Composite current collector, electrode plate, battery and electronic equipment

By introducing a functional conductive layer of buffer holes into the composite fluid collector, the problem of damage to the composite fluid collector during the charging and discharging process is solved, the battery capacity and conductivity are improved, and the polarization increase and coating process difficulty is reduced.

CN118943375APending Publication Date: 2024-11-12GUANGDONG OPPO MOBILE TELECOMMUNICATIONS CORP LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310534263.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing composite liquid collector is prone to damage during the battery charging and discharging process, resulting in local deactivation and increased polarization, and reducing battery capacity.

Method used

A composite fluid is designed, including a polymer layer, a first metal layer, a second metal layer and a functional conductive layer. The functional conductive layer has a buffer hole, and the buffer hole is located in the first functional conductive layer and the second functional conductive layer, respectively Located on one side of the first metal layer and the second metal layer away from the polymer layer, it buffers the stress strain generated by the insertion and release of active ions, and limits the release of metal ions to avoid damage to the composite fluid collection.

Benefits of technology

It effectively avoids damage to the composite liquid collector during charging and discharging, prevents local deactivation, improves battery capacity, and improves the conductivity and tolerance of the coating process, reducing material waste and polarization increase.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943375A_ABST
    Figure CN118943375A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electronic equipment, in particular to a composite current collector, an electrode plate, a battery and electronic equipment, the composite current collector comprises a polymer layer, a first metal layer, a second metal layer and a functional conductive layer, the first metal layer and the second metal layer are respectively located on two opposite sides of the polymer layer; the functional conductive layer comprises a first functional conductive layer and / or a second functional conductive layer; the first functional conductive layer is located at one side, far away from the polymer layer, of the first metal layer, and the second functional conductive layer is located at one side, far away from the polymer layer, of the second metal layer; and the first functional conductive layer and the second functional conductive layer are respectively and independently provided with buffer holes. The composite current collector can solve the problem that the composite current collector is easy to damage in the charging and discharging process of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electronic equipment, and in particular to a composite current collector, an electrode sheet, a battery and an electronic equipment. Background Art

[0002] Batteries, as energy storage devices, have been widely used in various electronic devices, and the market's requirements for battery energy density are constantly increasing. Generally speaking, the lighter the battery, the more conducive it is to improving energy density. The current collector is a necessary component of the battery, and this type of mass is called the "dead mass" of the battery. If the weight of the current collector is reduced, it will be beneficial to improve the battery's energy density.

[0003] Composite current collectors are products that use polymer layers to replace part of the metal layer to achieve weight reduction. Therefore, composite current collectors are expected to replace traditional current collectors in more fields. However, the current composite current collectors are easily damaged during the battery charging and discharging process. After damage, the composite current collectors will be partially inactivated, resulting in increased polarization and reduced battery capacity. Summary of the invention

[0004] Based on this, the present application provides a composite current collector to solve the problem of easy breakage during battery charging and discharging.

[0005] The first aspect of the present application provides a composite current collector, and its technical solution is as follows:

[0006] A composite current collector comprises a polymer layer, a first metal layer, a second metal layer and a functional conductive layer:

[0007] The first metal layer and the second metal layer are respectively located on opposite sides of the polymer layer;

[0008] The functional conductive layer comprises a first functional conductive layer and / or a second functional conductive layer; the first functional conductive layer is located on a side of the first metal layer away from the polymer layer, and the second functional conductive layer is located on a side of the second metal layer away from the polymer layer;

[0009] The first functional conductive layer and the second functional conductive layer each independently have a buffer hole.

[0010] A second aspect of the present application provides an electrode plate, which includes a composite current collector and an electrode active layer located on the composite current collector; the composite current collector is the composite current collector described above.

[0011] A third aspect of the present application provides a battery, comprising a battery shell and an electrode plate located in the battery shell, wherein the electrode plate is the electrode plate as described above.

[0012] A fourth aspect of the present application provides an electronic device, comprising a device body and a battery, wherein the device body has a battery cavity, the battery is located in the battery cavity, and the battery is the battery as described above.

[0013] This application has the following beneficial effects:

[0014] In the present application, the first functional conductive layer and the second functional conductive layer each independently have a buffer hole. On the one hand, when active ions are embedded and removed from the composite current collector during the battery charging and discharging process, the buffer hole can play a buffering role, offsetting the stress strain generated by the embedding and removal of active ions on the deformation of the entire composite current collector, and avoiding the damage of the composite current collector; on the other hand, the first functional conductive layer is located on the first metal layer, and the second functional conductive layer is located on the second metal layer. When the functional conductive layer includes the first functional conductive layer and / or the second functional conductive layer, during the battery charging and discharging process, the metal ions in the first metal layer and / or the second metal layer can be restricted to a certain extent to escape, avoiding the damage of the composite current collector. In summary, the present application can avoid the damage of the composite current collector during the charging and discharging process, avoid its local inactivation, and help avoid the increase in polarization caused by the local inactivation of the composite current collector, thereby improving the battery capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0016] Figure 1 is a schematic structural diagram of a composite current collector according to an embodiment;

