Graphene quantum dot modified perovskite solar cell and preparation method thereof
By modifying the SnO2 electron transport layer by N-doped graphene quantum dots, the problem of low charge transfer efficiency caused by the oxygen vacancies and well state in perovskite solar cell devices is solved, and higher photoelectric conversion efficiency and charge collection effect are achieved.
Patent Information
- Application Number
- CN202411019486.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The existing perovskite solar cell devices have low charge transfer efficiency due to the oxygen vacancies and well state of the SnO2 electron transport layer, and the interface recombination effect reduces the photoelectric performance.
The SnO2 electron transport layer is modified by N-doped graphene quantum dots, and the interface structure is regulated by spin coating and heat treatment, combined with the perovskite light absorption layer and hole transport layer to prepare a graphene quantum dot-modified perovskite solar cell. .
It significantly reduces the hysteresis phenomenon of perovskite solar cell devices, improves the photoelectric conversion efficiency, improves the contact quality between the perovskite layer and the electron transport layer, and enhances the efficiency of the charge collection channel.
Smart Images

Figure CN118946175A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cell devices, and in particular to a graphene quantum dot-modified perovskite solar cell and a preparation method thereof. Background Art
[0002] In the past decade, organic-inorganic hybrid perovskite solar cells (PSCs) have developed rapidly due to the excellent optoelectronic properties of perovskite materials and devices and different preparation methods. At present, planar heterojunction PSCs have become one of the most widely concerned devices due to their simple preparation process. It usually deposits a conductive substrate, an electron transport layer (ETL), a perovskite layer, a hole transport layer (HTL), and a counter electrode from bottom to top. ETLs play the role of extracting electrons from the perovskite absorption layer and suppressing surface carrier recombination. In addition, in a typical nip structure, ETLs are also the basis of the perovskite layer, HTL, and counter electrode structure. Therefore, in addition to having excellent optoelectronic properties, ETLs usually need to have a smooth surface morphology to be in close contact with the perovskite layer, which may lead to suppressed carrier loss channels and achieve more efficient charge transfer.
[0003] SnO2, as a promising ETL material, has a low preparation temperature (180°C) and exhibits optoelectronic properties such as a wider band gap, a deeper conduction band position, and a higher electron mobility. However, a large number of oxygen vacancy wells are likely to exist on the surface of devices prepared by SnO2 processed by low-temperature solutions, resulting in energy loss between device levels. This not only results in the blocking of the excited charges in the perovskite layer, but also causes the recombination of carriers at the interface between adjacent layers, ultimately reducing the efficiency of the device. Summary of the invention
[0004] The purpose of this section is to summarize some aspects of the embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0005] Therefore, the purpose of the present invention is to provide a graphene quantum dot modified perovskite solar cell and a preparation method thereof, by regulating the SnO2 electron transport layer interface through N-doped graphene quantum dots to reduce the hysteresis of the perovskite solar cell device, thereby obtaining a higher photoelectric conversion efficiency.
[0006] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0007] A graphene quantum dot modified perovskite solar cell consists of a substrate stacked in sequence, a SnO2 electron transport layer modified with N-doped graphene quantum dots, a perovskite light absorption layer, a hole transport layer and a metal electrode.
[0008] As a preferred solution of the graphene quantum dot modified perovskite solar cell described in the present invention, the metal electrode is made of gold material.
[0009] A method for preparing a graphene quantum dot-modified perovskite solar cell, the specific steps are as follows:
[0010] S1. Etching and cleaning of substrate:
[0011] Etching and cleaning the substrate ITO;
[0012] S2. Preparation of SnO2 electron transport layer modified by N-doped graphene quantum dots:
[0013] The SnO2 hydrosol was dispersed in ultrapure water to prepare a 3.33wt% solution, which was prepared by spin coating. The SnO2 solution was spin coated on the substrate surface at a speed of 4000rpm for 30s, annealed in air at 150℃ for 30min, and cooled to room temperature. Then, the N-GQDS solution was dispersed in ultrapure water to prepare different concentration solutions of 0-4mg / mL, and rotated on the SnO2 surface at a speed of 4000rpm for 30s, and then annealed at 80℃ for 30min and cooled to room temperature.
