to the sintering temperatures listed above. The sintering time is 8-12 hours, and can be specifically 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, and can include but are not limited to the sintering times listed above, and is preferably 10 hours.

[0046] In some embodiments, the step S6 is sintered at 700-800°C for 5-8h, and the sintering temperature can specifically be 700°C, 750°C, 800°C, and can include but is not limited to the sintering temperatures listed above, preferably 750°C; the sintering time is 5-8h, specifically 5h, 6h, 7h, 8h, and can include but is not limited to the sintering times listed above, preferably 6h.

[0047] Wherein, in step S1, the cobalt salt solution can be one of cobalt sulfate, cobalt nitrate, cobalt chloride, and cobalt acetate, preferably cobalt sulfate; the M salt solution of the doping element can be one of aluminum sulfate and magnesium sulfate, preferably aluminum sulfate; the precipitant solution can be one of sodium carbonate and sodium hydroxide, preferably sodium carbonate. In addition, the prepared (Co 1-z M z ) 3 O 4 For powder, the value range of z is 0≤z<0.02. Excessive doping is not conducive to particle growth.

[0048] The molar ratio of Na to Co in step S2 is (0.5-0.7): (1-1.2), specifically 0.5:1, 0.5:1.1, 0.5:1.2, 0.6:1, 0.6:1.1, 0.6; 1.2, 0.7:1, 0.7:1.1, 0.7:1.2 may include but are not limited to the values ​​​​exemplified above, preferably 0.7:1, wherein the Na of the generated P63mc structure n Co 1-z M z O 2 , wherein 0.5≤n≤0.7. In steps S3-S4, the lithium salt solution may be lithium nitrate, lithium chloride, lithium carbonate, lithium acetate, preferably lithium nitrate; in addition, the molar ratio of Li to Na in steps 3 and 4 is ≥5, and may be 5, 6, 7, 8, 9, 10, 11; and may include but not be limited to the values ​​exemplified above, preferably, the molar ratio of Li / Na is 10. If the ratio of Li / Na is too low, the ion exchange efficiency will be low, affecting the performance of the battery.

[0049] In step S5, the +3-valent iron salt solution includes one of ferric chloride, ferric sulfate, and ferric nitrate, preferably ferric chloride; the manganese salt solution includes one of manganese chloride, manganese sulfate, and manganese nitrate, preferably manganese chloride; the salt solution doped with element N includes one of aluminum sulfate and magnesium sulfate, preferably aluminum sulfate; the lithium salt is in a P, Li molar ratio of (0.8-1): (1.2-1.4), specifically 0.8:1.2, 0.8:1.3, 0.8:1.4, 0.9:1.2, 0.9:1.3, 0.9:1.4, 1:1.2, 1:1.3, 1:1.4, and may include but are not limited to the above-listed values, preferably 1:1.2, and excess lithium can avoid the volatilization of Li during calcination and cause "lithium deficiency".

[0050] Compared with the traditional single positive electrode active material, the present application has two types of positive electrode materials and three types of composite positive electrode materials with different particle sizes, P63mc positive electrode material and Pmnb positive electrode material. The P63mc positive electrode material is composed of LiO6 Octahedron and CoO 6 Octahedrons are connected in the same plane, and only CoO appears at high voltage 2 The slip of the layers and the arrangement of Li vacancies are highly reversible, avoiding the cycle attenuation caused by irreversible capacity loss; the Pmnb crystalline positive electrode material can still maintain a complete crystal skeleton when de-lithiation occurs due to high voltage, thereby alleviating the large volume expansion of the P63mc crystalline positive electrode material during the de-lithiation process, avoiding structural collapse, and improving the safety performance of the composite positive electrode material; the P63mc crystalline phase structure positive electrode material is crushed into two particles with different particle sizes and matched with the Pmnb crystalline phase structure positive electrode material. The three particles with different particle sizes constitute a three-level grading, which can increase the compaction density of the electrode sheet to achieve the purpose of increasing the energy density of the electrode sheet.

[0051] 2. Positive electrode

[0052] The third aspect of the present invention provides a positive electrode sheet, comprising the positive electrode material described above, specifically comprising a positive electrode current collector and a positive electrode active material layer coated on at least one surface of the positive electrode current collector, and the positive electrode active material is the positive electrode material described in the present invention.

