Polyurethane coated diaphragm as well as preparation method and application thereof
By using polyurethane to coat the separator in lithium-ion batteries and using the soft and hard segment structure of crosslinked polyurethane, the problem of polyolefin separator is easily contracted and poor wetting at high temperatures is solved, and the overall performance and safety of the battery are improved.
Patent Information
- Application Number
- CN202411120580.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The polyolefin separators in existing lithium-ion batteries are prone to shrink and have poor wetting properties at high temperatures, which limits the performance and cycle life of the battery. Existing modification methods such as inorganic coating have problems such as poor adhesion and reduced energy density.
The polyurethane coating is used to coat the separator, and the cross-linking polyurethane coating is prepared through polycondensation, chain extension and cross-linking reaction of polymer diol and diisocyanate. Combined with the soft and hard segment structure, the mechanical properties and wettability of the separator are improved.
It significantly improves the comprehensive performance of lithium-ion batteries, enhances the dimensional stability and electrochemical performance of the separator, reduces the heat shrinkage rate at high temperatures, and improves the safety and electrochemical performance of the battery.
Smart Images

Figure CN118943637A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to a polyurethane coated diaphragm and a preparation method and application thereof. Background Art
[0002] The main function of the separator is to be placed between the positive and negative electrodes, allowing rapid transmission of ionic charge carriers and preventing direct contact between the electrodes. Although the separator is an inactive component of the battery, the characteristics of the separator will affect the ion transport, cycle life, performance and safety of the battery. In view of the development trend of secondary batteries, especially lithium-ion batteries, towards high energy density and long cycle life, the currently used polyolefin separators have poor wettability with electrolytes and severe shrinkage at high temperatures, which limits their application. To this end, researchers have adopted coating, radiation grafting, blending and other methods to modify polyolefin separators, among which coating modification is one of the simplest and most effective methods.
[0003] There are two types of coating modification: inorganic coating and organic coating. Inorganic coating uses ceramic particles such as alumina and boehmite to modify polyolefin diaphragms to improve the wettability and dimensional stability of the diaphragm. However, the adhesion between the ceramic particles and the base film is poor and they are easy to fall off, resulting in a decrease in cycle life; in addition, ceramic particles will significantly increase the mass of the diaphragm, resulting in a decrease in energy density. Organic coatings mostly use polymers such as aramid and polyvinylidene fluoride. These materials have strong adhesion and can enhance the cycle life of the battery, but they do not significantly improve the capacity and cycle stability of lithium batteries, and it is difficult for them to have the ability to enhance dimensional stability and mechanical properties. Summary of the invention
[0004] In response to one or more of the above defects or improvement needs in the prior art, the present invention provides a polyurethane coated diaphragm and a preparation method and application thereof, which solves the problems of easy heat shrinkage and poor wettability of polyolefin diaphragms and improves the comprehensive performance of lithium-ion batteries.
[0005] To achieve the above-mentioned purpose, according to the first aspect of the present invention, there is provided a polyurethane coated diaphragm, characterized in that it comprises a base film and a coating layer arranged on the surface of at least one side of the base film; the base film is a polyolefin film, the polyolefin film is one of polyethylene, polypropylene, polypropylene / polyethylene / polypropylene composite diaphragm, and the coating layer is polyurethane.
[0006] As a further improvement of the present invention, the polyurethane has a cross-linked structure, and the cross-linking density of the polyurethane is 10% to 30%; the structural formula of the polyurethane is shown in formula (1):
[0007]
[0008] As a further improvement of the present invention, the polyurethane comprises a soft segment and a hard segment; the soft segment is a polymer diol, and the hard segment is a diisocyanate; the molar ratio of the polymer diol to the diisocyanate is 1:2 to 1:2.5.
[0009] As a further improvement of the present invention, the thickness of the coating layer is 1 to 3 μm.
