Positive plate and application thereof
By adopting a double-layer structure positive electrode sheet design in lithium-ion batteries, combined with positive electrode active materials and MOFs, the technical difficulties of improving the efficiency and cycle life of lithium-ion batteries for the first time have been solved, achieving higher battery performance and safety.
Patent Information
- Application Number
- CN202411353686.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-12
AI Technical Summary
The first Coulomb efficiency and cycle life of existing lithium-ion batteries need to be further improved, especially the positive electrode lithium supplement technology has shortcomings in circulation performance and safety.
The positive electrode sheet design adopts a double-layer structure, wherein the first positive electrode active layer includes a positive electrode active material and MOFs, and the second positive electrode active layer includes a positive electrode active material, MOFs, lithium supplement agent and lithium supplement agent decomposition agent, by optimizing the material composition and structure Design to improve battery storage capacity and circulation performance.
It significantly improves the first Coulomb efficiency and cycle life of lithium-ion batteries, reduces gas production problems, enhances the safety of the battery and the electrolyte transmission efficiency, and extends the service life of the battery.
Smart Images

Figure CN118943346A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries and relates to a positive electrode sheet, and in particular to a positive electrode sheet and application thereof. Background Art
[0002] In recent years, the rapid development of portable electronic products, new energy vehicles, smart grids, distributed energy storage, and the Internet of Things has continuously put forward higher requirements for the performance of lithium-ion batteries, among which the improvement of battery energy density is the most urgent. Under the existing lithium-ion battery system, lithium supplementation, as one of the effective ways to improve battery energy density, has been widely studied by researchers.
[0003] At present, lithium replenishment can be divided into two categories according to the technical route: negative electrode lithium replenishment and positive electrode lithium replenishment. Among them, the negative electrode lithium replenishment technology generally directly composites lithium foil on the surface of the negative electrode sheet or mixes lithium powder with the negative electrode slurry and coats it on the negative electrode current collector. However, this lithium replenishment method has defects such as cumbersome process, harsh production environment, high risk and difficulty in controlling the uniformity of lithium replenishment, which limits its large-scale application; the positive electrode lithium replenishment technology can effectively avoid the above problems by adding lithium replenishment materials to the positive electrode material, but the battery obtained by this positive electrode lithium replenishment technology still needs to be further improved in terms of cycle performance and first coulomb efficiency.
[0004] Therefore, it is necessary to further improve the first coulombic efficiency and cycle life of lithium-ion batteries. Summary of the invention
[0005] In view of the above-mentioned defects, the present invention provides a positive electrode sheet, which can effectively improve the initial coulombic efficiency and cycle life of a lithium-ion battery.
[0006] The present invention also provides a lithium ion battery, comprising the positive electrode sheet, so the lithium ion battery has a higher first coulomb efficiency and cycle life.
[0007] The present invention provides a positive electrode sheet, comprising a positive electrode current collector, a first positive electrode active layer and a second positive electrode active layer; the first positive electrode active layer is located on at least one functional surface of the positive electrode current collector, and the second positive electrode active layer is located on a surface of the first positive electrode active layer away from the positive electrode current collector;
[0008] The first positive electrode active layer includes a first positive electrode active material and a first MOFs; the second positive electrode active layer includes a second positive electrode active material, a second MOFs, a lithium supplement agent and a lithium supplement agent decomposing agent.
[0009] Furthermore, the mass percentage of the lithium replenisher in the second positive electrode active layer is 0.5-10wt%, and / or the mass percentage of the lithium replenisher decomposition agent in the second positive electrode active layer is 0.01-1wt%.
[0010] Further, the lithium supplement decomposing agent includes at least one of metal carbides, metal oxides and transition metal nanoparticles;
[0011] Preferably, the lithium supplement decomposition agent comprises Mo 2 C, NiO, MnO 2 , lithium nickel cobalt manganese oxide, Co 3 O 4 At least one of .
[0012] Furthermore, the mass percentage of the first MOFs in the first positive electrode active layer is greater than the mass percentage of the second MOFs in the second positive electrode active layer.
[0013] Further, the ratio of the median particle size Dv50 of the lithium supplement decomposing agent to the median particle size Dv50 of the lithium supplement is 0.08-0.30;
[0014] Preferably, the median particle size Dv50 of the lithium supplement decomposition agent is 1-2 nm;
[0015] Preferably, the median particle size Dv50 of the lithium supplement is 10-20 nm.
[0016] Furthermore, the adsorption enthalpy of the first MOFs is 20-50 kJ·mol -1 , and / or, the adsorption enthalpy of the second MOFs is 20-50 kJ·mol -1 .
[0017] Further, the pore size of the first MOFs is smaller than the pore size of the second MOFs;
[0018] Preferably, the pore size of the first MOFs is 0.25-3 nm, and / or the pore length of the first MOFs is 2-100 nm;
[0019] Preferably, the pore size of the second MOFs is 0.25-3 nm, and / or the pore length of the second MOFs is 2-100 nm.
[0020] Furthermore, the pore length of the first MOFs is 2-20 nm, and / or the pore length of the second MOFs is 30-100 nm.
[0021] Furthermore, the first positive electrode active layer and the second positive electrode active layer also include a binder;
[0022] The mass percentage of the binder in the first positive electrode active layer is greater than the mass percentage of the binder in the second positive electrode active layer.
[0023] Furthermore, the ratio of the particle size of the lithium supplement agent to the pore length of the second MOFs is 0.1-0.8.
[0024] Furthermore, the positive electrode sheet satisfies Formula 1,
[0025] 2×B / M b ≤A 1 ×(C 1 +D 1 )+A 2 ×(C 2 +D 2 ) Formula 1
[0026] In Formula 1, B is the mass percentage of the lithium supplement in the second positive electrode active layer; M b A is the molar mass of the lithium supplement; 1 A is the mass percentage of the first MOFs in the first positive electrode active layer; 2 is the mass percentage of the second MOFs in the second positive electrode active layer; C 1 is the carbon dioxide gas adsorption capacity of the first MOFs; D 1 is the fluorine adsorption capacity of the first MOFs; C 2 is the carbon dioxide gas adsorption capacity of the second MOFs; D 2 is the fluorine adsorption capacity of the second MOFs;
[0027] Preferably, the A 1 is 0.08-0.5wt%, and / or, the A 2 0.01-0.07wt%;
[0028] Preferably, the C 1 0.1-6mmol·g -1 , and / or, the D 1 0.05-5mmol·g -1 , and / or, the C 2 0.1-6mmol·g -1 , and / or, the D 2 0.05-5mmol·g -1 .