[0017] Figure 2 is a SEM image of the composite current collector of Example 1;

[0018] Figure 3 is a SEM image of the composite current collector of Example 2;

[0019] Figure 4 is a SEM image of the composite current collector of Example 3;

[0020] Figure 5 The test results of charging at 1C rate and discharging at 0.2C rate are shown in the figure;

[0021] Figure 6 The test results of charging at 3C rate and discharging at 0.2C rate are shown in the figure;

[0022] Figure 7The test results are shown for charging at 4C rate and discharging at 0.2C rate. DETAILED DESCRIPTION

[0023] The present application will be further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0025] the term

[0026] Unless otherwise specified or there is a contradiction, the terms and phrases used in this application have the following meanings:

[0027] In the present application, "multiple" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the present application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0028] In this application, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0029] In the present application, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0030] In the present application, when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may also be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time. It should also be understood that when explaining the connection relationship or positional relationship of elements, although not explicitly described, the connection relationship and positional relationship are interpreted as including an error range, which should be within the acceptable deviation range of a specific value determined by a person skilled in the art.

[0031] In this application, electronic devices may be, but are not limited to, various personal computers, laptops, smart phones, tablet computers, IoT devices, and portable wearable devices. IoT devices may be smart speakers, smart TVs, smart air conditioners, smart car devices, etc. Portable wearable devices may be smart watches, smart bracelets, head-mounted devices, etc.

[0032] Metals (such as copper foil and aluminum foil) are common current collectors for commercial batteries, but metals have very high density and are heavy. In order to reduce the weight of the current collector, composite current collectors came into being. Composite current collectors are products that use polymer layers to replace part of the metal layer to reduce the weight of the current collector. However, the current composite current collectors are easily damaged during the battery charging and discharging process, and the damaged composite current collectors will be partially inactivated, resulting in increased polarization and reduced battery capacity.

[0033] In order to solve the above problems, one embodiment of the present application provides a composite current collector, see Figure 1 The composite current collector 01 of this embodiment includes a polymer layer 10 , a first metal layer 20 , a second metal layer 30 , and a functional conductive layer 40 .

[0034] The first metal layer 20 and the second metal layer 30 are respectively located on opposite sides of the polymer layer 10 .

[0035] The functional conductive layer 40 includes a first functional conductive layer 401 and a second functional conductive layer 402 ; the first functional conductive layer 401 is located on a side of the first metal layer 20 away from the polymer layer 10 , and the second functional conductive layer 402 is located on a side of the second metal layer 30 away from the polymer layer 10 .

[0036] In this embodiment, both the first functional conductive layer 401 and the second functional conductive layer 402 have buffer holes 403 .

[0037] It can be understood that the buffer hole 403 may be located on the surface and / or inside the first functional conductive layer 401 . Similarly, the buffer hole 403 may be located on the surface and / or inside the second functional conductive layer 402 .

[0038] In this embodiment, by providing buffer holes 403 in the first functional conductive layer 401 and the second functional conductive layer 402, on the one hand, when active ions are embedded and removed from the composite current collector 01 during the battery charging and discharging process, the buffer holes 403 can play a buffering role, offsetting the deformation effect of the stress strain generated by the embedding and removal of active ions on the entire composite current collector 01, and avoiding the damage of the composite current collector 01; on the other hand, in this embodiment, the first functional conductive layer 401 is located on the first metal layer 20, and the second functional conductive layer 402 is located on the second metal layer 30. During the battery charging and discharging process, the metal ions in the first metal layer 20 and the second metal layer 30 can be restricted to a certain extent to escape, avoiding the damage of the composite current collector. In summary, this embodiment can prevent the composite current collector from being damaged during the charging and discharging process, and avoid its local inactivation, which is conducive to avoiding the increase of polarization caused by the local inactivation of the composite current collector, and improving the battery capacity.

[0039] Specifically, on the one hand, in a conventional composite current collector, when active ions are embedded and removed from the conventional current collector during the battery charge and discharge process, although the polymer layer can be used for deformation expansion, it cannot completely offset the deformation effect of the stress strain generated by the embedding and removal of active ions on the entire composite current collector. In this embodiment, since the first functional conductive layer and the second functional conductive layer with buffer holes are added, the buffer holes can play a buffering role, thus providing a second layer for deformation expansion to avoid damage to the composite current collector; on the other hand, during the battery charge and discharge process, the metal ions in the first metal layer and the second metal layer are easily removed. The reason is that: in order to increase the energy density of the battery, the charging cut-off voltage is often increased, and the energy density of the battery is expanded by using a high voltage cut-off platform. However, in a high-voltage working environment, the metals of the first metal layer and the second metal layer are easily transformed from simple substances to ions and removed from the first metal layer and the second metal layer. In a conventional composite current collector, the removal of metal ions directly leads to an incomplete structure of the composite current collector. In this embodiment, since the first metal layer and the second metal layer are respectively provided with the first functional conductive layer and the second functional conductive layer, the metal ions can be temporarily released from the composite current collector to a certain extent, thereby protecting the structural integrity of the composite current collector and preventing it from being damaged easily.