[0014] S3. Preparation of perovskite light absorption layer:
[0015] A certain amount of PbI2 solution was spin-coated on the SnO2 electron transport layer at 1500 rpm for 30 s, followed by annealing on a 70 °C hot stage for 2 min. The FAI:MAI:MACl mixed solution was spin-coated on the PbI2 film at 2000 rpm for 30 s, and finally placed on a 140 °C hot stage, annealed for 15 min, and cooled to room temperature.
[0016] S4. Preparation of hole transport layer:
[0017] Take 40 μL Spiro-OMeTAD solution, drop it onto the perovskite light absorption layer, and spin coat at 3000 rpm for 30 seconds to obtain the hole transport layer;
[0018] S5. Preparation of metal electrodes:
[0019] Take an appropriate amount of gold wire and place it in a tungsten boat, -4 Under vacuum conditions of 1.5 pa, a 100 nm gold film was evaporated on the hole transport layer as the positive electrode, and the evaporation rate was always maintained at
[0020] As a preferred embodiment of the method for preparing a graphene quantum dot-modified perovskite solar cell described in the present invention, in the step S1, the specific steps of etching and cleaning the substrate ITO are: etching the substrate ITO with a laser etcher, ultrasonically cleaning 2cm×2cm ITO with ultrapure water, acetone, and anhydrous ethanol for 15 minutes respectively, and then drying the cleaned conductive substrate with N2, and treating it with ultraviolet ozone for 12 minutes before use to improve the wettability of the substrate surface to facilitate the subsequent spin coating of the electron transport layer solution.
[0021] As a preferred embodiment of the method for preparing a graphene quantum dot-modified perovskite solar cell described in the present invention, in step S4, the Spiro-OMeTAD solution is prepared as follows: 72.25 mg of spiro-OMeTAD powder is weighed in a glove box and dissolved in 1 mL of chlorobenzene, and then 28.75 μL of 4-tert-butylpyridine and 17.5 μL of Li-TFSI acetonitrile solution are added and mixed evenly to obtain a doped Spiro-OMeTAD solution.
[0022] As a preferred embodiment of the method for preparing a graphene quantum dot-modified perovskite solar cell described in the present invention, in step S3, the PbI2 solution is prepared as follows: 691.5 mg of PbI2 powder is weighed and dispersed in a mixed solution of 1 mL DMF:DMSO=9:1, placed on a magnetic stirring hot stage and stirred overnight at 70°C, a FAI / MAI / MACl mixed solution is prepared, FAI:MAI:MACl powder is weighed, the mass ratio is 90 mg:6.39 mg:9 mg, dispersed in 1 mL IPA solution, stirred at room temperature for 30 min, and set aside.
[0023] As a preferred embodiment of the method for preparing a graphene quantum dot-modified perovskite solar cell according to the present invention, in step S2, the preparation of N-doped graphene quantum dots is as follows:
[0024] 0.1 g of graphene oxide was dispersed in a mixed solution of 20 mL of 98% H2SO4 and 6.7 mL of 63% HNO3 and ultrasonicated for 4 h;
[0025] Then put it into a reactor lined with polytetrafluoroethylene and heat it to 200°C for 10 hours. After cooling to room temperature, add 260 mL of deionized water to the solution, and add NaCO3 to adjust the pH value of the solution to 5.
[0026] Then, 10 mL of aqueous ammonia was added to the solution and ultrasonicated for 20 min. Subsequently, the solution was transferred to a polytetrafluoroethylene-lined autoclave and heated at 200 °C for 10 h;
[0027] The solution was then heated to 100 °C to remove the ammonia, and then the solution was dialyzed in a dialysis bag for 48 hours to obtain N-doped graphene quantum dots.