[0053] The positive electrode current collector can be any material suitable for use as a positive electrode current collector for lithium-ion batteries in the art. For example, the positive electrode current collector can include but is not limited to metal foil, and more specifically can include but is not limited to aluminum foil.

[0054] 3. Secondary battery

[0055] A fourth aspect of the present invention is to provide a secondary battery, comprising a positive electrode sheet, a negative electrode sheet and a separator between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet described above.

[0056] The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer coated on at least one surface of the negative electrode current collector. The negative electrode active material layer may include but is not limited to one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, silicon-based materials, tin-based materials, lithium titanate or other metals that can form alloys with lithium. Among them, the graphite can be selected from one or more of artificial graphite, natural graphite and modified graphite; the silicon-based material can be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, and silicon alloys; the tin-based material can be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. The negative electrode current collector is usually a structure or part that collects current. The negative electrode current collector can be various materials in the art that are suitable for use as a negative electrode current collector for lithium-ion batteries. For example, the negative electrode current collector can be, but is not limited to, metal foil, and more specifically, can be, but is not limited to, copper foil.

[0057] The separator can be any material suitable for lithium-ion battery separators in the art, for example, it can be a combination of one or more materials including but not limited to polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fibers.

[0058] The secondary battery also includes an electrolyte, which includes an organic solvent, an electrolyte lithium salt and an additive. The electrolyte lithium salt can be LiPF used in high temperature electrolytes. 6 and / or LiBOB; it can also be LiBF used in low temperature electrolytes 4 、LiBOB、LiPF 6 It can also be LiBF used in the overcharge-proof electrolyte 4 、LiBOB、LiPF 6 , LiTFSI; it can also be LiClO 4 、LiAsF 6 、LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2 At least one of the above. The organic solvent may be a cyclic carbonate, including PC, EC; it may also be a chain carbonate, including DFC, DMC, or EMC; it may also be a carboxylic acid ester, including MF, MA, EA, MP, etc. The additives include but are not limited to film-forming additives, conductive additives, flame retardant additives, overcharge prevention additives, and additives for controlling H in the electrolyte. 2 At least one of an additive for increasing the content of O and HF, an additive for improving low temperature performance, and a multifunctional additive.

[0059] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be described in further detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.

[0060] Example 1

[0061] The preparation method of the composite positive electrode material in this embodiment is:

[0062] 1) Cobalt sulfate solution and aluminum sulfate were mixed evenly in a molar ratio of Co to Al of 0.99:0.01, and an excess of sodium carbonate solution was added, stirred and filtered to obtain a precipitate; the precipitate was sintered at 550°C for 10 hours to obtain (Co 0.99 Al 0.01 ) 3 O 4 Powder.

[0063] 2) Co0.99 Al 0.01 ) 3 O 4 with Na 2 CO 3 The Na and Co were mixed evenly in a molar ratio of 0.7:1; the Na was sintered at 950°C for 48h to obtain a P63mc structure. 0.7 Co 0.99 Al 0.01 O 2 .

[0064] 3) Put Na 0.7 Co 0.99 Al 0.01 O 2 Dispersed in lithium nitrate solution, mixed evenly in a molar ratio of Li to Na of 10:1, reacted in a reactor at 150°C for 24 hours, filtered, rinsed with deionized water, dried, and mechanically crushed (feed frequency of 35 Hz) to obtain Li with a Dv50 of 15 μm 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Large particles.

[0065] 4) Put Na 0.7 Co 0.99 Al 0.01 O 2 Dispersed in lithium nitrate solution, mixed evenly in a molar ratio of Li to Na of 10:1, reacted in a reactor at 150°C for 12 hours, filtered, rinsed with deionized water, dried, and mechanically crushed (feed frequency of 21 Hz) to obtain Li with a Dv50 of 4 μm 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Small particles.

[0066] 5) Mix the ferric sulfate solution, manganese sulfate solution and aluminum sulfate solution in a molar ratio of Mn, Fe and Al of 0.4:0.59:0.01, then mix and precipitate in a molar ratio of (Fe+Al+Mn) to P of 1:1, and filter to obtain Mn 0.4 Fe 0.59 Al 0.01 PO 4 Precipitation; then mix it with lithium salt in a P:Li molar ratio of 1:1.2, sinter it at 850℃ in an oxygen atmosphere for 10h, and prepare LiMn with a Dv50 of 1μm by mechanical crushing (feed frequency of 15Hz). 0.4 Fe 0.59 Al 0.01 PO4 Positive electrode material.