[0040] In addition, in the composite current collector, since the polymer layer is generally not conductive, the conductivity of the traditional composite current collector mainly comes from the metal layer. Due to the need to reduce the weight of the composite current collector, the metal layer of the composite current collector is usually thin, which results in low conductivity and high internal resistance of the composite current collector. In this embodiment, a first functional conductive layer and a second functional conductive layer are provided on the first metal layer and the second metal layer, which is conducive to improving the conductivity of the composite current collector and enhancing the conductivity of the composite current collector, thereby improving the battery performance and increasing the energy density of the battery.

[0041] In addition, the metal layer on the traditional composite current collector can be formed by evaporation coating, magnetron sputtering coating, electroplating, chemical coating and other coating methods. After the metal layer is formed by the above method, some metal protrusions or wrinkles are likely to appear on the surface of the metal layer, resulting in low yield. In order to prevent such a situation from occurring, the traditional composite current collector has high requirements for the coating process when coating the metal film. In this embodiment, a first functional conductive layer and a second functional conductive layer are arranged on the first metal layer and the second metal layer, which is equivalent to a secondary modification of the metal layer. The coating process of the metal layer is more tolerant, and some metal protrusions or wrinkles can be allowed to appear on the surface of the metal layer, thereby avoiding material waste and improving product utilization.

[0042] In addition, in this embodiment, due to the presence of the buffer hole, the wettability of the first functional conductive layer and the second functional conductive layer to the electrolyte can be improved.

[0043] In addition, the buffer holes can be located on the surface of the first functional conductive layer and the second functional conductive layer, which is beneficial to improving the coating performance of the electrode active slurry and improving the bonding force between the electrode active layer and the first functional conductive layer and the second functional conductive layer.

[0044] In other embodiments, the functional conductive layer may include a first functional conductive layer or a second functional conductive layer. When the functional conductive layer includes the first functional conductive layer, it means that the second functional conductive layer may not be included; when the functional conductive layer includes the second functional conductive layer, it means that the first functional conductive layer may not be included. In this case, the cost can be reduced. At the same time, since the first functional conductive layer or the second functional conductive layer has buffer holes, it can also play a buffering role, offsetting the deformation effect of the stress strain generated by the embedding and extraction of active ions on the entire composite current collector, and avoiding damage to the composite current collector; and the first functional conductive layer is located on the first metal layer, and the second functional conductive layer is located on the second metal layer. During the battery charging and discharging process, the metal ions in the first metal layer or the second metal layer can be limited to a certain extent to escape, avoiding damage to the composite current collector.

[0045] In addition, the addition of the first functional conductive layer or the second functional conductive layer can also improve the conductivity of the composite current collector, and is also more tolerant to the coating process of the metal layer, allowing some metal protrusions or wrinkles to appear on the surface of the metal layer, and can also improve the wetting ability of the functional conductive layer to the electrolyte, and can also improve the bonding force between the electrode active layer and the functional conductive layer.

[0046] In some examples, the aperture of the buffer hole satisfies the following conditions: during the charge and discharge process, the metal ions released from the first metal layer and / or the second metal layer cannot be discharged through the buffer hole. At this time, the metal ions in the first metal layer and / or the second metal layer can escape from the metal layer, but ultimately cannot escape from the functional conductive layer, that is, the metal ions cannot leave the composite current collector, which is beneficial for the composite current collector to further maintain structural integrity.

[0047] In some examples, the aperture of the buffer hole satisfies the following conditions: during the charge and discharge process, the metal ions released from the first metal layer and / or the second metal layer cannot enter the buffer hole. At this time, although the metal ions in the first metal layer and / or the second metal layer theoretically escape, they cannot enter the functional conductive layer, that is, they cannot leave the metal layer, which is more conducive to the composite current collector maintaining structural integrity.

[0048] Optionally, the pore size of the buffer hole is 1nm to 10000nm. It is understandable that the pore size of the buffer hole can be any value in any two numerical endpoint value ranges including two numerical endpoint values ​​of 1nm, 10nm, 50nm, 100nm, 500nm, 1000nm, 5000nm and 10000nm. Further optionally, the pore size of the buffer hole is 1nm to 1000nm. Further optionally, the pore size of the buffer hole is 1nm to 300nm.