[0028] As a preferred embodiment of the method for preparing a graphene quantum dot-modified perovskite solar cell according to the present invention, the steps for preparing graphene oxide are as follows:
[0029] Add 6 g of graphite powder to a mixed solution of 24 mL of H2SO4, 5 g of K2S2O8 and 5 g of P2O5, heat at 80 °C for 4.5 h, then add 1000 mL of deionized water and continue heating for 12 h;
[0030] The solution was then filtered and deionized water was used to remove the residual acid, and the product was dried in an atmospheric environment for 12 h. The product was then added to 240 mL of H2SO4, and 30 g of KMnO4 was added in a portion while stirring in an ice-water bath, keeping the solution temperature below 20 °C;
[0031] The solution was then stirred at 40°C for 30 min and at 90°C for another 90 min;
[0032] Then, 500 mL of deionized water was added for dilution, and the mixture was reacted at 105 °C for 25 min. Stirring was continued for 2 h, and 1400 mL of deionized water and 40 mL of 30% H2O2 were added to terminate the reaction. The solution was filtered and rinsed with 1:10 dilute hydrochloric acid, and then rinsed with water for several times.
[0033] Finally, the product was dialyzed and purified for one week to remove metal ions, and the obtained product was ultrasonicated for 20 minutes to finally obtain a uniform 0.01 mg / mL graphene oxide suspension, and finally the solution was dried to obtain graphene oxide solid.
[0034] Compared with the prior art, the present invention has the following beneficial effects: graphene quantum dots are a new type of graphene nanomaterial, which has good crystallinity compared with traditional graphene materials, and due to its special edge effect, it exhibits excellent photoelectron transfer, provides tunable band gap and good chemical stability. Therefore, in recent years, it has been used in perovskite solar cells to significantly improve the morphology and crystallinity of perovskite crystal films, provide effective charge collection channels, and promote the extraction of electrons from the perovskite layer to the electron transport layer. Therefore, the present invention prepares N-doped graphene quantum dots to regulate the interface of the SnO2 electron transport layer, reduce the hysteresis of the perovskite solar cell device, and thus obtain a higher photoelectric conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the present invention will be described in detail below in combination with the accompanying drawings and detailed embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0036] Figure 1 The transmission electron microscope image of the graphene quantum dots doped with N provided by the present invention;
[0037] Figure 2 A scanning electron microscope image of the SnO2 interface modified by N-doped graphene quantum dots provided by the present invention;
[0038] Figure 3 0mgmL provided by the present invention -1 Schematic diagram of the JV curve of the device during forward-reverse scanning after the SnO2 interface is modified by N-doped graphene quantum dots;
[0039] Figure 4 2mgmL provided by the present invention -1 Schematic diagram of the JV curve of the device during forward-reverse scanning after the SnO2 interface is modified by N-doped graphene quantum dots;
[0040] Figure 5 This is a flow chart for preparing the perovskite absorption layer provided by the present invention. DETAILED DESCRIPTION
[0041] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0042] Secondly, the present invention is described in detail with reference to schematic diagrams. When describing the embodiments of the present invention in detail, for the sake of convenience, the cross-sectional diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of the present invention. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.
[0043] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.
[0044] The present invention provides a graphene quantum dot modified perovskite solar cell and a preparation method thereof, wherein the hysteresis of the perovskite solar cell device is reduced by regulating the SnO2 electron transport layer interface through N-doped graphene quantum dots, thereby obtaining a higher photoelectric conversion efficiency.
[0045] The graphene quantum dot-modified perovskite solar cell consists of a substrate stacked in sequence, a SnO2 electron transport layer modified with N-doped graphene quantum dots, a perovskite light absorption layer, a hole transport layer and a metal electrode, wherein the metal electrode is made of gold material.
[0046] The present invention first prepares graphene oxide from graphite powder, then prepares N-doped graphene quantum dots from the graphene oxide as a preparatory material, and then prepares a graphene quantum dot-modified perovskite solar cell based on the preparatory material.