[0010] According to a second aspect of the present invention, there is provided a method for preparing a polyurethane coated diaphragm, comprising the following steps:
[0011] (1) using a polymer diol as a soft segment raw material and a diisocyanate as a hard segment raw material, mixing the soft segment raw material and the hard segment raw material in a first solvent for polycondensation reaction to obtain an isocyanate-terminated polyurethane prepolymer;
[0012] The molar ratio of the polymer diol to the diisocyanate is 1:2 to 1:2.5;
[0013] (2) mixing the polyurethane prepolymer obtained in step (1) with an amino or hydroxyl terminated chain extender in a first solvent to carry out a chain extension reaction to obtain a polyurethane chain extension prepolymer;
[0014] The molar ratio of the chain extender to the diisocyanate is 0.2:1 to 0.4:1;
[0015] (3) mixing the polyurethane chain extension prepolymer obtained in step (2) with a crosslinking agent in a first solvent to carry out a crosslinking reaction to obtain a crosslinked polyurethane;
[0016] The molar ratio of the crosslinking agent to the diisocyanate is 0.2:1 to 0.7:1;
[0017] (4) dissolving the cross-linked polyurethane obtained in step (3) in a second solvent, heating at 30 to 80° C. and stirring uniformly to obtain a coating slurry;
[0018] (5) coating the coating slurry obtained in step (4) on one side or both sides of the base film, and obtaining the polyurethane coated diaphragm after curing;
[0019] Wherein, the base film is one of polyethylene, polypropylene, and polypropylene / polyethylene / polypropylene composite membrane.
[0020] As a further improvement of the present invention, the cross-linking density of the cross-linked polyurethane is 10% to 30%; preferably, the structural formula of the cross-linked polyurethane is as shown in formula (1):
[0021]
[0022] As a further improvement of the present invention, the polymer diol is selected from one or more of polytetrahydrofuran, polycaprolactone, and polycarbonate; and / or,
[0023] The diisocyanate is selected from one or more of hexamethylene diisocyanate and dicyclohexylmethane diisocyanate; and / or,
[0024] The chain extender is a diamino or dihydroxy chain extender, selected from one or more of N,N'-bis(2-hydroxyethyl)oxalamide and tartaric acid; and / or,
[0025] The cross-linking agent is selected from one or more of polyamine compounds and phenylboronic acid compounds.
[0026] As a further improvement of the present invention, the first solvent is one or more of N-methylpyrrolidone, dimethylformamide and tetrahydrofuran; and / or,
[0027] The second solvent is one or more of dichloromethane, dimethylformamide and tetrahydrofuran.
[0028] As a further improvement of the present invention, the polycondensation reaction in step (1), the chain extension reaction in step (2) and the cross-linking reaction in step (3) are all carried out under the action of a catalyst; the catalyst is an amine, tin or bismuth catalyst; and / or,
[0029] In the polycondensation reaction in step (1), the chain extension reaction in step (2) and the cross-linking reaction in step (3), the reaction temperature is 30 to 70° C. and the reaction time is 12 to 24 hours.
[0030] As a further improvement of the present invention, in step (5), the coating method is one of gravure coating, blade coating, and anilox roller coating.
[0031] According to a third aspect of the present invention, there is provided an application of a polyurethane coated separator in a secondary battery, wherein the polyurethane coated separator is used, or the polyurethane coated separator is prepared by the preparation method.
[0032] In general, the above technical solution conceived by the present invention has the following beneficial effects compared with the prior art:
[0033] (1) The present invention prepares a modified diaphragm with excellent comprehensive performance. The unique soft and hard segments and cross-linked structure give the polyurethane high strength and toughness, further improving the mechanical properties of the diaphragm, reducing the risk of lithium dendrites penetrating the diaphragm, and increasing battery safety; the molecular mobility of the cross-linked polyurethane coating is reduced, so it has excellent dimensional stability at high temperatures, greatly reducing the thermal shrinkage rate of the diaphragm at high temperatures, and reducing the risk of thermal runaway of the diaphragm at high temperatures; polyurethane contains rich polar groups and hydrogen bonds, which can effectively improve the wettability of the diaphragm with the electrolyte, increase the interface compatibility between the diaphragm and the electrode, promote ion transmission, and achieve improved electrochemical and battery performance.
