Manufacturing method of OLED RGB sub-pixel
Through photolithography, etching, evaporation and ion implantation technologies, OLED RGB subpixels are accurately prepared on silicon wafer substrates, and OLED luminescent materials of different colors are directly evaporated, solving the problems caused by FMM size limitations and color filters, realizing the High-precision color display and brightness improvement have been enhanced, enhancing the competitiveness of high-end display devices.
Patent Information
- Application Number
- CN202411019346.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The existing OLED RGB subpixel production technology is difficult to achieve ultra-fine pixels due to the size limitation of Fine Metal Mask (FMM), and the use of color filters leads to increased costs, decreased brightness and reduced color saturation, which limits the high-end application field of OLED display technology. competitiveness.
The anode and cathode layers are accurately prepared on the silicon wafer substrate by photolithography, etching, evaporation and ion implantation technology, and the OLED luminescent materials of different colors are directly evaporated to different regions through the deposition and local damage technology of multi-layer organic luminescent materials. , combine atomic layer deposition technology to form a sealing layer, avoiding the use of color filters.
It realizes the precise production of ultra-fine pixels, improves display brightness and color saturation, reduces production costs and pollution in the manufacturing process, simplifies production processes, and enhances the competitiveness of high-end display equipment.
Smart Images

Figure CN118946224A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor silicon-based OLED display, and in particular to a method for manufacturing an OLED RGB sub-pixel. Background Art
[0002] There are several significant problems and challenges in the current OLED RGB sub-pixel manufacturing technology. First, when using Fine Metal Mask (FMM) evaporation technology to make OLED RGB pixels, it is difficult to achieve smaller OLED RGB pixels due to the physical size limitation of FMM. This size limitation hinders the development of ultra-fine display technology, especially in applications that require high resolution and compact pixel layout.
[0003] In addition, in order to bypass the limitations of FMM technology, the industry generally adopts the method of combining white light OLED screens with color filters (CF) to manufacture small-sized OLED RGB pixels. However, although this method can achieve a smaller pixel size, it brings problems such as increased cost, decreased brightness, and reduced color saturation. The use of color filters not only increases manufacturing costs, but also reduces display brightness due to the loss of light energy during the filtering process, affecting the display effect of the final product.
[0004] The above problems limit the competitiveness of OLED display technology in certain high-end application fields, such as smart phones, high-definition TVs and professional display devices, which have extremely high requirements on pixel size, display brightness and color performance; therefore, there is an urgent need to develop new technical methods to overcome the limitations of existing manufacturing technology and improve the manufacturing efficiency and display performance of OLED RGB sub-pixels. Summary of the invention
[0005] The purpose of the present invention is to solve the above problems in the prior art and to propose a method for manufacturing OLED RGB sub-pixels.
[0006] The object of the present invention can be achieved by the following technical solution: a method for manufacturing an OLED RGB sub-pixel, the method for manufacturing an OLED RGB sub-pixel comprising the following steps:
[0007] S1 uses a photolithography device to perform photolithography on a silicon wafer substrate to prepare an anode pixel structure, and uses an etching device to remove unnecessary parts to form an anode pixel layer on the silicon wafer substrate;
[0008] S2 applies a layer of hole transport material on the anode pixel layer by evaporation or spin coating to form a hole layer to ensure a good interface between the layers; then uses OLED evaporation equipment to evenly evaporate R color luminescent material on the hole layer to cover the entire silicon wafer substrate to form an R color luminescent layer;
[0009] S3 uses ion implantation equipment to implant BF3 or PH3 at the GB position, and by implanting B+ or P- ions, destroys the R color luminous area at the GB position;
[0010] S4 uses OLED evaporation equipment to evaporate the G color luminescent material on the damaged R color luminescent layer, covering the entire substrate to form a G color luminescent layer;
[0011] S5 uses ion implantation equipment to implant BF2 or PH3 at the RB position, and destroys the G color luminescent area at the RB position by implanting B+ or P- ions;
[0012] S6 uses OLED evaporation equipment to evaporate B color luminescent material on the damaged G color luminescent layer, covering the entire substrate to form a B color luminescent layer;
[0013] S7 uses ion implantation equipment to implant BF2 or PH3 at the RG position, and by implanting B+ or P- ions, destroys the B color luminescent area at the RG position;
[0014] S8 uses OLED coating equipment to evenly coat the cathode material on the damaged B-color light-emitting layer to form a cathode layer; then uses ALD sealing equipment to coat a sealing layer on the cathode layer using atomic layer deposition technology.