[0047] First, graphene oxide is prepared as follows:
[0048] Add 6 g of graphite powder to a mixed solution of 24 mL of H2SO4, 5 g of K2S2O8 and 5 g of P2O5, heat at 80 °C for 4.5 h, then add 1000 mL of deionized water and continue heating for 12 h;
[0049] The solution was then filtered and deionized water was used to remove the residual acid, and the product was dried in an atmospheric environment for 12 h. The product was then added to 240 mL of H2SO4, and 30 g of KMnO4 was added in a portion while stirring in an ice-water bath, keeping the solution temperature below 20 °C;
[0050] The solution was then stirred at 40°C for 30 min and at 90°C for another 90 min;
[0051] Then, 500 mL of deionized water was added for dilution, and the mixture was reacted at 105 °C for 25 min. Stirring was continued for 2 h, and 1400 mL of deionized water and 40 mL of 30% H2O2 were added to terminate the reaction. The solution was filtered and rinsed with 1:10 dilute hydrochloric acid, and then rinsed with water for several times.
[0052] Finally, the product was dialyzed and purified for one week to remove metal ions, and the obtained product was ultrasonicated for 20 minutes to finally obtain a uniform 0.01 mg / mL graphene oxide suspension, and finally the solution was dried to obtain graphene oxide solid.
[0053] N-doped graphene quantum dots (N-GQDS) were prepared as follows:
[0054] 0.1 g of graphene oxide was dispersed in a mixed solution of 20 mL of 98% H2SO4 and 6.7 mL of 63% HNO3 and ultrasonicated for 4 h;
[0055] Then put it into a reactor lined with polytetrafluoroethylene and heat it to 200°C for 10 hours. After cooling to room temperature, add 260 mL of deionized water to the solution, and add NaCO3 to adjust the pH value of the solution to 5.
[0056] Then, 10 mL of aqueous ammonia was added to the solution and ultrasonicated for 20 min. Subsequently, the solution was transferred to a polytetrafluoroethylene-lined autoclave and heated at 200 °C for 10 h;
[0057] The solution was then heated to 100 °C to remove the ammonia, and then the solution was dialyzed in a dialysis bag for 48 hours to obtain N-doped graphene quantum dots.
[0058] The transmission electron microscopy image of the prepared N-doped graphene quantum dots is shown in Figure 1 As shown, it can be clearly seen from the figure that the quantum dots are uniform in size and well dispersed.
[0059] The specific steps of the preparation method of graphene quantum dot modified perovskite solar cell are as follows:
[0060] S1. Etching and cleaning of substrate:
[0061] The ITO substrate was etched using a laser etcher, and 2 cm × 2 cm ITO was ultrasonically cleaned with ultrapure water, acetone, and anhydrous ethanol for 15 min each. The cleaned conductive substrate was then blown dry with N2 and treated with ultraviolet ozone for 12 min before use to improve the wettability of the substrate surface and facilitate the subsequent spin coating of the electron transport layer solution.
[0062] S2. Preparation of SnO2 electron transport layer modified by N-doped graphene quantum dots:
[0063] The SnO2 hydrosol was dispersed in ultrapure water to prepare a 3.33wt% solution, which was prepared by spin coating. The SnO2 solution was spin coated on the substrate surface at a speed of 4000rpm for 30s, annealed in air at 150℃ for 30min, and cooled to room temperature. Then, the N-GQDS solution was dispersed in ultrapure water to prepare different concentration solutions of 0-4mg / mL, and rotated on the SnO2 surface at a speed of 4000rpm for 30s, and then annealed at 80℃ for 30min and cooled to room temperature.
[0064] like Figure 2 As shown in the figure, it can be seen that the SnO2 interface introduced with N-GQDS is smooth, flat, uniform and dense. Figure 3 and Figure 4 It can be seen that the hysteresis of SnO2 after N-GQDS treatment is significantly reduced, indicating that N-GQDS modification improves the extraction and transport of carriers. In addition, the forward-reverse scanning JV curve of the device treated with N-GQDS shows that the PCE and FF are significantly improved. The FF is increased to 80.28%, and the photoelectric conversion efficiency is increased to 21.19%.