[0029] The present invention also provides a lithium ion battery, comprising the positive electrode sheet described in any one of the above items.
[0030] The present invention makes the positive electrode sheet include a first positive electrode active layer and a second positive electrode active layer which are stacked in sequence, and the first positive electrode active layer includes a first positive electrode active material and a first MOFs, and the second positive electrode active layer includes a second positive electrode active material, a second MOFs, a lithium replenisher and a lithium replenisher decomposer. This can not only effectively improve the gas production problem caused by the decomposition of the lithium replenisher, but also significantly increase the battery liquid storage capacity and ensure higher cycle performance; at the same time, it can also effectively improve the lithium replenishment effect of the lithium replenisher, so that the battery has a higher first coulomb efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic structural diagram of the positive electrode sheet of the present invention.
[0032] Description of reference numerals:
[0033] 1- positive electrode current collector;
[0034] 2-first positive electrode active layer;
[0035] 3- second positive electrode active layer;
[0036] 4-a first positive electrode active material;
[0037] 5-First MOFs;
[0038] 6- a second positive electrode active material;
[0039] 7- Second MOFs;
[0040] 8-Lithium supplements;
[0041] 9-Lithium supplement decomposer. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] The first aspect of the present invention provides a positive electrode sheet, such as Figure 1 As shown, the positive electrode sheet includes a positive electrode collector 1, a first positive electrode active layer 2 and a second positive electrode active layer 3; the first positive electrode active layer 2 is located on at least one functional surface of the positive electrode collector 1, and the second positive electrode active layer 3 is located on the surface of the first positive electrode active layer 2 away from the positive electrode collector 1;
[0044] The first positive electrode active layer 2 includes a first positive electrode active material 4 and a first MOFs 5 ; the second positive electrode active layer 3 includes a second positive electrode active material 6 , a second MOFs 7 , a lithium supplement agent 8 and a lithium supplement agent decomposing agent 9 .
[0045] The "MOFs" in the present invention are metal organic framework compounds, which are coordination polymers formed by metal elements and bridging organic ligands interconnected by self-assembly.
[0046] Preferably, the chemical formula of MOFs is M 4 OB x , wherein M is a metal ion and B is an organic ligand; preferably, M comprises a +2-valent metal cation; preferably, B comprises an aromatic acid.
[0047] Preferably, M is selected from all subgroup elements from Sc to Zn, from Y to Cd, and from La to Hg; preferably, M is selected from at least one of Ti, V, Cr, Mn, Fe, Co, Cu, Zn, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Cd, Hf, Ta, W, Re, Os, Ir, Pt, Au, and Hg; preferably, M is selected from at least one of Zn, Cd, and Hg.
[0048] Preferably, B is selected from at least one of benzoic acid, terephthalic acid and trimellitic acid.
[0049] Preferably, the first MOFs and the second MOFs independently include at least one of MIL-100, MIL-101, ZIF-67, ZIF-8, MOF-5, UIO-66, HKUST-1, PCN-14, and PCN-222.
[0050] The lithium supplement decomposing agent in the present invention refers to a substance that can reduce the decomposition potential of the lithium supplement by more than 10-20% at a 1C-2C rate.
[0051] The present invention does not impose any specific restrictions on the specific type of the lithium supplement decomposing agent, and it only needs to be able to reduce the decomposition potential of the lithium supplement by more than 10-20% at a 1C-2C rate.
[0052] The lithium supplement in the present invention is preferably Li 2 O、LiO 2 , Li 2 O 2 , Li 2 C 3 O 5 、LiF、Li 2 S. Li 3 N.Li 5 FeO 4 , Li 2 NiO2 , Li 6 CoO 4 , Li 2 MnO 3 , Li 2 Mn 2 O 4 , Li 8 ZrO 6 , Li 5 V 2 (PO 4 ) 3 , Li 2 C 2 O 4 , Li 2 C 4 O 4 , Li 2 C 6 O 6 , 3,4-dihydroxybenzonitrile dilithium, Li 2 CuO 2 At least one of .
[0053] When the lithium supplement is selected from a plurality of specific compounds among the aforementioned compounds, the present invention does not specifically limit the ratio between the specific compounds.
[0054] The first MOFs and the second MOFs in the present invention may be made of the same material or different materials.
[0055] The first positive electrode active material and the second positive electrode active material in the present invention may be the same material or different materials.
[0056] The present invention does not specifically limit the chemical composition and structure of the first positive electrode active material and the second positive electrode active material.
[0057] The present invention does not specifically limit the sources of the first MOFs, the second MOFs, the first positive electrode active material, the second positive electrode active material, the lithium supplement agent, and the lithium supplement agent decomposition agent. Commercially available products or products prepared by conventional preparation methods known to those skilled in the art may be used.