[0049] Optionally, the thickness of the first functional conductive layer and the second functional conductive layer are each independently 0.001 μm to 40 μm. It is understandable that the thickness of the first functional conductive layer and the second functional conductive layer can be any value in any two numerical endpoint value ranges including two numerical endpoint values ​​of 0.001 μm, 0.01 μm, 0.1 μm, 1 μm, 10 μm and 40 μm. Further optionally, the thickness of the first functional conductive layer and the second functional conductive layer are each independently 0.01 μm to 10 μm. Further optionally, the thickness of the first functional conductive layer and the second functional conductive layer are each independently 0.01 μm to 2 μm.

[0050] It can be understood that due to the presence of buffer holes, the surfaces of the first functional conductive layer and the second functional conductive layer may have a certain roughness, and the electrode active slurry can be more tightly combined on the first functional conductive layer and / or the second functional conductive layer, which is beneficial to improving the bonding force between the composite current collector and the electrode active layer.

[0051] In this embodiment, the materials of the first functional conductive layer 401 and the second functional conductive layer 402 can be selected so that the first functional conductive layer 401 and the second functional conductive layer 403 have buffer holes 403, and the pore size of the buffer holes 403 can be adjusted by adjusting the components and amounts of the materials of the first functional conductive layer 401 and the second functional conductive layer 402.

[0052] Optionally, the materials of the first functional conductive layer and the second functional conductive layer each independently include one or more of porous carbon material, foamed metal, porous conductive liquid crystal polymer (LCP), porous oxide and yttria-stabilized zirconia (YSZ).

[0053] Further optionally, the porous carbon material includes one or more of graphite, soft carbon, hard carbon, carbon nanotubes and graphene. Among them, the hard carbon includes one or more of carbon black (Super-p), resin carbon and organic polymer pyrolytic carbon.

[0054] Further optionally, the metal foam includes one or more of copper foam, aluminum foam, iron foam, cobalt foam, nickel foam and titanium foam.

[0055] Further optionally, the porous oxide includes one or more of porous aluminum oxide and porous copper oxide.

[0056] In this embodiment, the materials of the first functional conductive layer 401 and the second functional conductive layer 402 both include porous carbon materials, and the porous carbon materials constitute a carbon skeleton framework. Further, the porous carbon materials include graphite, carbon black and carbon nanotubes. By adjusting the amount of graphite, carbon black and carbon nanotubes, the aperture of the buffer hole 403 in the first functional conductive layer 401 and the second functional conductive layer 402 is adjusted.

[0057] Optionally, in the first functional conductive layer and the second functional conductive layer, the weight ratio of graphite, carbon black and carbon nanotubes is (80-97):(0.1-5):(0.1-5). At this time, the aperture of the buffer pores of the first functional conductive layer and the second functional conductive layer is 1nm-300nm, and when the first metal layer and the second metal layer are copper layers or aluminum layers, copper ions and aluminum ions cannot enter the buffer pores during the charge and discharge process.

[0058] Further optionally, in the first functional conductive layer and the second functional conductive layer, the weight ratio of graphite, carbon black and carbon nanotubes is (90-97):(0.5-5):(0.5-5).

[0059] Further optionally, in the first functional conductive layer and the second functional conductive layer, the weight ratio of graphite, carbon black and carbon nanotubes is (92-97):(0.8-3):(0.8-3).

[0060] In this embodiment, the materials of the first functional conductive layer and the second functional conductive layer also include a bonding material. For example, the materials of the first functional conductive layer include a bonding material, graphite, carbon black and carbon nanotubes, and the graphite, carbon black and carbon nanotubes are bonded together by the bonding material to form a first functional conductive layer with buffer holes. Similarly, the materials of the second functional conductive layer include a bonding material, graphite, carbon black and carbon nanotubes, and the graphite, carbon black and carbon nanotubes are bonded together by the bonding material to form a second functional conductive layer with buffer holes.

[0061] In other embodiments, the material of the first functional conductive layer includes a bonding material and yttria-stabilized zirconia (YSZ), and the yttria-stabilized zirconia (YSZ) is bonded together by the bonding material.

[0062] In other embodiments, a porous oxide may be formed by evaporating oxide particles to form a functional conductive layer having buffer pores.

[0063] In this embodiment, the method for preparing the first functional conductive layer includes the following steps:

[0064] mixing a solvent, a binder, graphite, carbon black and carbon nanotubes to obtain a mixed slurry;

[0065] The mixed slurry is coated on the first metal layer, and the solvent is removed to obtain a first functional conductive layer.

[0066] Similarly, the preparation method of the second functional conductive layer includes the following steps:

[0067] mixing a solvent, a binder, graphite, carbon black and carbon nanotubes to obtain a mixed slurry;

[0068] The mixed slurry is coated on the second metal layer, and the solvent is removed to obtain a second functional conductive layer.