[0034] (2) The present invention adopts a coating method to prepare a polyurethane coated diaphragm. The process is simple and shows commercial potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The long cycle performance comparison of lithium iron phosphate batteries assembled with polyurethane-coated polypropylene diaphragms and uncoated polypropylene diaphragms prepared in Example 1 of the present invention at a rate of 1C is shown;
[0036] Figure 2 The dimensional stability comparison of the polyurethane-coated polypropylene diaphragm and the uncoated polypropylene diaphragm at different temperatures prepared in Example 1 of the present invention is shown;
[0037] Figure 3 is the lithium ion migration number of the lithium symmetric battery assembled with the polyurethane coated diaphragm prepared in Example 2;
[0038] Figure 4 Lithium ion transference number of lithium symmetric battery assembled without coated separator;
[0039] Figure 5 The contact angle comparison between the polyurethane coated separator and the uncoated separator prepared in Example 3 of the present invention and the electrolyte;
[0040] Figure 6 Comparison of the stress-strain curves in the transverse direction of the polyurethane coated diaphragm and the uncoated diaphragm prepared in Example 4 of the present invention;
[0041] Figure 7 Comparison of longitudinal stress-strain curves of the polyurethane coated diaphragm and the uncoated diaphragm prepared in Example 4 of the present invention;
[0042] Figure 8 The electrochemical stability window test results of the polyurethane coated diaphragm and the uncoated diaphragm prepared in Example 5 of the present invention;
[0043] Fig. 9The ionic conductivity-temperature images of the polyurethane coated membrane and the uncoated membrane prepared in Example 6 of the present invention;
[0044] Fig.10 The dimensional stability comparison is between the polypropylene diaphragm, the cross-linked polyurethane coated diaphragm in Example 1 and the non-cross-linked polyurethane coated diaphragm in Comparative Example 1;
[0045] Fig.11 The long cycle performance of lithium iron phosphate batteries assembled with polyurethane coated diaphragms with coating thickness of 3 μm in Example 1 and 5 μm in Comparative Example 2 at a 1C rate is compared. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0047] As a preferred embodiment of the present invention, a polyurethane coated diaphragm is provided, comprising a base film and a coating layer arranged on at least one surface of the base film; the base film is a polyolefin film, the polyolefin film is one of polyethylene, polypropylene, polypropylene / polyethylene / polypropylene composite diaphragm, and the coating layer is polyurethane.
[0048] As a polymer with flexible structural design, easy modification and diverse functions, polyurethane has certain ion transport capabilities, excellent mechanical properties, abundant polar groups and hydrogen bond interactions, and good thermal stability. It has the potential to improve the wettability, dimensional stability, mechanical properties, electrochemical properties and battery performance of polyolefin separators.
[0049] Preferably, the polyurethane of the embodiment of the present invention is a polyurethane with a cross-linked structure, which is synthesized by a soft segment, a hard segment, a chain extender and a cross-linking agent, and the cross-linking density of the polyurethane is 10% to 30%, and its structural formula is shown in Formula (I):
[0050]
[0051] Preferably, the thickness of the coating layer of the polyurethane-coated diaphragm is 1 to 3 μm.
[0052] Furthermore, as a preferred embodiment of the present invention, a method for preparing a polyurethane coated diaphragm is provided, comprising the following steps:
[0053] (1) using a polymer diol as a soft segment raw material and a diisocyanate as a hard segment raw material, mixing the soft segment raw material and the hard segment raw material in a first solvent for polycondensation reaction to obtain an isocyanate-terminated polyurethane prepolymer;
[0054] Preferably, the molar ratio of polymer diol to diisocyanate is 1:2 to 1:2.5;
[0055] (2) mixing the polyurethane prepolymer obtained in step (1) with an amino or hydroxyl terminated chain extender in a first solvent to carry out a chain extension reaction to obtain a polyurethane chain extension prepolymer;
[0056] Preferably, the molar ratio of the chain extender to the diisocyanate in step (1) is 0.2:1 to 0.4:1;
[0057] (3) mixing the chain extension prepolymer obtained in step (2) with a crosslinking agent in a first solvent to carry out a crosslinking reaction to obtain a crosslinked polyurethane;
[0058] Preferably, the molar ratio of the crosslinking agent to the diisocyanate is 0.2:1 to 0.7:1, and the crosslinking density of the polyurethane is 10% to 30%;
[0059] (4) dissolving the cross-linked polyurethane obtained in step (3) in a second solvent, heating at 30 to 80° C. and stirring uniformly to obtain a coating slurry;
[0060] (5) coating the coating slurry obtained in step (4) on one side or both sides of the base film, and obtaining a polyurethane coated diaphragm after curing; wherein the base film is one of polyethylene, polypropylene, and polypropylene / polyethylene / polypropylene composite diaphragm.