[0065] S3. Preparation of perovskite light absorption layer:
[0066] Weigh 691.5 mg of PbI2 powder, disperse it in 1 mL of DMF:DMSO = 9:1 mixed solution, place it on a magnetic stirring hot plate and stir it overnight at 70 ° C. Prepare FAI / MAI / MACl mixed solution, weigh FAI:MAI:MACl powder, the mass ratio is 90 mg:6.39 mg:9 mg, disperse it in 1 mL of IPA solution, stir it at room temperature for 30 min, and obtain PbI2 solution, such as Figure 5 As shown, a certain amount of PbI2 solution was spin-coated on the SnO2 electron transport layer at 1500 rpm for 30 s, followed by annealing on a 70 °C hot stage for 2 min, and the FAI:MAI:MACl mixed solution was spin-coated on the PbI2 film at 2000 rpm for 30 s, and finally placed on a 140 °C hot stage, annealed for 15 min, and cooled to room temperature;
[0067] S4. Preparation of hole transport layer:
[0068] In a glove box, weigh 72.25 mg of spiro-OMeTAD powder and dissolve it in 1 mL of chlorobenzene. Then add 28.75 μL of 4-tert-butylpyridine and 17.5 μL of Li-TFSI acetonitrile solution and mix well to obtain a doped Spiro-OMeTAD solution. Take 40 μL of Spiro-OMeTAD solution and drop it onto the perovskite light absorption layer. Spin-coat at 3000 rpm for 30 seconds to obtain a hole transport layer.
[0069] S5. Preparation of metal electrodes:
[0070] Take an appropriate amount of gold wire and place it in a tungsten boat, -4 Under vacuum conditions of 1.5 pa, a 100 nm gold film was evaporated on the hole transport layer as the positive electrode, and the evaporation rate was always maintained at
[0071] Although the present invention has been described above with reference to the embodiments, various modifications may be made thereto and parts thereof may be replaced by equivalents without departing from the scope of the present invention. In particular, as long as there is no structural conflict, the various features in the embodiments disclosed in the present invention may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A graphene quantum dot modified perovskite solar cell, It is characterized in that The SnO substrate is stacked sequentially and modified with N-doped graphene quantum dots. 2 It consists of an electron transport layer, a perovskite light absorption layer, a hole transport layer and a metal electrode.
2. A graphene quantum dot modified perovskite solar cell according to claim 1, It is characterized in that The metal electrode is made of gold.
3. A method for preparing a graphene quantum dot modified perovskite solar cell as claimed in claim 1 or 2, It is characterized in that The specific steps are as follows: S1. Etching and cleaning of substrate: Etching and cleaning the substrate ITO; S2, SnO modified by N-doped graphene quantum dots 2 Preparation of electron transport layer: SnO 2 The hydrosol was dispersed in ultrapure water to prepare a 3.33 wt% solution, which was prepared by spin coating at a speed of 4000 rpm for 30 s. 2 The solution was spin-coated on the substrate surface, annealed in air at 150 °C for 30 min, cooled to room temperature, and then the N-GQDS solution was dispersed in ultrapure water to prepare different concentrations of 0-4 mg / mL. The solution was rotated at 4000 rpm for 30 s on the SnO 2 The surface was then annealed at 80 °C for 30 min and cooled to room temperature; S3. Preparation of perovskite light absorption layer: Take a certain amount of PbI 2 The solution was spin-coated on SnO at 1500 rpm for 30 s. 2 The electron transport layer was then annealed on a 70 °C hot plate for 2 min, and the FAI:MAI:MACl mixed solution was heated at 2000 rpm on the PbI 2 The film was spin-coated for 30 s and finally placed on a 140 °C hot stage for annealing for 15 min and cooled to room temperature; S4. Preparation of hole transport layer: Take 40 μL Spiro-OMeTAD solution, drop it onto the perovskite light absorption layer, and spin coat at 3000 rpm for 30 seconds to obtain the hole transport layer; S5. Preparation of metal electrodes: Take an appropriate amount of gold wire and place it in a tungsten boat, -4 Under vacuum conditions of 1.5 pa, a 100 nm gold film was evaporated on the hole transport layer as the positive electrode, and the evaporation rate was always maintained at 4. A method for preparing a graphene quantum dot-modified perovskite solar cell according to claim 3, It is characterized in that In step S1, the specific steps of etching and cleaning the substrate ITO are as follows: using a laser etcher to etch the substrate ITO, ultrasonically cleaning the 2 cm×2 cm ITO with ultrapure water, acetone, and anhydrous ethanol for 15 min each, and then cleaning the cleaned conductive substrate with N 2 Blow dry and treat with UV ozone for 12 minutes before use to improve the wettability of the substrate surface and facilitate the subsequent spin coating of the electron transport layer solution.