[0067] 6) Li prepared in step 3 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Large particles, Li prepared in step 4 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Small particles and LiMn prepared in step 5 0.4 Fe 0.59 Al 0.01 PO 4 The positive electrode materials were mixed in a mass ratio of 77:19:4 and sintered at 750°C for 6h to obtain the composite positive electrode material LMFP@LCO-1.

[0068] Example 2

[0069] The difference between this embodiment and embodiment 1 is that in step (3), the feeding frequency of the mechanical crushing is adjusted from 35 Hz to 38 Hz, and Li with a Dv50 of 20 μm is prepared. 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Large particles.

[0070] The rest is the same as in Example 1 and will not be described again here.

[0071] Example 3

[0072] The difference between this embodiment and embodiment 1 is that in step (3), the feeding frequency of the mechanical crushing is adjusted from 35 Hz to 32 Hz, and Li with a Dv50 of 10 μm is prepared. 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Large particles.

[0073] The rest is the same as in Example 1 and will not be described again here.

[0074] Example 4

[0075] The difference between this embodiment and embodiment 1 is that in step (4), the feeding frequency of the mechanical crushing is adjusted from 21 Hz to 18 Hz, and Li with a Dv50 of 2 μm is prepared. 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Small particles.

[0076] The rest is the same as in Example 1 and will not be described again here.

[0077] Example 5

[0078] The difference between this embodiment and embodiment 1 is that in step (4), the feeding frequency of the mechanical crushing is adjusted from 21 Hz to 24 Hz, and Li with a Dv50 of 6 μm is prepared. 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Small particles.

[0079] The rest is the same as in Example 1 and will not be described again here.

[0080] Example 6

[0081] The difference between this embodiment and embodiment 1 is that in step (5), the feeding frequency of the mechanical crushing is adjusted from 15 Hz to 12 Hz, and the LiMn with a Dv50 of 0.2 μm is prepared. 0.4 Fe 0.59 Al 0.01 PO 4 Positive electrode material.

[0082] The rest is the same as in Example 1 and will not be described again here.

[0083] Example 7

[0084] The difference between this embodiment and embodiment 5 is that in step (5), the feeding frequency of mechanical crushing is adjusted from 15 Hz to 19 Hz, and LiMn with a Dv50 of 3 μm is prepared. 0.4 Fe 0.59 Al 0.01 PO 4 Small particles.

[0085] The rest is the same as in Example 5 and will not be described again here.

[0086] Comparative Example 1

[0087] The preparation method is:

[0088] Step 1: Mix the cobalt sulfate solution and aluminum sulfate in a molar ratio of Co to Al of 0.99:0.01, add excess sodium carbonate solution, stir and filter to obtain a precipitate; sinter the precipitate at 550°C for 10 hours to obtain (Co 0.99 Al 0.01 ) 3 O 4 Powder.

[0089] Step 2: 0.99 Al0.01 ) 3 O 4 with Na 2 CO 3 The Na and Co were mixed evenly in a molar ratio of 0.7:1; the Na was sintered at 950°C for 48h to obtain a P63mc structure. 0.7 Co 0.99 Al 0.01 O 2 .

[0090] Step 3: Add Na 0.7 Co 0.99 Al 0.01 O 2 Dispersed in lithium nitrate solution, mixed evenly in a molar ratio of Li to Na of 10:1, reacted in a reactor at 150°C for 24 hours, filtered, rinsed with deionized water, dried, and mechanically crushed (feed frequency of 35 Hz) to obtain Li with a Dv50 of 15 μm 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Positive electrode material.

[0091] Step 4: Li prepared in step 3 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 The positive electrode material was sintered at 750° C. for 6 h to obtain comparative example LCO-1.

[0092] Comparative Example 2

[0093] Step 1: Mix the cobalt sulfate solution and aluminum sulfate in a molar ratio of Co to A1 of 0.99:0.01, add excess sodium carbonate solution, stir and filter to obtain a precipitate; sinter the precipitate at 550°C for 10 hours to obtain (Co 0.99 Al 0.01 ) 3 O 4 Powder.