[0061] Further preferably, the polycondensation reaction in step (1), the chain extension reaction in step (2) and the cross-linking reaction in step (3) are all carried out under the action of a catalyst. More preferably, the catalysts are all amine, tin or bismuth catalysts; more preferably, in the above reactions, the reaction temperature is 30 to 70°C and the reaction time is 12 to 24 hours.
[0062] Further preferably, in step (1), the polymer diol of the soft segment is selected from one or more of polytetrahydrofuran, polycaprolactone, and polycarbonate; the diisocyanate of the hard segment is selected from one or more of hexamethylene diisocyanate and dicyclohexylmethane diisocyanate; in step (2), the chain extender is a diamino or dihydroxy chain extender selected from one or more of N,N'-di(2-hydroxyethyl)oxamide and tartaric acid; in step (3), the crosslinking agent is selected from one or more of polyamine compounds and phenylboronic acid-containing compounds.
[0063] Further preferably, in steps (1), (2) and (3), the first solvent is one or more of N-methylpyrrolidone, dimethylformamide and tetrahydrofuran; in step (4), the second solvent is one or more of dichloromethane, dimethylformamide and tetrahydrofuran.
[0064] Further preferably, in step (5), the coating method is one of gravure coating, blade coating, and anilox roller coating.
[0065] The technical solution of the present invention is further described below by listing embodiments and comparative examples, but the present invention is not limited to these embodiments.
[0066] Example 1
[0067] The polyurethane coated diaphragm of this embodiment is synthesized by polycaprolactone diol (soft segment), dicyclohexylmethane diisocyanate (hard segment), tartaric acid (chain extender) and 3-aminophenylboronic acid (cross-linking agent), wherein the molar ratio of the soft and hard segments is 1:2 and the cross-linking density is 10%.
[0068] The polyurethane coated diaphragm of this embodiment is prepared according to the following steps:
[0069] Step 1, preparation of polyurethane: dissolve dihydroxy-terminated polycaprolactone diol (2mmol) with a relative molecular mass of 1000 in N-methylpyrrolidone to obtain a polymer solution; dissolve dicyclohexylmethane diisocyanate (4mmol) in an appropriate amount of N-methylpyrrolidone to obtain an isocyanate solution; add the above isocyanate solution to the polymer solution, add 3 drops of dibutyltin dilaurate, and then heat to 65°C to react for 12 hours to obtain a polyurethane prepolymer. Dissolve tartaric acid (1.58mmol) in a small amount of N-methylpyrrolidone, then add the obtained tartaric acid solution to the polyurethane prepolymer and react at 65°C for 12 hours, then cool to 30°C, add 3-aminophenylboronic acid (0.84mmol) and continue to react at 30°C for 24 hours. Pour the obtained solution into a polytetrafluoroethylene mold, and obtain polyurethane after evaporating the solvent.
[0070] Step 2, preparation of a polyurethane coated diaphragm: dissolve polyurethane in dichloromethane, stir evenly at 30°C to obtain a coating slurry; apply the coating slurry to one side of a 12μm polypropylene diaphragm by blade coating, and obtain a polyurethane coated diaphragm after drying, wherein the thickness of the polyurethane coating layer is 3μm.
[0071] The polyurethane coated separator obtained in this example is applied to the field of secondary batteries and assembled into button batteries.
[0072] Figure 1The long cycle performance of the Li / SSE / LiFePO4 battery with the polyurethane coated diaphragm prepared in this example is compared with that of the uncoated diaphragm. It can be seen that the initial capacity of the battery with the polyurethane coated diaphragm is increased from 114 mAh g -1 Up to 130mAh g -1 The coated diaphragm still has a capacity retention rate of 90% after 1100 charge and discharge cycles at a 1C rate, greatly improving the battery life.
[0073] Figure 2 The dimensional stability comparison between the polyurethane coated diaphragm and the uncoated diaphragm prepared in this example shows that the dimensional stability of the polypropylene diaphragm coated with polyurethane is significantly enhanced, and there is basically no thermal shrinkage at different temperatures, while the polypropylene diaphragm has severe thermal shrinkage.