[0058] The present invention makes the positive electrode active layer have a special double-layer structure. Specifically, the first positive electrode active layer 2 is located on at least one side of the positive electrode current collector 1, and the second positive electrode active layer 3 is located on the side of the first positive electrode active layer 2 away from the positive electrode current collector 1. At the same time, the first positive electrode active layer 2 includes a first positive electrode active material 4 and a first MOFs5, and the second positive electrode active layer 3 includes a second positive electrode active material 6, a second MOFs7, a lithium supplement 8 and a lithium supplement decomposer 9; wherein, the first MOFs5 and the second MOFs7 can effectively adsorb the gas (carbon dioxide and fluorine gas) generated during the decomposition of the lithium supplement 8, which can not only alleviate the battery thickness expansion caused by gas production and eliminate safety hazards; and the first MOFs5 and the second MOFs7 after adsorbing the gas can act as a buffer medium to ensure that the conductive network in the pole piece will not be broken due to the rigid contraction and expansion of the volume during the cycle, affecting the conductivity of the pole piece, thereby effectively reducing On the other hand, it can increase the storage capacity of the electrolyte in the battery. When the amount of electrolyte in the first positive electrode active layer 2 is sufficient, the electrolyte can be quickly replenished to the entire area of the electrode during the battery cycle, shortening the transportation distance of the electrolyte, increasing the penetration rate of the electrolyte, and further extending the service life of the battery; at the same time, the lithium supplement decomposition agent 9 can cooperate with the lithium supplement 8 to reduce the activation energy of the lithium release reaction of the lithium supplement 8, reduce the decomposition potential of the lithium supplement 8, and ensure that the lithium supplement 8 can be fully decomposed before the cut-off voltage during the first charging process to release lithium ions; with the second MOFs 7, its porous structure is conducive to providing more reaction sites for the lithium supplement 8, and can selectively slow down the passage of hexafluorosulfonyl imide anions (TFSI-) in the electrolyte, thereby realizing uniform transmission of lithium ions, which is conducive to the lithium supplement 8 to provide lithium ions more efficiently and improve the lithium supplement effect of the lithium supplement 8. Therefore, the positive electrode sheet in the present invention can effectively improve the lithium replenishment effect and reduce gas production, so that the lithium ion battery including the positive electrode sheet has a higher first coulombic efficiency and cycle life.
[0059] In a specific embodiment, the mass percentage of the lithium replenisher in the second positive electrode active layer is 0.5-10wt%. Within this range, on the one hand, it can ensure that sufficient lithium ions can be released during the first charging process, further reducing the consumption of lithium ions, thereby further improving the lithium replenishment effect and making the battery have a higher first coulomb efficiency; at the same time, it can also avoid excessive gas production, which exceeds the adsorption capacity of the first MOFs and the second MOFs, causing battery expansion and causing safety hazards; on the other hand, it can ensure a larger liquid storage capacity and improve the transmission effect of lithium ions.
[0060] Illustratively, the mass percentage of the lithium supplement in the second positive electrode active layer is 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%.
[0061] In a specific embodiment, the mass percentage of the lithium supplement decomposition agent in the second positive electrode active layer is 0.01-1wt%. Within this range, the lithium supplement decomposition agent can better cooperate with the lithium supplement agent to further improve the release effect of lithium ions, so that the lithium ion battery has enough lithium ions to generate a solid electrolyte membrane during the first charge, further reducing the consumption of lithium ions and effectively improving the first coulomb efficiency of the battery; at the same time, it will not affect the internal electron transmission of the battery, so that the battery has a higher rate performance.
[0062] Illustratively, the mass percentage of the lithium supplement decomposition agent in the second positive electrode active layer is 0.01wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1wt%.
[0063] In a specific embodiment, the lithium supplement decomposition agent includes at least one of metal carbides, metal oxides, and transition metal nanoparticles;
[0064] Preferably, the lithium supplement decomposition agent includes Mo 2 C, NiO, MnO 2 , lithium nickel cobalt manganese oxide, Co 3 O 4 At least one of .
[0065] Preferably, the transition metal in the transition metal nanoparticles is at least one of Fe, Co, Ni and Cu.
[0066] Preferably, the lithium supplement decomposition agent in the second positive electrode active layer is NiO, and the lithium supplement is Li 2 C 4 O 4 .
[0067] When the above lithium supplement decomposition agent is selected, it can better interact with the lithium supplement, increase the decomposition degree of the lithium supplement during the first charging process, improve the lithium supplement effect, and make the battery have a higher first coulombic efficiency.
[0068] In a specific embodiment, the mass percentage of the first MOFs in the first positive electrode active layer is greater than the mass percentage of the second MOFs in the second positive electrode active layer. At this time, on the one hand, it can ensure that the first MOFs and the second MOFs can fully exert their liquid storage function and gas adsorption function to achieve a good balance; on the other hand, since the second MOFs in the second active layer are in contact with the electrolyte earlier than the second MOFs in the first active layer, when the mass content of the second MOFs is less than the mass content of the first MOFs, it is conducive to forming a gradient difference in the liquid storage, promoting the electrolyte to infiltrate and penetrate into the first active layer.
[0069] In a specific embodiment, the ratio of the median particle size Dv50 of the lithium supplement decomposing agent to the median particle size Dv50 of the lithium supplement is 0.08-0.30;
[0070] Preferably, the median particle size Dv50 of the lithium supplement decomposition agent is 1-2 nm;
[0071] Preferably, the median particle size Dv50 of the lithium supplement is 10-20 nm.
[0072] Exemplarily, the median particle size Dv50 of the lithium supplement decomposing agent is 0.08, 0.10, 0.15, 0.20, 0.25 or 0.30 of the median particle size Dv50 of the lithium supplement.
[0073] Illustratively, the median particle size Dv50 of the lithium supplement decomposing agent is 1 nm, 1.2 nm, 1.4 nm, 1.6 nm, 1.8 nm or 2 nm.
[0074] Exemplarily, the median particle size Dv50 of the lithium supplement is 10 nm, 12 nm, 14 nm, 16 nm, 18 nm or 20 nm.
[0075] The "median particle size Dv50" in the present invention refers to the particle size corresponding to when the cumulative particle size distribution percentage of the sample reaches 50%, which can be obtained by testing with a laser particle size analyzer.
[0076] When the median particle size Dv50 of the lithium supplement decomposer and the median particle size Dv50 of the lithium supplement satisfy the aforementioned relationship, and further, when the median particle size Dv50 of the lithium supplement decomposer and / or the lithium supplement is within the aforementioned range, it can be ensured that the lithium supplement decomposer and the lithium supplement can fully contact each other, that is, the lithium supplement decomposer can wrap and adhere to the surface of the lithium supplement, which can not only increase the conductivity of the lithium supplement, but also change the electron cloud distribution of the lithium supplement, further reduce the decomposition activation energy of the lithium supplement, so that the lithium supplement can be fully decomposed in the first charge, further improve the lithium supplement effect, and make the battery have a higher first coulomb efficiency.