[0094] Step 2: 0.99 Al 0.01 ) 3 O 4 with Na 2 CO 3 The Na and Co were mixed evenly in a molar ratio of 0.7:1; the Na was sintered at 950°C for 48h to obtain a P63mc structure. 0.7 Co 0.99 Al 0.01 O 2 .

[0095] Step 3: Add Na 0.7 Co 0.99 Al 0.01 O 2 Dispersed in lithium nitrate solution, mixed evenly in a molar ratio of Li to Na of 10:1, reacted in a reactor at 150°C for 12 hours, filtered, rinsed with deionized water, dried, and mechanically crushed (feed frequency of 21 Hz) to obtain Li with a Dv50 of 4 μm 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Positive electrode material.

[0096] Step 4: Li prepared in step 3 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 The positive electrode material was sintered at 750° C. for 6 h to obtain comparative example LCO-2.

[0097] Comparative Example 3

[0098] Step 1: Mix the ferric sulfate solution, manganese sulfate solution and aluminum sulfate solution in a molar ratio of Mn, Fe and Al of 0.4:0.59:0.01, and then precipitate them in a molar ratio of (Fe+Al+Mn) to P of 1:1, and filter to obtain Mn 0.4 Fe 0.59 Al 0.01 PO 4 Precipitation; then mix it with lithium salt in a P:Li molar ratio of 1:1.2, sinter it at 850℃ in an oxygen atmosphere for 10h, and prepare LiMn with a Dv50 of 1μm by mechanical crushing (feed frequency of 15Hz). 0.4 Fe 0.59 Al 0.01 PO 4 Positive electrode material.

[0099] Step 2: LiMn prepared in step 1 0.4 Fe 0.59 Al 0.01 PO 4 The positive electrode material was sintered at 750° C. for 6 h to obtain comparative example LMFP-2.

[0100] Comparative Example 4

[0101] The difference between this comparative example and Example 1 is that in step (5), the feeding frequency of the mechanical crushing is adjusted from 15 Hz to 21 Hz, and LiMn with a Dv50 of 4 μm is prepared. 0.4 Fe0.59 Al 0.01 PO 4 Positive electrode material.

[0102] The rest is the same as in Example 1 and will not be described again here.

[0103] Comparative Example 5

[0104] The difference between this comparative example and Example 1 is that in step (5), the feeding frequency of the mechanical crushing is adjusted from 15 Hz to 19 Hz, and LiMn with a Dv50 of 3 μm is prepared. 0.4 Fe 0.59 Al 0.01 PO 4 Positive electrode material.

[0105] The rest is the same as in Example 1 and will not be described again here.

[0106] Comparative Example 6

[0107] The difference between this comparative example and Example 1 is that in step (4), the feeding frequency of the mechanical crushing is adjusted from 21 Hz to 25 Hz, and Li with a Dv50 of 7 μm is prepared. 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Small particles.

[0108] The rest is the same as in Example 1 and will not be described again here.

[0109] Comparative Example 7

[0110] The difference between this comparative example and Example 1 is that in step (6), Li 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Large particles, Li 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Small particles and LiMn 0.4 Fe 0.59 Al 0.01 PO 4 The mass ratio of the positive electrode material is 75:20:5.

[0111] The rest is the same as in Example 1 and will not be described again here.

[0112] Comparative Example 8

[0113] The difference between this comparative example and Example 1 is that in step (6), Li 0.87 Na0.13 Co 0.99 Al 0.01 O 2 Large particles, Li 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Small particles and LiMn 0.4 Fe 0.59 Al 0.01 PO 4 The mass ratio of the positive electrode material is 75:15:10.

[0114] The rest is the same as in Example 1 and will not be described again here.

[0115] Comparative Example 9

[0116] The difference between this comparative example and Example 1 is that in step (6), Li 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Large particles, Li 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 Small particles and LiMn 0.4 Fe 0.59 Al 0.01 PO 4 The mass ratio of the positive electrode material is 70:20:10.

[0117] The rest is the same as in Example 1 and will not be described again here.