[0074] Example 2
[0075] The polyurethane coated diaphragm of this embodiment is synthesized by polytetramethylene diol and polycarbonate diol (soft segment), hexamethylene diisocyanate (hard segment), N,N'-bis(2-hydroxyethyl)oxamide (chain extender) and 3-aminophenylboronic acid (cross-linking agent), wherein the molar ratio of the soft segment to the hard segment is 1:2.5, and the cross-linking density is 30%.
[0076] The polyurethane coated diaphragm of this embodiment is prepared according to the following steps:
[0077] Step 1, preparation of polyurethane: dissolve dihydroxy-terminated polytetrahydrofuran diol (1 mmol) with a relative molecular mass of 850 and polycarbonate diol (1 mmol) with a relative molecular mass of 2000 in anhydrous dimethylformamide to obtain a polymer solution; dissolve hexamethylene diisocyanate (5 mmol) in an appropriate amount of anhydrous dimethylformamide to obtain an isocyanate solution; add the above isocyanate solution to the polymer solution, add 5 drops of dimethylcyclohexylamine, and heat to 70°C for reaction for 12 hours to obtain a polyurethane prepolymer. Dissolve N,N'-bis(2-hydroxyethyl)oxamide (1.15 mmol) in a small amount of anhydrous dimethylformamide, add the obtained N,N'-bis(2-hydroxyethyl)oxamide solution to the polyurethane prepolymer, react at 70°C for 12 hours, then cool to 30°C, add 3-aminophenylboronic acid (3.5 mmol) and continue to react at 30°C for 24 hours. The obtained solution is poured into a polytetrafluoroethylene mold, and polyurethane is obtained after the solvent is evaporated.
[0078] Step 2, preparation of a polyurethane coated diaphragm: dissolve polyurethane in tetrahydrofuran, stir evenly at 30°C to obtain a coating slurry; use an anilox roller coating method to apply the coating slurry to one side of a 20μm polyethylene diaphragm, and obtain a polyurethane coated diaphragm after drying, wherein the thickness of the polyurethane coating layer is 1μm.
[0079] The polyurethane coated separator obtained in this example is applied to the field of secondary batteries and assembled into button batteries.
[0080] Figure 3 and Figure 4 The comparison of the lithium ion migration number of the lithium symmetric battery assembled with the polyurethane coated diaphragm prepared in this example and the uncoated diaphragm shows that the polyurethane coating is more conducive to ion conduction and effectively improves the lithium ion migration number compared with the uncoated diaphragm.
[0081] Example 3
[0082] The polyurethane coated diaphragm of this embodiment is synthesized by polycaprolactone diol (soft segment), dicyclohexylmethane diisocyanate (hard segment), tartaric acid (chain extender) and triethanolamine (cross-linking agent), wherein the molar ratio of the soft segment to the hard segment is 1:2.2 and the cross-linking density is 11%.
[0083] The polyurethane coated diaphragm of this embodiment is prepared according to the following steps:
[0084] Step 1, preparation of polyurethane: dissolve dihydroxy-terminated polycaprolactone diol (2mmol) with a relative molecular mass of 1000 in anhydrous tetrahydrofuran to obtain a polymer solution; dissolve dicyclohexylmethane diisocyanate (4.4mmol) in an appropriate amount of anhydrous tetrahydrofuran to obtain an isocyanate solution; add the above isocyanate solution to the polymer solution, add 4 drops of bismuth isooctanoate, and then heat to 60°C and react for 24h to obtain a polyurethane prepolymer. Dissolve tartaric acid (0.87mmol) in a small amount of anhydrous tetrahydrofuran, then add the obtained tartaric acid solution to the polyurethane prepolymer and react at 60°C for 12h, then add triethanolamine (0.88mmol) and continue to react at 60°C for 24h. Pour the obtained solution into a polytetrafluoroethylene mold, and obtain a polyurethane after evaporating the solvent.
[0085] Step 2, preparation of polyurethane coated diaphragm: dissolve polyurethane in dimethylformamide, stir evenly at 80°C to obtain coating slurry; apply the coating slurry to both sides of a 30μm PP / PE / PP composite diaphragm by blade coating, and obtain a polyurethane coated diaphragm after drying, wherein the coating thickness on both sides is 1μm.
[0086] Figure 5The contact angles of the coated and uncoated separators prepared in this example with the electrolyte are shown in Figure 2. It can be seen that the wettability of the separator coated with polyurethane with the electrolyte is improved, and the contact angle is reduced from 56° to 35°.