[0077] In one embodiment, the adsorption enthalpy of the first MOFs is 20-50 kJ·mol -1 , and / or, the adsorption enthalpy of the second MOFs is 20-50 kJ·mol -1 When the adsorption enthalpy of the first MOFs and / or the second MOFs is within the aforementioned range, the byproduct gas generated by the decomposition of the lithium supplement agent can be better adsorbed, thereby further improving the gas adsorption effect and reducing battery expansion caused by gas production.
[0078] The adsorption enthalpy in the present invention is obtained by testing with a high-precision gas and vapor adsorption instrument.
[0079] In one embodiment, the pore size of the first MOFs is smaller than the pore size of the second MOFs.
[0080] In a specific embodiment, the pore size of the first MOFs is 0.25-3 nm, and / or the pore length of the first MOFs is 2-100 nm. Within this range, the first MOFs can achieve a higher specific surface area, which can further increase the electrolyte storage capacity; and can also adsorb more gas molecules, further improve the lithium replenishment effect, reduce the battery expansion rate, and improve the first coulomb efficiency and cycle performance of the battery.
[0081] Illustratively, the pore size of the first MOFs is 0.25 nm, 0.5 nm, 0.75 nm, 1 nm, 1.25 nm, 1.5 nm, 1.75 nm, 2 nm, 2.25 nm, 2.5 nm, 2.75 nm, or 3 nm.
[0082] Illustratively, the pore length of the first MOFs is 2 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0083] In a specific embodiment, the pore size of the second MOFs is 0.25-3 nm, and / or the pore length of the second MOFs is 2-100 nm. Within this range, it can be ensured that the lithium supplement and the lithium supplement decomposition agent can be well embedded in the vicinity of the pores of the second MOFs, so that more lithium supplement and lithium supplement decomposition agent can be accommodated, and more gas molecules can be adsorbed, thereby increasing the electrolyte storage capacity, so that the battery has a higher first coulomb efficiency and cycle performance.
[0084] Illustratively, the pore size of the second MOFs is 0.25 nm, 0.5 nm, 0.75 nm, 1 nm, 1.25 nm, 1.5 nm, 1.75 nm, 2 nm, 2.25 nm, 2.5 nm, 2.75 nm, or 3 nm.
[0085] Illustratively, the pore length of the second MOFs is 2 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0086] It can be understood that there are multiple holes on the surface of the first MOFs and the second MOFs, and the internal structure or channels of the holes constitute pores, including open holes and closed holes. Open holes refer to cavities or channels connected to the outside world, and closed holes refer to cavities or channels not connected to the outside world. Then "pore size" refers to the diameter of the hole on its surface, and "pore channel" refers to the length of the channel.
[0087] The "pore size" and "pore channel" in the present invention can be obtained by testing with a specific surface area and pore size analyzer.
[0088] In a specific embodiment, the pore length of the first MOFs is 2-20nm, and / or the pore length of the second MOFs is 30-100nm. Within this range, the specific surface area of the first MOFs can be further increased, ensuring more electrolyte storage capacity and further increasing gas adsorption capacity; at the same time, the second MOFs can also accommodate more lithium supplements and lithium supplement decomposition agents, and can also adsorb more byproduct gases, thereby further improving the first coulomb efficiency and cycle performance of the battery.
[0089] In a specific embodiment, the first positive electrode active layer and the second positive electrode active layer further include a binder;
[0090] The mass percentage of the binder in the first positive electrode active layer is greater than the mass percentage of the binder in the second positive electrode active layer.
[0091] Since the first MOFs have smaller pores and higher specific surface area than the second MOFs, in order to ensure the bonding strength between the first positive electrode active layer and the positive electrode current collector and the second positive electrode active layer, and the bonding strength between the first MOFs in the first positive electrode active layer and the first positive electrode active material, the first positive electrode active layer requires more adhesive to ensure sufficient bonding strength to prevent the first positive electrode active layer from falling off and cracking; at the same time, the second MOFs in the second positive electrode active layer have larger pores and lower specific surface area, so the amount of adhesive used can be less, which can not only ensure a higher bonding strength, but also improve the conductivity of the electrode and reduce the loss of energy density.
[0092] The binder in the present invention is preferably at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polystyrene, polybutadiene, polyacrylonitrile, polyvinyl fluoride, polypropylene fluoride, butyl rubber, nitrile rubber, styrene-butadiene rubber (SBR), polysulfide rubber, butyl rubber, nitrile rubber, butyl rubber, nitrile rubber, styrene-butadiene rubber (SBR), polysulfide rubber, nitrocellulose, cyanoethyl cellulose, various latexes, acrylic resins, polyfluorene, polyaniline, polypyrrole, poly-3,4-ethylenedioxythiophene, polythiophene and poly(3,4-ethylenedioxythiophene).
[0093] When the binder is selected from a plurality of specific compounds among the aforementioned compounds, the present invention does not specifically limit the ratio between the specific compounds.
[0094] The present invention does not specifically limit the source of the binder, and any commercially available product or a product prepared by a conventional preparation method well known to those skilled in the art may be used.
[0095] In a specific embodiment, the ratio of the particle size of the lithium supplement agent to the pore length of the second MOFs is 0.1-0.8. When the above relationship is met, the lithium supplement agent can be better embedded and attached to the pores of the second MOFs, which helps the gas generated after the decomposition of the lithium supplement agent to be quickly adsorbed by the first MOFs and the second MOFs, thereby improving the adsorption effect, further alleviating the expansion problem caused by gas production, and making the battery have higher cycle performance.
[0096] Exemplarily, the ratio of the particle size of the lithium supplement agent to the pore size of the second MOFs is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7 or 0.8.