5. A method for preparing a graphene quantum dot modified perovskite solar cell according to claim 3, It is characterized in that In step S4, the preparation of the Spiro-OMeTAD solution is as follows: 72.25 mg of spiro-OMeTAD powder is weighed and dissolved in 1 mL of chlorobenzene in a glove box, and then 28.75 μL of 4-tert-butylpyridine and 17.5 μL of Li-TFSI acetonitrile solution are added and mixed evenly to obtain a doped Spiro-OMeTAD solution.
6. A method for preparing a graphene quantum dot modified perovskite solar cell according to claim 3, It is characterized in that In step S3, PbI 2 The solution was prepared as follows: 691.5 mg of PbI 2 The powder was dispersed in a mixed solution of 1 mL DMF:DMSO = 9:1, placed on a magnetic stirring hot stage and stirred overnight at 70°C to prepare a FAI / MAI / MACl mixed solution. The FAI:MAI:MACl powders were weighed at a mass ratio of 90 mg:6.39 mg:9 mg and dispersed in 1 mL IPA solution. The mixture was stirred at room temperature for 30 min and set aside.
7. A method for preparing a graphene quantum dot modified perovskite solar cell according to claim 3, It is characterized in that In step S2, the preparation of N-doped graphene quantum dots is as follows: Disperse 0.1 g of graphene oxide in 20 mL of 98% H 2 SO 4 and 6.7 mL of 63% HNO 3 The mixed solution was ultrasonicated for 4 h; Then, the mixture was placed in a polytetrafluoroethylene-lined reactor and heated to 200 °C for 10 h. After cooling to room temperature, 260 mL of deionized water was added to the solution, and NaCO 3 Adjust the pH value of the solution to 5; Then, 10 mL of aqueous ammonia was added to the solution and ultrasonicated for 20 min. Subsequently, the solution was transferred to a polytetrafluoroethylene-lined autoclave and heated at 200 °C for 10 h; The solution was then heated to 100 °C to remove the ammonia, and then the solution was dialyzed in a dialysis bag for 48 hours to obtain N-doped graphene quantum dots.
8. A method for preparing a graphene quantum dot modified perovskite solar cell according to claim 7, It is characterized in that The preparation steps of graphene oxide are as follows: Add 6 g of graphite powder into 24 mL of H 2 SO 4 , 5g K 2 S 2 O 8 and 5g P 2 O 5 The mixed solution was heated at 80 °C for 4.5 h, then 1000 mL of deionized water was added and the heating was continued for 12 h; The solution was then filtered and deionized water was used to remove the residual acid, and the product was dried under atmospheric conditions for 12 h, then added to 240 mL of H 2 SO 4 In an ice water bath, 30 g of KMnO was added gradually while stirring. 4 , keep the solution temperature below 20°C; The solution was then stirred at 40°C for 30 min and at 90°C for another 90 min; Then, 500 mL of deionized water was added for dilution, and the mixture was reacted at 105 °C for 25 min. Stirring was continued for 2 h, and 1400 mL of deionized water and 40 mL of 30% H 2 O 2 The reaction was terminated, the solution was filtered and washed with 1:10 dilute hydrochloric acid, and then washed with water several times; Finally, the product was dialyzed and purified for one week to remove metal ions, and the obtained product was ultrasonicated for 20 minutes to finally obtain a uniform 0.01 mg / mL graphene oxide suspension, and finally the solution was dried to obtain graphene oxide solid.