[0087] Example 4
[0088] The polyurethane coated diaphragm of this embodiment is synthesized by polytetramethylene glycol (soft segment), dicyclohexylmethane diisocyanate (hard segment), tartaric acid (chain extender) and 3-aminophenylboronic acid (cross-linking agent), wherein the molar ratio of the soft segment to the hard segment is 1:2 and the cross-linking density is 22%.
[0089] The polyurethane coated diaphragm of this embodiment is prepared according to the following steps:
[0090] Step 1, preparation of polyurethane: dissolve dihydroxy-terminated polytetrahydrofuran diol (0.5 mol) with a relative molecular mass of 850 in anhydrous dimethylformamide to obtain a polymer solution; dissolve dicyclohexylmethane diisocyanate (1 mol) in an appropriate amount of anhydrous dimethylformamide to obtain an isocyanate solution; add the above isocyanate solution to the polymer solution, add 12 ml of dimethylcyclohexylamine dropwise, and heat to 70°C for reaction for 24 hours to obtain a polyurethane prepolymer. Dissolve tartaric acid (0.25 mol) in anhydrous dimethylformamide, add the obtained tartaric acid solution dropwise to the polyurethane prepolymer and react at 70°C for 24 hours, then cool to 30°C, add 3-aminophenylboronic acid (0.5 mol) and continue to react at 30°C for 24 hours. Pour the obtained solution into a polytetrafluoroethylene mold, and volatilize the solvent to obtain a polyurethane.
[0091] Step 2, preparation of polyurethane coated diaphragm: dissolve polyurethane in tetrahydrofuran, stir evenly at 30°C to obtain coating slurry; use anilox roller coating to apply the coating slurry to both sides of the 30μm PP / PE / PP composite diaphragm, and obtain a polyurethane coated diaphragm after drying, wherein the coating thickness on both sides is 1μm.
[0092] Figure 6 and Figure 7 The stress-strain curves of the coated diaphragm and the uncoated diaphragm prepared in this example in the transverse and longitudinal directions respectively. It can be seen that the tensile strength and elongation at break of the diaphragm coated with polyurethane are improved, further enhancing the mechanical properties of the diaphragm.
[0093] Example 5
[0094] The polyurethane coated diaphragm of this embodiment is synthesized by polycarbonate diol (soft segment), hexamethylene diisocyanate (hard segment), N,N'-di(2-hydroxyethyl)oxamide (chain extender) and triethanolamine (cross-linking agent), wherein the molar ratio of the soft and hard segments is 1:2 and the cross-linking density is 25%.
[0095] The polyurethane coated diaphragm of this embodiment is prepared according to the following steps:
[0096] Step 1, preparation of polyurethane: dissolve dihydroxy-terminated polycarbonate diol (0.5 mol) with a relative molecular mass of 1000 in anhydrous tetrahydrofuran to obtain a polymer solution; dissolve hexamethylene diisocyanate (1 mol) in an appropriate amount of anhydrous tetrahydrofuran to obtain an isocyanate solution; add the above isocyanate solution to the polymer solution, add 10 ml of bismuth isooctanoate dropwise, and then heat to 60°C and react for 24 hours to obtain a polyurethane prepolymer. Dissolve N, N'-di(2-hydroxyethyl) oxamide (0.3 mol) in anhydrous tetrahydrofuran, add the obtained N, N'-di(2-hydroxyethyl) oxamide solution dropwise to the polyurethane prepolymer and react at 60°C for 24 hours, then add triethanolamine (0.6 mol) and continue to react at 60°C for 24 hours. Pour the obtained solution into a polytetrafluoroethylene mold, and obtain a polyurethane after the solvent is evaporated.
[0097] Step 2, preparation of polyurethane coated diaphragm: dissolve polyurethane in dimethylformamide, stir evenly at 80°C to obtain coating slurry; use anilox roller coating to apply the coating slurry to one side of a 12μm polypropylene diaphragm, and obtain a polyurethane coated diaphragm after drying, wherein the thickness of the polyurethane coating layer is 3μm.
[0098] The polyurethane coated separator obtained in this example is applied to the field of secondary batteries and assembled into button batteries.