[0118] The composite positive electrode material obtained in Examples 1-7 and Comparative Examples 1-9, the conductive agent, and polyvinylidene fluoride as a binder were mixed uniformly at a mass ratio of 97.9:1.3:0.8 to prepare a positive electrode slurry. 2The surface density is coated on the surface of the current collector aluminum foil, and then dried and rolled at 85°C. The prepared pole piece coated with the positive electrode active material layer on both sides of the aluminum foil is cold pressed, and the pole piece compaction density test is carried out according to the pressure of 200T and the roller gap of 150μm. The cold pressed pole pieces are assembled into lithium-ion button batteries, and the gram capacity test is carried out at 25°C, the charge and discharge conditions are 0.1C, and the charge and discharge range is 3.0V-4.58V; the 100cls cycle test is carried out at 45°C, the charge and discharge conditions are 1.0C, and the charge and discharge range is 3.0V-4.58V; the pole pieces after the gram capacity test are dried at 100°C and sent to DSC for testing. The test conditions are: 25°C~450°C, the temperature rise rate is 10K / min, and the nitrogen protective atmosphere. The specific parameters and test results of the above embodiments and comparative examples are organized into Tables 1 and 2

[0119] Table 1

[0120]

[0121]

[0122] Table 1

[0123]

[0124]

[0125] It can be seen from the test results in Table 2 above that the positive electrode active materials of two crystal forms and the composite positive electrode materials prepared by combining these two crystal forms and three particle sizes in the embodiment of the present invention can simultaneously take into account the advantages of improving battery capacity, cycle performance, safety performance and pole piece compaction density.

[0126] From the test results of the embodiments and comparative examples, the positive electrode material Li 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 The gram capacity of the second active particle is better than that of the first active particle, and the cycle stability is slightly weaker than that of the first active particle; the positive electrode material LiMn of the Pmnb crystal type 0.4 Fe 0.59 Al 0.01 PO 4 The higher the DSC peak temperature, the better the stability and the better the safety performance. 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 When the first active particle and the second active particle increase, the specific capacity of the composite material decreases slightly, the cycle performance becomes better, and the stability decreases; when LiMn 0.4 Fe0.59 Al 0.01 PO 4 As the particle size increases, the gram capacity, cycle performance and stability remain the same. 0.87 Na 0.13 Co 0.99 Al 0.01 O 2 The trend is consistent. In the comparative example, the electrode compaction density of the material with a larger particle size is low. After the three-level particle matching, the electrode compaction is significantly improved. When the three-level particle matching of Experimental Examples 1 to 7 simultaneously meets the conditions of R2 / R1≤0.414, R3 / R1≤0.225, R3 / R2≤0.543, m1 / m2≥4, m1 / m3≥15, the electrode compaction is as high as 4.25~4.35g / cm 3 In summary, the composite material prepared in Example 1 has high gram capacity, long circulation, high safety performance and high compaction density.

[0127] In summary, the present invention designs a three-level graded composite material comprising a P63mc crystalline positive electrode material and a Pmnb crystalline positive electrode material. The composite positive electrode material improves the cycle and safety performance under high voltage through two components. At the same time, the two components are designed with a three-level graded design to improve the compaction density of the electrode. Among them, the P63mc crystalline positive electrode material has high reversibility under high voltage, reducing the irreversible capacity loss; the Pmnb crystalline positive electrode material has a ... 4 Consistent with the structure of the main material, it can stabilize the crystal skeleton, avoid structural collapse, and improve safety performance. The three-level particle design of the positive electrode material with two different particle sizes of P63mc crystal phase structure and Pmnb crystal phase structure improves the compaction density of the electrode and further improves the energy density.

[0128] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. A composite positive electrode material, characterized in that: A first positive electrode active material comprising a P63mc crystal form and a second positive electrode active material comprising a Pmnb crystal form, wherein the first positive electrode active material comprises first active particles and second active particles, the particle size of the first active particles is R1, the particle size of the second active particles is R2, and the average particle size of the second positive electrode active material is R3; wherein R1, R2 and R3 satisfy the relationship: R2 / R1≤0.414, R3 / R1≤0.225, R3 / R2≤0.

543.

2. A composite positive electrode material according to claim 1, characterized in that: The XRD diffraction spectrum of the composite positive electrode material contains at least three diffraction peaks in the range of 17.8° to 22°; wherein, there is a first diffraction peak in the range of 17.8° to 18.3°, with a peak intensity of I1; there is a second diffraction peak in the range of 18.3° to 19.0°, with a peak intensity of I2; there is a third diffraction peak in the range of 19.0° to 22°, with a peak intensity of I3; the peak intensities I1, I2 and I3 of the diffraction peaks satisfy the relationship: I2>I3>I1, and I2 / (I1+I3)≥2.