[0097] In one specific embodiment, the positive electrode sheet satisfies Formula 1,
[0098] 2×B / M b ≤A 1 ×(C 1 +D 1 )+A 2 ×(C 2 +D 2 ) Formula 1
[0099] In Formula 1, B is the mass percentage of the lithium supplement in the second positive electrode active layer; M b is the molar mass of the lithium supplement; A 1 A is the mass percentage of the first MOFs in the first positive electrode active layer; 2 is the mass percentage of the second MOFs in the second positive electrode active layer; C 1 is the carbon dioxide gas adsorption capacity of the first MOFs; D 1 is the fluorine adsorption capacity of the first MOFs; C 2 is the carbon dioxide gas adsorption capacity of the second MOFs; D 2 is the fluorine adsorption capacity of the second MOFs;
[0100] Preferably, A 1 0.08-0.5wt%, and / or, A 2 0.01-0.07wt%;
[0101] Preferably, C 1 0.1-6mmol·g -1 , and / or, and / or, D 1 0.05-5mmol·g -1 , C 2 0.1-6mmol·g -1 , and / or, D 2 0.05-5mmol·g -1 .
[0102] For example, A 1 0.08wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt% or 0.5wt%; and / or, A 2 It is 0.01wt%, 0.02wt%, 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt% or 0.07wt%.
[0103] For example, C 1 0.1mmol·g -1 , 1mmol·g -1 , 2mmol·g -1 , 3mmol·g -1 , 4mmol·g -1 , 5mmol·g -1 or 6mmol·g -1 ; and / or, C 2 0.1mmol·g -1 , 1mmol·g -1 , 2mmol·g -1 , 3mmol·g -1 , 4mmol·g -1 , 5mmol·g -1 or 6mmol·g -1 .
[0104] For example, D 1 0.05mmol·g -1 , 0.5mmol·g -1 , 1mmol·g -1 , 1.5mmol·g -1 , 2mmol·g -1 , 2.5mmol·g -1 , 3mmol·g -1 、3.5mmol·g -1 , 4mmol·g -1 , 4.5mmol·g -1 , 5mmol·g -1 ; and / or, D 2 0.05mmol·g -1 , 0.5mmol·g -1 , 1mmol·g -1 , 1.5mmol·g -1 , 2mmol·g -1 , 2.5mmol·g -1 , 3mmol·g -1 、3.5mmol·g -1, 4mmol·g -1 , 4.5mmol·g -1 , 5mmol·g -1 .
[0105] The gas adsorption amount in the present invention is obtained by testing with a multi-component high-pressure adsorption instrument, the calibration gas is helium, and the test gases are carbon dioxide and fluorine.
[0106] When the positive electrode satisfies Formula 1, further, A 1 and / or A 2 and / or C 1 and / or C 2 When within the aforementioned range, the first MOFs, the second MOFs and the lithium supplement agent can cooperate with each other to ensure that the byproduct gas generated by the decomposition of the lithium supplement agent can be completely absorbed, further reducing the battery expansion problem caused by gas production, and making the battery have higher cycle performance.
[0107] The second aspect of the present invention provides a lithium ion battery, comprising the positive electrode sheet of the first aspect. Since the lithium ion battery comprises the positive electrode sheet, the lithium ion battery has a higher first coulombic efficiency and cycle life.
[0108] The positive electrode sheet of the present invention is described in detail below through specific embodiments.
[0109] Example 1
[0110] Lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF) and the first MOFs material UIO-66 were mixed uniformly in a mass ratio of 97.4:0.5:2:0.1, added into N-methylpyrrolidone (NMP), and stirred uniformly to obtain a first positive electrode active layer slurry with a solid content of 70wt%;
[0111] Among them, the adsorption enthalpy of UIO-66 is 23.2-28.5 kJ·mol -1 , carbon dioxide gas adsorption capacity is 2mmol·g -1 、Fluorine adsorption capacity is 3mmol·g -1 , pore length is 15nm, pore diameter is 2nm;
[0112] Lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), the second MOFs material UIO-66, Li 2 C 4 O 4 and a lithium supplement decomposing agent NiO are uniformly mixed in a mass ratio of 96.95:0.5:1:0.05:1:0.5, added into N-methylpyrrolidone (NMP), and stirred to obtain a second positive electrode active layer slurry with a solid content of 70 wt%;
[0113] Among them, the adsorption enthalpy of UIO-66 is 38.3-42.6 kJ·mol -1 , carbon dioxide gas adsorption capacity is 4mmol·g -1 , fluorine gas adsorption capacity is 3.5mmol·g -1 , the pore size is 100nm, the pore size is 1nm; the particle size of the lithium supplement agent is 15nm, and the particle size of the lithium supplement agent decomposition agent is 1.2nm;
[0114] The first positive electrode active layer slurry was coated on the two functional surfaces of the aluminum foil. The density after coating was 8.29 mg / cm 2 After drying, the second positive electrode active layer slurry is coated on the surface of the first positive electrode active layer. The density of the coated surface is 6.11 mg / cm 2 After drying, rolling and slitting, the compacted density is 4.15g / cm 3 The total thickness of the first positive electrode active layer on both sides is 40 μm, and the total thickness of the second positive electrode active layer on both sides is 30 μm.
[0115] Example 2
[0116] Lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF) and the first MOFs material MIL-100 are mixed uniformly in a mass ratio of 97.42:0.5:2:0.08, added into N-methylpyrrolidone (NMP), and stirred uniformly to obtain a first positive electrode active layer slurry with a solid content of 70wt%;
[0117] Among them, the adsorption enthalpy of MIL-100 is 20.2-23.5 kJ·mol -1 , carbon dioxide gas adsorption capacity is 0.1mmol·g -1 、Fluorine adsorption capacity is 0.05mmol·g -1 , pore length is 2nm, pore diameter is 0.25nm;
[0118] Lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), the second MOFs material MIL-101, Li 2 MnO 3 and lithium supplement decomposition agent Mo 2 C is mixed uniformly in a mass ratio of 97.98:0.5:1:0.01:0.5:0.01, added into N-methylpyrrolidone (NMP), and stirred uniformly to obtain a second positive electrode active layer slurry with a solid content of 70 wt%;
[0119] Among them, the adsorption enthalpy of MIL-101 is 20.2-23.5 kJ·mol -1 , carbon dioxide gas adsorption capacity is 0.1mmol·g -1、Fluorine adsorption capacity is 0.05mmol·g -1 , the pore size is 30nm, the pore size is 0.25nm; the particle size of the lithium supplement agent is 10nm, and the particle size of the lithium supplement agent decomposition agent is 1nm;
[0120] The first positive electrode active layer slurry was coated on the two functional surfaces of the aluminum foil. The density after coating was 8.29 mg / cm 2 After drying, the second positive electrode active layer slurry is coated on the surface of the first positive electrode active layer. The density of the coated surface is 6.11 mg / cm 2 After drying, rolling and slitting, the compacted density is 4.15g / cm 3 The total thickness of the first positive electrode active layer on both sides is 40 μm, and the total thickness of the second positive electrode active layer on both sides is 30 μm.