[0069] Optionally, the solvent is N-methylpyrrolidone (NMP) or water.

[0070] In other embodiments, if the bonding material itself is liquid, the solvent may be omitted when preparing the first functional conductive layer and the second functional conductive layer.

[0071] In this embodiment, when the mixed slurry is coated on the first metal layer and the second metal layer, the mixed slurry can be evenly distributed on the first metal layer and the second metal layer, which is equivalent to a secondary modification of the first metal layer and the second metal layer. The plating process of the first metal layer and the second metal layer is more tolerant, and some metal protrusions or wrinkles can be allowed to appear on the surface of the first metal layer and the second metal layer, thereby reducing the difficulty of plating the first metal layer and the second metal layer.

[0072] Optionally, the bonding material includes one or more of polyvinylidene fluoride (PVDF), vinyl cellulose and terpineol.

[0073] Optionally, the mass percentage of the bonding material in the first functional conductive layer and the second functional conductive layer is independently 0.1% to 50%.

[0074] In some examples, the first functional conductive layer and the second functional conductive layer each independently include vinylidene fluoride, graphite, carbon black and carbon nanotubes, and the mass percentage of vinylidene fluoride in the first functional conductive layer and the second functional conductive layer is each independently 0.1% to 10%. It can be understood that the mass percentage of vinylidene fluoride in the first functional conductive layer and the second functional conductive layer can be any value in any two numerical endpoint value ranges including 0.1%, 0.5%, 1%, 2%, 5% and 10%, respectively. Preferably, the mass percentage of vinylidene fluoride in the first functional conductive layer and the second functional conductive layer is each independently 0.1% to 5%. At this time, the porous carbon material composed of graphite, carbon black and carbon nanotubes is more evenly distributed.

[0075] In some examples, the first functional conductive layer and the second functional conductive layer include ethylene cellulose, pinene alcohol, and yttria-stabilized zirconia, and the ethylene cellulose and pinene alcohol are used as bonding materials, and their mass percentages in the first functional conductive layer and the second functional conductive layer are independently 30% to 50%. It can be understood that the mass percentages of ethylene cellulose and pinene alcohol as bonding materials in the first functional conductive layer and the second functional conductive layer can be any value in the range of any two numerical endpoints including 30%, 40% and 50%.

[0076] Optionally, the materials of the first metal layer and the second metal layer independently include one or more of copper (Cu), aluminum (Al), iron (Fe), cobalt (Co), nickel (Ni), titanium (Ti), zinc-copper alloy (Zn-Cu), aluminum-silver alloy (Al-Ag) and aluminum-tin alloy (Al-Sn).

[0077] Optionally, the thickness of the first metal layer and the second metal layer are independently 10 nm to 10000 nm. It is understandable that the thickness of the first metal layer and the second metal layer can be independently any value in any two numerical endpoint value ranges including two numerical endpoint values ​​of 10 nm, 50 nm, 100 nm, 500 nm, 1000 nm, 5000 nm and 10000 nm.

[0078] Optionally, the material of the polymer layer includes one or more of biaxially oriented polypropylene (OPP), polyethylene terephthalate (PET), polyimide (PI), polyethylene (PE) and polyethylene naphthalate (PEN).

[0079] Optionally, the thickness of the polymer layer is 1 μm to 40 μm. It is understood that the thickness of the polymer layer can be any value in any range of any two numerical endpoints including 1 μm, 5 μm, 10 μm, 20 μm, 30 μm and 40 μm.

[0080] In this implementation, please continue to refer to Figure 1 The polymer layer 10 is provided with a through hole 50 connecting the first metal layer 20 and the second metal layer 30. The presence of the through hole 50 can enhance the conductivity of the composite current collector.

[0081] In other embodiments, the polymer layer may not be provided with a through hole connecting the first metal layer and the second metal layer.

[0082] In this embodiment, the first metal layer 20 is provided with a first tab welding area, the area outside the first tab welding area is a first non-welding area, and the first functional conductive layer 401 is located in the first non-welding area. The second metal layer 30 is provided with a second tab welding area, the area outside the second tab welding area is a second non-welding area, and the second functional conductive layer 402 is located in the second non-welding area. This can prevent the high temperature generated when welding the tabs from melting the first functional conductive layer and the second functional conductive layer.

[0083] In this embodiment, the first tab welding area is located at the edge of the first metal layer 20 . Similarly, the second tab welding area is located at the edge of the second metal layer 30 .

[0084] It can be understood that by selecting the materials for the polymer layer, the first metal layer, the second metal layer and the functional conductive layer, the layers of the composite current collector can be tightly bonded, not easy to fall off, and not easy to be corroded, and at the same time have the characteristics of low barrier properties, high conductivity, light weight, high strength and good toughness.

[0085] The composite current collector of the present application may be a positive electrode current collector, a negative electrode current collector, or a bipolar current collector.