[0099] Figure 8 The electrochemical stability window test results of the polyurethane coated membrane and the uncoated membrane prepared in the embodiment of the present invention are compared. Due to the excellent chemical stability of the polyurethane coating, the electrochemical stability window of the polyurethane coated membrane is 5.0V, which is higher than that of the uncoated membrane (4.5V).
[0100] Example 6
[0101] The polyurethane coated diaphragm of this embodiment is synthesized by polycaprolactone diol (soft segment), hexamethylene diisocyanate (hard segment), N,N'-bis(2-hydroxyethyl)oxamide (chain extender) and 3-aminophenylboronic acid (cross-linking agent), wherein the molar ratio of the soft and hard segments is 1:2 and the cross-linking density is 17%.
[0102] The polyurethane coated diaphragm of this embodiment is prepared according to the following steps:
[0103] Step 1, preparation of polyurethane: dissolve dihydroxy-terminated polycaprolactone diol (0.5 mol) with a relative molecular mass of 1000 in N-methylpyrrolidone to obtain a polymer solution; dissolve hexamethylene diisocyanate (1 mol) in an appropriate amount of N-methylpyrrolidone to obtain an isocyanate solution; add the above isocyanate solution to the polymer solution, add 12 ml of dibutyltin dilaurate dropwise, and then heat to 65°C and react for 24 hours to obtain a polyurethane prepolymer. Dissolve N,N'-bis(2-hydroxyethyl)oxamide (0.4 mol) in a small amount of N-methylpyrrolidone, then add the obtained N,N'-bis(2-hydroxyethyl)oxamide solution dropwise to the polyurethane prepolymer and react at 65°C for 24 hours, then cool to 30°C, add 3-aminophenylboronic acid (0.4 mol) and continue to react at 30°C for 24 hours. Pour the obtained solution into a polytetrafluoroethylene mold, and volatilize the solvent to obtain a polyurethane.
[0104] Step 2, preparation of a polyurethane coated diaphragm: dissolve polyurethane in dichloromethane, stir evenly at 30°C to obtain a coating slurry; apply the coating slurry to one side of a 12μm polypropylene diaphragm by blade coating, and obtain a polyurethane coated diaphragm after drying, wherein the thickness of the polyurethane coating layer is 1μm.
[0105] The polyurethane coated separator obtained in this example is applied to the field of secondary batteries and assembled into button batteries.
[0106] Fig. 9 The ionic conductivity-temperature images of the polyurethane coated membrane and the uncoated membrane prepared in the embodiment of the present invention. Since the polyurethane coating can improve the wettability of the membrane and promote the dissociation of lithium salts, the ionic conductivity of the polyurethane coated membrane is higher than that of the uncoated membrane at different temperatures.
[0107] Comparative Example 1
[0108] In this comparative example, 3-aminophenylboronic acid in step 1 of Example 1 was deleted, and the rest was consistent with Example 1. Fig.10 By comparing the dimensional stability of the polypropylene membrane, the cross-linked polyurethane coated membrane in Example 1 and the uncross-linked polyurethane coated membrane in Comparative Example 1, it can be seen that the dimensional stability of the uncross-linked polyurethane coated membrane is greatly reduced, indicating that the cross-linked structure of the polyurethane has a greater influence on the dimensional stability of the membrane.
[0109] Comparative Example 2
[0110] In this comparative example, the coating thickness in step 2 of Example 1 was increased to 5 μm, and the rest was consistent with Example 1. Fig.11The long cycle performance of Li / SSE / LiFePO4 batteries with polyurethane coated diaphragms of 3 μm in Example 1 and 5 μm in Comparative Example 2 is compared. It can be seen that the increase in thickness leads to a decrease in energy density, so the discharge specific capacity of the Li / SSE / LiFePO4 battery assembled with the obtained coated diaphragm is significantly reduced, indicating that the coating thickness has a great influence on the dimensional stability of the diaphragm and the battery performance.
[0111] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A polyurethane coated diaphragm, characterized in that: It comprises a base film and a coating layer arranged on at least one side of the base film; the base film is a polyolefin film, the polyolefin film is one of polyethylene, polypropylene, polypropylene / polyethylene / polypropylene composite membrane, and the coating layer is polyurethane.