[0121] Example 3
[0122] Lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF) and the first MOFs material MOF-5 were mixed uniformly in a mass ratio of 97.2:0.5:2:0.3, added into N-methylpyrrolidone (NMP), and stirred uniformly to obtain a first positive electrode active layer slurry with a solid content of 70wt%;
[0123] Among them, the adsorption enthalpy of MOF-5 is 40.4-44.7 kJ·mol -1 , carbon dioxide gas adsorption capacity is 4mmol·g -1 , fluorine gas adsorption capacity is 3.8mmol·g -1 , the pore length is 10nm, and the pore diameter is 1nm;
[0124] Lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), the second MOFs material UIO-66, LiF and lithium supplement decomposition agent LiNi 0.8 Co 0.1 Mn 0.1 O 2 The mixture was uniformly mixed in a mass ratio of 92.97:0.5:1:0.03:5:0.5, added into N-methylpyrrolidone (NMP), and stirred uniformly to obtain a second positive electrode active layer slurry with a solid content of 70 wt%;
[0125] Among them, the adsorption enthalpy of UIO-66 is 30.5-34.1 kJ·mol -1 , carbon dioxide gas adsorption capacity is 2mmol·g -1 , fluorine gas adsorption capacity is 1.5mmol·g -1 , pore size is 50nm, pore diameter is 2nm; the particle size of lithium supplement agent is 15nm, and the particle size of lithium supplement agent decomposition agent is 1.6nm;
[0126] The first positive electrode active layer slurry was coated on the two functional surfaces of the aluminum foil. The density after coating was 8.29 mg / cm 2 After drying, the second positive electrode active layer slurry is coated on the surface of the first positive electrode active layer. The density of the coated surface is 6.11 mg / cm 2 After drying, rolling and slitting, the compacted density is 4.15g / cm 3 The total thickness of the first positive electrode active layer on both sides is 40 μm, and the total thickness of the second positive electrode active layer on both sides is 30 μm.
[0127] Example 4
[0128] Lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF) and the first MOFs material PCN-14 were mixed uniformly in a mass ratio of 97:0.5:2:0.5, added into N-methylpyrrolidone (NMP), and stirred uniformly to obtain a first positive electrode active layer slurry with a solid content of 70wt%;
[0129] Among them, the adsorption enthalpy of PCN-14 is 48.1-50.0 kJ·mol -1 , carbon dioxide gas adsorption capacity is 6mmol·g -1 , fluorine gas adsorption capacity is 4.7mmol·g -1 , the pore length is 20nm, and the pore diameter is 3nm;
[0130] Lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), the second MOFs material HKUST-1, Li5FeO 4 and the lithium supplement agent decomposition agent Ni nanoparticles are uniformly mixed in a mass ratio of 87.43:0.5:1:0.07:10:1, added into N-methylpyrrolidone (NMP), and stirred to obtain a second positive electrode active layer slurry with a solid content of 70wt%;
[0131] Among them, the adsorption enthalpy of HKUST-1 is 48.6-50.0 kJ·mol -1 , carbon dioxide gas adsorption capacity is 6mmol·g -1 , fluorine gas adsorption capacity is 4.8mmol·g -1 , the pore size is 70nm, the pore size is 3nm; the particle size of the lithium supplement agent is 20nm, and the particle size of the lithium supplement agent decomposition agent is 2nm;
[0132] The first positive electrode active layer slurry was coated on the two functional surfaces of the aluminum foil. The density after coating was 8.29 mg / cm 2 After drying, the second positive electrode active layer slurry is coated on the surface of the first positive electrode active layer. The density of the coated surface is 6.11 mg / cm 2After drying, rolling and slitting, the compacted density is 4.15g / cm 3 The total thickness of the first positive electrode active layer on both sides is 40 μm, and the total thickness of the second positive electrode active layer on both sides is 30 μm.
[0133] Example 5
[0134] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in embodiment 1, except that lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), the second MOFs material UIO-66, Li 2 C 4 O 4 The mass ratio of the lithium supplement agent to the lithium supplement agent decomposition agent NiO is adjusted to 97.7:0.5:1:0.05:0.25:0.5, and the mass percentage of the lithium supplement agent in the second active layer is 0.25wt%.
[0135] Example 6
[0136] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in embodiment 1, except that lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), the second MOFs material UIO-66, Li 2 C 4 O 4 The mass ratio of NiO to the lithium supplement decomposing agent is adjusted to 95.45:0.5:1:0.05:1:2, and the mass percentage of the lithium supplement decomposing agent in the second active layer is 2wt%.
[0137] Example 7
[0138] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in embodiment 1, except that lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), the second MOFs material UIO-66, Li 2 C 4 O 4 The mass ratio of the first MOFs to the lithium supplement decomposition agent NiO is adjusted to 95.45:0.5:1:0.2:1:2, then the mass percentage of the first MOFs in the first positive electrode active layer is less than the mass percentage of the second MOFs in the second positive electrode active layer.
[0139] Example 8
[0140] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in Embodiment 1, except that the median particle size Dv50 of the lithium supplement decomposition agent is adjusted to 4 nm.
[0141] Example 9
[0142] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in Embodiment 1, except that the median particle size Dv50 of the lithium supplement agent is adjusted to 8 nm.