[0086] The composite current collector of the present application can be used in lithium-ion batteries and sodium-ion batteries. When used in lithium-ion batteries, the active ions in the battery charge and discharge process are lithium ions; when used in sodium-ion batteries, the active ions in the battery charge and discharge process are sodium ions.

[0087] One embodiment of the present application further provides an electrode plate, which includes a composite current collector and an electrode active layer located on the composite current collector; the composite current collector is the composite current collector as described above.

[0088] It can be understood that the electrode active layer can be a positive electrode active layer or a negative electrode active layer. When a positive electrode active layer is disposed on the composite current collector, the electrode plate can be a positive electrode plate; when a negative electrode active layer is disposed on the composite current collector, the electrode plate can be a negative electrode plate; when a positive electrode active layer and a negative electrode active layer are disposed on opposite sides of the composite current collector, the electrode plate is a bipolar plate.

[0089] The above-mentioned electrode plate has all the advantages of the above-mentioned composite current collector, which will not be described in detail here.

[0090] One embodiment of the present application further provides a battery, which includes a battery shell and an electrode plate located in the battery shell, and the electrode plate is the electrode plate as described above.

[0091] The above-mentioned battery has all the advantages of the above-mentioned composite current collector, which will not be described in detail here.

[0092] An embodiment of the present application further provides an electronic device, which includes a device body and a battery. The device body has a battery cavity. The battery is located in the battery cavity. The battery is the battery as described above.

[0093] The above electronic device has all the advantages of the above composite current collector, which will not be described in detail here.

[0094] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.

[0095] Example 1

[0096] This embodiment provides a composite current collector and a preparation method thereof, the steps are as follows:

[0097] Step 1: A PET film with a thickness of 6 μm and a through hole with a pore size of 0.1 μm is used as a polymer layer. A first aluminum layer with a thickness of 750 nm and a second aluminum layer with a thickness of 750 nm are formed on two opposite surfaces of the PET film to obtain an intermediate product.

[0098] Step 2: Mix 1884g of water, 425g of PVDF, 4699g of graphite, 31g of carbon black and 31g of carbon nanotubes to obtain a mixed slurry. Apply the mixed slurry on the first aluminum layer, evaporate the solvent, and obtain a first functional conductive layer with buffer holes with a thickness of 1μm. Apply the mixed slurry on the second aluminum layer, evaporate the solvent, and obtain a second functional conductive layer with buffer holes with a thickness of 1μm, that is, a composite current collector.

[0099] Example 2

[0100] This embodiment provides a composite current collector and a preparation method thereof, the steps are as follows:

[0101] Step 1: Take a PET film with a thickness of 6 μm and a through hole with a pore size of 0.1 μm as the polymer layer, and form a first aluminum layer with a thickness of 1000 nm and a second aluminum layer with a thickness of 1000 nm on opposite sides of the PET film to obtain an intermediate product.

[0102] Step 2: Mix 1884g of water, 51g of PVDF, 4990g of graphite, 83g of carbon black and 62g of carbon nanotubes to obtain a mixed slurry. Apply the mixed slurry on the first aluminum layer, evaporate the solvent, and obtain a first functional conductive layer with buffer holes with a thickness of 1μm. Apply the mixed slurry on the second aluminum layer, evaporate the solvent, and obtain a second functional conductive layer with buffer holes with a thickness of 1μm, thus obtaining a composite current collector.

[0103] Example 3

[0104] This embodiment provides a composite current collector and a preparation method thereof, the steps are as follows:

[0105] Step 1: Take a PET film with a thickness of 6 μm and a through hole with a pore size of 0.1 μm as the polymer layer, and form a first aluminum layer with a thickness of 1000 nm and a second aluminum layer with a thickness of 1000 nm on opposite sides of the PET film to obtain an intermediate product.

[0106] Step 2: Mix 1884g of water, 78g of PVDF, 4980g of graphite, 78g of carbon black and 52g of carbon nanotubes to obtain a mixed slurry. Apply the mixed slurry on the first aluminum layer, evaporate the solvent, and obtain a first functional conductive layer with buffer holes with a thickness of 0.3μm. Apply the mixed slurry on the second aluminum layer, evaporate the solvent, and obtain a second functional conductive layer with buffer holes with a thickness of 0.3μm, thus obtaining a composite current collector.

[0107] Example 4

[0108] This embodiment provides a composite current collector and a preparation method thereof, the steps are as follows:

[0109] Step 1: Take a PET film with a thickness of 6 μm and a through hole with a pore size of 0.1 μm as the polymer layer, and form a first aluminum layer with a thickness of 1000 nm and a second aluminum layer with a thickness of 1000 nm on opposite sides of the PET film to obtain an intermediate product.