3. A composite positive electrode material according to claim 1, characterized in that: The value range of R1 is: 10μm≤R1≤20μm; the value range of R2 is: 2μm≤R2≤6μm; the value range of R3 is: 0.2μm≤R3≤3μm.

4. A composite positive electrode material according to claim 1, characterized in that: The chemical formula of the composite positive electrode material is: LiMn a Fe 1-a-b N b PO4@Li x Na y Co 1-z M z O2, wherein M and N include at least one of Al, Mg, Ti, La, Y, Zn, Ni, Mn, Co, V, and Si elements; wherein 0≤a<0.5, 0≤b<0.02; 0.7≤x<1, 0.01<y<0.1, 0≤z<0.

02.

5. A composite positive electrode material according to claim 4, characterized in that: The first positive electrode active material is Li x Na y Co 1-z M z O2, the second positive electrode active material is LiMn a Fe 1-a-b N b PO4; wherein, 0≤a<0.5, 0≤b<0.02; 0.7≤x<1, 0.01<y<0.1, 0≤z<0.

02.

6. A composite positive electrode material according to claim 1, characterized in that: The mass of the first active particles of the first positive electrode active material is m1, the mass of the second active particles is m2, and the mass of the second positive electrode active material is m3, wherein m1, m2 and m3 satisfy the relationship: m1>m2>m3, m1 / m2≥4, m1 / m3≥15.

7. A method for preparing a composite positive electrode material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: Mix the cobalt salt solution and the salt solution of the doping element M in a molar ratio of Co to M of (1-z):z, add an excess of the precipitant solution, stir, and filter to obtain a precipitate; sinter the precipitate at 400°C to 600°C for 6 to 12 hours to obtain (Co 1-z M z )3O4 powder, wherein 0≤z<0.02; S2:Co 1-z M z )3O4 and sodium salt are mixed evenly in a molar ratio of Na to Co of (0.5-0.7): (1-1.2); sintered at 800-1100°C for 45-52h to obtain Na with P63mc crystal structure n Co 1-z M z O2, where 0.5≤n≤0.7; S3: Put Na n Co 1-z M z O2 is dispersed in the lithium salt solution, mixed evenly in a ratio of Li to Na molar ratio ≥5, reacted in a reactor at 140-160°C for 22-26h, filtered, rinsed with deionized water, dried, and crushed to obtain Li x Na y Co 1-z M z O2 first active particles; S4: Put Na n Co 1-z M z O2 is dispersed in the lithium salt solution, mixed evenly in a ratio of Li to Na molar ratio ≥5, reacted in a reactor at 140-160°C for 10-14h, filtered, rinsed with deionized water, dried, and crushed to obtain Li x Na y Co 1-z M z O2 second active particles; S5: The +3-valent iron salt solution, manganese salt solution, and salt solution doped with element N are mixed evenly according to the molar ratio of Mn, Fe, and N being a: (1-ab): b to form a mixed solution, and then the mixed solution is mixed with the phosphate solution according to the molar ratio of (Fe+N+Mn) to P being 1:1, and Mn is obtained by filtering. a Fe 1-a-b N b PO4 precipitation; then Mn a Fe 1-a-b N b The PO4 precipitate is mixed evenly with the lithium salt so that the molar ratio of P to Li is (0.8-1):(1.2-1.4), and then sintered at 700-1000°C in an oxygen atmosphere for 8-12 hours to obtain LiMn a Fe 1-a-b N b PO4 positive electrode active material; S6: After mixing the materials prepared in steps S3, S4 and S5 according to a certain proportion, sintering at 700-800° C. for 5-8 hours, the composite positive electrode material is obtained.

8. A positive electrode sheet, characterized in that: The composite positive electrode material comprises the composite positive electrode material according to any one of claims 1 to 6.

9. A positive electrode sheet according to claim 8, characterized in that: The compaction density of the positive electrode sheet is P≥4.25g / cm 3 .

10. A secondary battery, comprising a positive electrode sheet, a negative electrode sheet and a separator between the positive electrode sheet and the negative electrode sheet, characterized in that: The positive electrode sheet is the positive electrode sheet according to any one of claims 8 to 9.