[0143] Example 10
[0144] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in Embodiment 1, except that the median particle size Dv50 of the lithium supplement decomposer is adjusted to 1 nm, and the median particle size Dv50 of the lithium supplement is adjusted to 20 nm, and the ratio of the median particle size Dv50 of the lithium supplement decomposer to the lithium supplement is 0.05.
[0145] Embodiment 11
[0146] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in Example 1, except that the adsorption enthalpy of the first MOFs material UIO-66 is 13.4-15.9 kJ·mol -1 .
[0147] Example 12
[0148] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in Example 1, except that the adsorption enthalpy of the second MOFs material UIO-66 is 13.4-15.9 kJ·mol -1 .
[0149] Embodiment 13
[0150] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in Embodiment 1, except that the pore length of the first MOFs material UIO-66 is 110 nm and the pore diameter is 5 nm.
[0151] Embodiment 14
[0152] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in Embodiment 1, except that the pore size of the second MOFs material UIO-66 is 115 nm and the pore diameter is 5 nm.
[0153] Embodiment 15
[0154] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in Example 1, except that the mass ratio of lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF) and the first MOFs material UIO-66 is adjusted to 98.4:0.5:1:0.1;
[0155] Lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), the second MOFs material UIO-66, Li 2 C 4 O 4The mass ratio of the lithium supplement decomposition agent NiO is adjusted to 95.95:0.5:2:0.05:1:0.5;
[0156] At this time, the mass percentage of the binder in the first positive electrode active layer is greater than the mass percentage of the binder in the second positive electrode active layer.
[0157] Example 16
[0158] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in Embodiment 1, except that the particle size of the lithium supplement agent is 20 nm, and the pore length of the second MOFs material UIO-66 is 15 nm, and the ratio of the particle size of the lithium supplement agent to the pore length of the second MOFs is 1.33.
[0159] Embodiment 17
[0160] The preparation method of the positive electrode sheet in this embodiment is basically the same as that in embodiment 2, except that the first MOFs material MIL-100 is replaced by PCN-222, and the adsorption enthalpy is 20.0-22.2 kJ·mol -1 ; The second MOFs material MIL-101 was replaced by PCN-222, and the adsorption enthalpy was 20.0-22.2 kJ·mol -1 ; Lithium supplement Li 2 MnO 3 Replaced by Li 2 O;
[0161] Then, 2×B / M b is 0.033, A 1 ×(C 1 +D 1 )+A 2 ×(C 2 +D 2 ) is 0.0135, 2×B / M b >A 1 ×(C 1 +D 1 )+A 2 ×(C 2 +D 2 ), which does not conform to Formula 1.
[0162] Comparative Example 1
[0163] The preparation method of the positive electrode sheet in this comparative example is basically the same as that in Example 1, except that the positive electrode sheet does not include the first positive electrode active layer, but only has the second positive electrode active layer, and the second positive electrode active layer is located on two functional surfaces of the aluminum foil.
[0164] Comparative Example 2
[0165] The preparation method of the positive electrode sheet in this comparative example is basically the same as that in Example 1, except that the second positive electrode active layer does not include a lithium supplement decomposition agent, namely, lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), a second MOFs material UIO-66, and Li 2 C 4 O 4 The mass ratio is 97.45:0.5:1:0.05:1.
[0166] Comparative Example 3
[0167] The preparation method of the positive electrode sheet in this comparative example is basically the same as that in Example 1, except that the second positive electrode active layer does not include the second MOFs material, namely lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), Li 2 C 4 O 4 And the lithium supplement decomposer NiO is in a mass ratio of 97:0.5:1:1:0.5.
[0168] Comparative Example 4
[0169] The preparation method of the positive electrode sheet in this comparative example is basically the same as that in Example 1, except that the second positive electrode active layer does not include the second MOFs material and the lithium supplement decomposition agent, namely, lithium cobalt oxide, single-walled carbon nanotubes, polyvinylidene fluoride (PVDF), Li 2 C 4 O 4 According to the mass ratio of 97.5:0.5:1:1.
[0170] Test example
[0171] The positive electrode sheets prepared in the above embodiments and comparative examples were made into lithium-ion batteries, and the initial coulombic efficiency, thickness expansion rate, electrolyte retention amount, and cycle capacity retention rate of the prepared lithium-ion batteries were tested:
[0172] Graphite, SiO, SP carbon black, dispersant sodium carboxymethyl cellulose (CMC), and adhesive styrene-butadiene rubber (SBR) were mixed uniformly in a mass ratio of 90:5:1.2:1.5:2.3, added into deionized water, and stirred uniformly to prepare a negative electrode slurry with a solid content of 50 wt%. The negative electrode slurry was uniformly coated on both sides of the functional surface of the copper foil, and after drying, rolling, and slitting, a surface density of 7.89 mg / cm was obtained. 2 , compacted density is 1.8g / cm 3The positive electrode sheet, the polyethylene porous separator and the negative electrode sheet in the above-mentioned embodiment and the comparative example are stacked in sequence, wound to obtain a winding core, and then packaged, injected, formed, and sorted to obtain the lithium ion battery of this embodiment; wherein the electrolyte comprises lithium salt lithium hexafluorophosphate, organic solvents ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC) and additive fluoroethylene carbonate, and the molar concentration of lithium hexafluorophosphate in the electrolyte is 1 mol / L, the mass percentage of fluoroethylene carbonate in the electrolyte is 5wt%, and the mass ratio of EC, DEC, and EMC is 2:3:5.
[0173] 1) First Coulombic efficiency
[0174] The charge and discharge in the formation stage is taken as the first charge and discharge, and the first coulomb efficiency is obtained. The charge and discharge mechanism is: let the battery cell stand for 5 minutes, charge at 30mA for 10 minutes, and then charge at 0.1C constant current and constant voltage. The cut-off voltage is 4.45V, the cut-off current is 0.02C, and the charging capacity is recorded as Q 0 ; Let stand for 5 minutes, then discharge at a constant current of 0.1C, the cut-off voltage is 3.0V, and the discharge capacity is recorded as Q 1 , then the first coulombic efficiency (%) = (Q 1 / Q 0 )×100%.