[0110] Step 2: Vapor-deposit aluminum oxide particles on the first aluminum layer to obtain a first functional conductive layer with a thickness of 0.5 μm and buffer holes. Vapor-deposit aluminum oxide particles on the first aluminum layer to obtain a second functional conductive layer with a thickness of 0.5 μm and buffer holes, thereby obtaining a composite current collector.

[0111] Example 5

[0112] This embodiment provides a composite current collector and a preparation method thereof, the steps are as follows:

[0113] Step 1: Take a PET film with a thickness of 6 μm and a through hole with a pore size of 0.1 μm as the polymer layer, and form a first aluminum layer with a thickness of 1000 nm and a second aluminum layer with a thickness of 1000 nm on opposite sides of the PET film to obtain an intermediate product.

[0114] Step 2: Mix 400g of ethyl cellulose and 1600g of pine alcohol as a binder, add 3000g of yttria-stabilized zirconia (YSZ) and grind for 1.5h to obtain a mixed slurry. Apply the mixed slurry on the first aluminum layer, evaporate the solvent, and obtain a first functional conductive layer with buffer holes with a thickness of 1.5μm. Apply the mixed slurry on the second aluminum layer, evaporate the solvent, and obtain a second functional conductive layer with buffer holes with a thickness of 1.5μm, thus obtaining a composite current collector.

[0115] Comparative Example 1

[0116] In this comparative example, the intermediate product obtained in step 1 of Example 3 is used as the composite current collector.

[0117] test

[0118] Test 1: Scanning electron microscope test

[0119] The composite current collectors of Examples 1 to 5 were sampled and observed by scanning electron microscope, wherein the composite current collectors of Examples 1 to 3 were subjected to secondary processing by using focused ion beam cutting (FIB) technology, and the obtained images are as follows: Figures 2 to 4 shown.

[0120] from Figures 2 to 4 It can be seen from the ion beam cutting cross section that the porous carbon material is located on the aluminum layer. Compared with Example 1, the distribution of the porous carbon material in Example 2 and Example 3 is more uniform.

[0121] Test 2: Based on the SEM test images of the composite current collectors of Examples 1 to 5, the pore size range of the buffer pores was obtained. The results are shown in Table 1.

[0122] Test 3: Using LB-092 electrolyte as the test electrolyte, the contact angle of the electrolyte on the surface of the composite current collector of each embodiment and comparative example was tested. The results are shown in Table 1.

[0123] Test 4: The surface resistance and conductivity of the composite current collectors of the above embodiments and comparative examples were tested. The results are shown in Table 1.

[0124] Table 1

[0125] Pore ​​size (nm) Contact angle (°) Square resistance (□ / mΩ) Conductivity (S / cm) Example 1 100~300 36 50 <![CDATA[1.77×10 5 ]]> Example 2 100~200 30 40 <![CDATA[1.80×10 5 ]]> Example 3 100~200 31 40 <![CDATA[1.79×10 5 ]]> Example 4 100~300 40 60 <![CDATA[1.76×10 5 ]]> Example 5 300~600 45 70 <![CDATA[1.75×10 5 ]]> Comparative Example 1 \ 40 40 <![CDATA[1.88×10 5 ]]>

[0126] Note: “\” indicates that the aperture was not observed.

[0127] Test 5: Battery performance test

[0128] Take the composite current collector of Example 3 and the composite current collector of Comparative Example 1, use lithium cobalt oxide as the positive electrode active material and graphite as the negative electrode active material, prepare the positive electrode sheet of Example 3 and the negative electrode sheet of Comparative Example 1 respectively, and further prepare the battery cell of Example 3 and the battery cell of Comparative Example 1.

[0129] The battery cells of Example 3 and the battery cells of Comparative Example 1 were subjected to rate charge and discharge tests: the test procedure was a rate charging tester, the battery cells were charged at 1C / 3C / 4C rates, and discharged at 0.2C, the charging procedure selected constant current and constant voltage charging, the charging current was set to 5A / 15A / 20A, the voltage was 4.45V, and the cut-off current was 0.05C, i.e. 250mA. Each rate cycle was repeated 3 times, and the first cycle data of each rate charge was taken to make a capacity-voltage graph. At the same time, a new y-axis was added to make a capacity-time graph. The results are shown in Figures 5 to 7 ,in, Figure 5 This is the test result chart of charging at 1C rate and discharging at 0.2C. Figure 6 This is the test result chart of charging at 3C rate and discharging at 0.2C. Figure 7 This is the test result diagram of charging at 4C rate and discharging at 0.2C.

[0130] from Figure 5-7 From the capacity-voltage graph, we can easily see that, compared with Comparative Example 1, the battery cell of Example 3 reaches the 4.45V voltage platform later in the rate charging process, indicating that the battery cell of Example 3 is less polarized during the charging process; at the same time, during the 0.2C discharge process, it can be seen that the battery cell of Example 3 releases a capacity of about 5800mAh, while the battery cell of Comparative Example 1 releases a capacity of about 5600mAh. Figure 5-7From the capacity-time curve, it can be found that, compared with Comparative Example 1, the battery cell of Example 3 requires a shorter time to charge to the same capacity, and the constant current charging capacity (straight line portion) increases.