2. The polyurethane coated diaphragm according to claim 1, characterized in that: The polyurethane has a cross-linked structure, and the cross-linking density of the polyurethane is 10% to 30%. Preferably, the structural formula of the polyurethane is as shown in formula (1):
3. The polyurethane coated diaphragm according to claim 1 or 2, characterized in that: The polyurethane comprises a soft segment and a hard segment; the soft segment is a polymer diol, and the hard segment is a diisocyanate; the molar ratio of the polymer diol to the diisocyanate is 1:2 to 1:2.
5.
4. The polyurethane coated diaphragm according to claim 1 or 2, characterized in that: The coating layer has a thickness of 1 to 3 μm.
5. A method for preparing a polyurethane coated diaphragm, characterized in that: The following steps are involved: (1) using a polymer diol as a soft segment raw material and a diisocyanate as a hard segment raw material, mixing the soft segment raw material and the hard segment raw material in a first solvent for polycondensation reaction to obtain an isocyanate-terminated polyurethane prepolymer; The molar ratio of the polymer diol to the diisocyanate is 1:2 to 1:2.5; (2) mixing the polyurethane prepolymer obtained in step (1) with an amino or hydroxyl terminated chain extender in a first solvent to carry out a chain extension reaction to obtain a polyurethane chain extension prepolymer; The molar ratio of the chain extender to the diisocyanate is 0.2:1 to 0.4:1; (3) mixing the polyurethane chain extension prepolymer obtained in step (2) with a crosslinking agent in a first solvent to carry out a crosslinking reaction to obtain a crosslinked polyurethane; The molar ratio of the crosslinking agent to the diisocyanate is 0.2:1 to 0.7:1; (4) dissolving the cross-linked polyurethane obtained in step (3) in a second solvent, heating at 30 to 80° C. and stirring uniformly to obtain a coating slurry; (5) coating the coating slurry obtained in step (4) on one side or both sides of the base film, and obtaining the polyurethane coated diaphragm after curing; Wherein, the base film is one of polyethylene, polypropylene, and polypropylene / polyethylene / polypropylene composite membrane.
6. The method for preparing the polyurethane coated diaphragm according to claim 5, characterized in that: The cross-linking density of the cross-linked polyurethane is 10% to 30%; preferably, the structural formula of the cross-linked polyurethane is as shown in formula (1):
7. The method for preparing a polyurethane coated diaphragm according to claim 5 or 6, characterized in that: The polymer diol is selected from one or more of polytetrahydrofuran, polycaprolactone, and polycarbonate; and / or, The diisocyanate is selected from one or more of hexamethylene diisocyanate and dicyclohexylmethane diisocyanate; and / or, The chain extender is a diamino or dihydroxy chain extender, selected from one or more of N,N'-bis(2-hydroxyethyl)oxalamide and tartaric acid; and / or, The cross-linking agent is selected from one or more of polyamine compounds and phenylboronic acid compounds.
8. The method for preparing a polyurethane coated diaphragm according to claim 5 or 6, characterized in that: The first solvent is one or more of N-methylpyrrolidone, dimethylformamide and tetrahydrofuran; and / or, The second solvent is one or more of dichloromethane, dimethylformamide and tetrahydrofuran.
9. The method for preparing a polyurethane coated diaphragm according to claim 5 or 6, characterized in that: The polycondensation reaction in step (1), the chain extension reaction in step (2) and the cross-linking reaction in step (3) are all carried out under the action of a catalyst; the catalyst is an amine, tin or bismuth catalyst; and / or, In the polycondensation reaction in step (1), the chain extension reaction in step (2) and the cross-linking reaction in step (3), the reaction temperature is 30 to 70° C. and the reaction time is 12 to 24 hours.
10. Application of a polyurethane coated separator in a secondary battery, characterized in that: The polyurethane coated diaphragm according to any one of claims 1 to 4 is used, or the polyurethane coated diaphragm is prepared by the preparation method of the polyurethane coated diaphragm according to any one of claims 5 to 9.
Citation Information
Patent Citations
Aqueous polyurethane resin dispersion for secondary battery separator, secondary battery separator, and secondary battery
CN115191060A
Polyurea and / or polyurethane-based gel electrolyte as well as preparation method and application thereof
CN116565307A
Battery diaphragm and battery
CN220106806U
Li / SOCl2 Battery Comprising Separator for Battery Coated by Polyurethane Polymer
KR1020080073969A
Cited By
Lithium battery diaphragm with self-repairing function and preparation method thereof
CN120749339A