[0175] 2) Thickness expansion rate and capacity retention rate
[0176] At an ambient temperature of 25°C, the thickness of the lithium-ion battery prepared above was measured using a flat pressure PPG thickness gauge, and the initial thickness was recorded as T 0 Then charge the lithium-ion battery at 1C constant current to 4.45V, then charge it at constant voltage to a cut-off current of 0.05C, let it stand for 5 minutes, and discharge it at 1C constant current to 3.0V. This is the first cycle, and the discharge capacity is recorded as C 0 ; Cycle according to the above charge and discharge mechanism, and record the discharge capacity after 200 cycles as C 1 The thickness of the battery after 200 cycles was measured using a flat pressure PPG thickness gauge, and the thickness of the battery after the cycle was recorded as T 1 , then capacity retention rate (%) = (C 1 / C 0 )×100%, thickness expansion rate (%) = (T 1 / T 0 )×100%
[0177] 3) Electrolyte retention volume
[0178] The battery weight (g) before and after injection is tested respectively, and the electrolyte retention amount = battery weight before injection - battery weight after injection.
[0179] The test and calculation results are shown in Table 1.
[0180] Table 1
[0181]
[0182]
[0183] From Table 1, we can see that:
[0184] Compared with Comparative Examples 1 to 4, the lithium ion batteries in Examples 1 to 17 have higher electrolyte retention, lower thickness expansion rate, and higher first coulomb efficiency and cycle capacity retention rate, wherein the electrolyte retention of the lithium ion battery in Example 1 is as high as 7.75g, and correspondingly, its thickness expansion rate is only 4.95%, the first coulomb efficiency is 92.2%, and the cycle capacity retention rate is 96.50%. It can be seen that the positive electrode sheet of the present invention can effectively improve the first coulomb efficiency and cycle life of the lithium ion battery.
[0185] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises a positive electrode current collector, a first positive electrode active layer and a second positive electrode active layer; the first positive electrode active layer is located on at least one functional surface of the positive electrode current collector, and the second positive electrode active layer is located on a surface of the first positive electrode active layer away from the positive electrode current collector; The first positive electrode active layer includes a first positive electrode active material and a first MOFs; the second positive electrode active layer includes a second positive electrode active material, a second MOFs, a lithium supplement agent and a lithium supplement agent decomposing agent.
2. The positive electrode sheet according to claim 1, characterized in that: The mass percentage of the lithium replenisher in the second positive electrode active layer is 0.5-10wt%, and / or the mass percentage of the lithium replenisher decomposing agent in the second positive electrode active layer is 0.01-1wt%.
3. The positive electrode sheet according to claim 1 or 2, characterized in that: The lithium supplement decomposing agent comprises at least one of metal carbides, metal oxides and transition metal nanoparticles; Preferably, the lithium supplement decomposition agent includes at least one of Mo2C, NiO, MnO2, lithium nickel cobalt manganese oxide, and Co3O4.
4. The positive electrode sheet according to any one of claims 1 to 3, characterized in that: The mass percentage of the first MOFs in the first positive electrode active layer is greater than the mass percentage of the second MOFs in the second positive electrode active layer.
5. The positive electrode sheet according to any one of claims 1 to 4, characterized in that: The ratio of the median particle size Dv50 of the lithium supplement decomposing agent to the median particle size Dv50 of the lithium supplement is 0.08-0.30; Preferably, the median particle size Dv50 of the lithium supplement decomposition agent is 1-2 nm; Preferably, the median particle size Dv50 of the lithium supplement agent is 10-20 nm.
6. The positive electrode sheet according to any one of claims 1 to 5, characterized in that: The adsorption enthalpy of the first MOFs is 20-50 kJ·mol -1 , and / or, the adsorption enthalpy of the second MOFs is 20-50 kJ·mol -1 .
7. The positive electrode sheet according to any one of claims 1 to 6, characterized in that: The pore size of the first MOFs is smaller than the pore size of the second MOFs; Preferably, the pore size of the first MOFs is 0.25-3 nm, and / or the pore length of the first MOFs is 2-100 nm; Preferably, the pore size of the second MOFs is 0.25-3 nm, and / or the pore length of the second MOFs is 2-100 nm.
8. The positive electrode sheet according to claim 7, characterized in that: The pore length of the first MOFs is 2-20 nm, and / or the pore length of the second MOFs is 30-100 nm.
9. The positive electrode sheet according to claim 1, characterized in that: The first positive electrode active layer and the second positive electrode active layer also include a binder; The mass percentage of the binder in the first positive electrode active layer is greater than the mass percentage of the binder in the second positive electrode active layer.
10. The positive electrode sheet according to any one of claims 1 to 9, characterized in that: The ratio of the particle size of the lithium supplement agent to the pore length of the second MOFs is 0.1-0.
8.
11. The positive electrode sheet according to any one of claims 1 to 10, characterized in that: The positive electrode sheet satisfies Formula 1, 2×B / M b ≤A1×(C1+D1)+A2×(C2+D2) Formula 1 In Formula 1, B is the mass percentage of the lithium supplement in the second positive electrode active layer; M b is the molar mass of the lithium supplement; A1 is the mass percentage of the first MOFs in the first positive electrode active layer; A2 is the mass percentage of the second MOFs in the second positive electrode active layer; C1 is the carbon dioxide gas adsorption capacity of the first MOFs; D1 is the fluorine gas adsorption capacity of the first MOFs; C2 is the carbon dioxide gas adsorption capacity of the second MOFs; D2 is the fluorine gas adsorption capacity of the second MOFs; Preferably, the A1 is 0.08-0.5wt%, and / or the A2 is 0.01-0.07wt%; Preferably, the Cl is 0.1-6 mmol·g -1 , and / or, said D1 is 0.05-5 mmol·g -1 , and / or, the C2 is 0.1-6 mmol·g -1 , and / or, said D2 is 0.05-5 mmol·g -1 .
12. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to any one of claims 1 to 11.