[0131] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0132] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A composite current collector, characterized in that: Comprising a polymer layer, a first metal layer, a second metal layer and a functional conductive layer: The first metal layer and the second metal layer are respectively located on opposite sides of the polymer layer; The functional conductive layer comprises a first functional conductive layer and / or a second functional conductive layer; the first functional conductive layer is located on a side of the first metal layer away from the polymer layer, and the second functional conductive layer is located on a side of the second metal layer away from the polymer layer; The first functional conductive layer and the second functional conductive layer each independently have a buffer hole.

2. The composite current collector according to claim 1, characterized in that: The aperture of the buffer hole satisfies the following conditions 1) or 2): 1) During the charge and discharge process, the metal ions released from the first metal layer and / or the second metal layer cannot be discharged through the buffer pores; 2) During the charge and discharge process, metal ions released from the first metal layer and / or the second metal layer cannot enter the buffer pores.

3. The composite current collector according to claim 2, characterized in that: The buffer hole has a pore diameter of 1 nm to 10000 nm.

4. The composite current collector according to claim 1, characterized in that: The thickness of the first functional conductive layer and the second functional conductive layer are each independently 0.001 μm to 40 μm.

5. The composite current collector according to any one of claims 1 to 4, characterized in that: The materials of the first functional conductive layer and the second functional conductive layer include one or more of porous carbon materials, foamed metals, porous conductive liquid crystal polymers, porous oxides, and yttria-stabilized zirconia.

6. The composite current collector according to claim 5, characterized in that: The porous carbon material includes one or more of graphite, soft carbon, hard carbon, carbon nanotubes and graphene.

7. The composite current collector according to claim 6, characterized in that: The hard carbon includes one or more of carbon black, resin carbon, and organic polymer pyrolytic carbon.

8. The composite current collector according to claim 5, characterized in that: The porous carbon material includes graphite, carbon black and carbon nanotubes.

9. The composite current collector according to claim 8, characterized in that: The weight ratio of the graphite, carbon black and carbon nanotubes is (80-97):(0.1-5):(0.1-5).

10. The composite current collector according to claim 5, characterized in that: The foam metal includes one or more of foam copper, foam aluminum, foam iron, foam cobalt, foam nickel and foam titanium.

11. The composite current collector according to claim 5, characterized in that: The porous oxide includes one or more of porous aluminum oxide and porous copper oxide.

12. The composite current collector according to claim 5, characterized in that: The materials of the first functional conductive layer and the second functional conductive layer further include a bonding material.

13. The composite current collector according to claim 12, characterized in that: The bonding material satisfies at least one of the following conditions 1) and 2): 1) The bonding material includes one or more of polyvinylidene fluoride, ethylene cellulose and terpineol; 2) The mass percentage of the bonding material in the first functional conductive layer and the second functional conductive layer is independently 0.1% to 50%.

14. The composite current collector according to any one of claims 1 to 4 and 6 to 13, characterized in that: The composite current collector satisfies at least one of the following conditions 1) to 6): 1) The materials of the first metal layer and the second metal layer independently include one or more of copper, aluminum, iron, cobalt, nickel, titanium, zinc-copper alloy, aluminum-silver alloy and aluminum-tin alloy; 2) The thickness of the first metal layer and the second metal layer are independently 10 nm to 10000 nm; 3) The material of the polymer layer includes one or more of biaxially oriented polypropylene, polyethylene terephthalate, polyimide, polyethylene and polyethylene naphthalate; 4) The thickness of the polymer layer is 1 μm to 40 μm; 5) The polymer layer is provided with a through hole connecting the first metal layer and the second metal layer; 6) A first tab welding area is provided on the first metal layer, an area outside the first tab welding area is a first non-welding area, and the first functional conductive layer is located in the first non-welding area; a second tab welding area is provided on the second metal layer, an area outside the second tab welding area is a second non-welding area, and the second functional conductive layer is located in the second non-welding area.

15. An electrode plate, characterized in that: It comprises a composite current collector and an electrode active layer located on the composite current collector; the composite current collector is the composite current collector according to any one of claims 1 to 14.

16. A battery, characterized in that: It comprises a battery shell and an electrode plate located in the battery shell, and the electrode plate is the electrode plate as claimed in claim 15.

17. An electronic device, characterized in that: The device comprises a device body and a battery, wherein the device body has a battery cavity, the battery is located in the battery cavity, and the battery is the battery as claimed in claim 16.

Citation Information

Cited By

  • Bipolar current collector, preparation method therefor, bipolar electrode sheet, and bipolar battery