[0015] In the above method, by combining the deposition of multiple layers of organic light-emitting materials with local destruction technology, the color output of a single pixel can be accurately controlled, thereby achieving high-precision color display. In this process, ion implantation technology is used to accurately adjust the light-emitting characteristics of each pixel on the silicon wafer to ensure that each sub-pixel only displays the predetermined red, green or blue light.
[0016] Preferably, in steps S3, S5 and S7, the specific process of using ion implantation equipment to implant BF3 or PH2 is as follows:
[0017] Preparation phase: Clean and inspect the ion implantation equipment to ensure it is dust-free and operating properly to prevent any potential contamination or mechanical failure;
[0018] Setting parameters: Setting the parameters of the ion implantation equipment according to the production requirements, including the implantation voltage and beam current, to ensure that the implantation depth and dose meet the requirements, thereby achieving precise modification of the predetermined area;
[0019] Directional injection: Directly implant the ion beam into the predetermined area through the opening to achieve ultra-fine pixel manufacturing without FMM preparation; the opening width is 3-5um;
[0020] Perform implantation: activate the ion source, start implanting BF2 or PH2, and control the implantation time to meet the required ion dose and depth; during the implantation process, monitor the implantation depth and distribution in real time, and make adjustments when necessary to ensure overall uniformity and consistency.
[0021] Reasons for setting the openings: Directional injection: The setting of the openings allows the ion beam to be precisely directed to a predetermined area. This directional capability is achieved by physically limiting the propagation area of the ion beam, ensuring that only the predetermined sub-pixel area is modified by ions, thereby controlling the color transition of the light-emitting area;
[0022] Reduced crosstalk: In OLED display technology, precise control of the size and position of the light-emitting area is critical, especially when achieving high-resolution displays. The openings can limit the range of ion implantation and prevent interference between adjacent pixels, thereby improving image clarity and color accuracy.
[0023] Reasons for the opening width of 3-5um: Resolution and fineness: The opening width determines the minimum area that the injected ions can reach, which is directly related to the pixel size of the display. The width of 3-5um allows the manufacture of small pixels, which is suitable for the needs of high-resolution displays without sacrificing display quality.
[0024] Technical limitations and optimization: This width range provides a balance that ensures implant accuracy while taking into account the technical limitations of the manufacturing process (such as equipment accuracy, ion beam diffusion, etc.). Too narrow an opening may lead to technical challenges and increased costs, while too wide an opening may affect implant accuracy and pixel definition.
[0025] Reduce crosstalk and improve color purity: In OLED display technology, crosstalk refers to the unwanted interaction between adjacent pixels, which may cause color mixing or light leakage; using an opening width of 3-5um helps to limit the area of action of the ion beam, thereby reducing crosstalk between adjacent pixels and improving the color purity and quality of the display.
[0026] Preferably, the ion implantation equipment is directly connected to the OLED evaporation equipment to form a completely closed processing environment, thereby reducing the potential damage of pollutants introduced during the manufacturing process and ensuring that the life of the OLED is not affected.
[0027] Preferably, the specific steps of evaporation using OLED evaporation equipment are as follows:
[0028] Preparation and preheating: Before the evaporation begins, the OLED evaporation equipment is preheated to reach the required working temperature to ensure the evaporation rate and stability of the material during the evaporation process;
[0029] Loading materials: Loading materials into the evaporation source of the evaporation equipment;
[0030] Vacuum extraction: Start the vacuum pump in the OLED evaporation equipment to pump the air in the evaporation chamber to a preset pressure to reduce the collision between gas molecules and evaporated material molecules, ensuring that the material can migrate from the source to the substrate without hindrance;
[0031] Evaporation: heating the evaporation source to convert the material directly from solid to gas, controlling the heating temperature and time to adjust the evaporation rate to ensure that the evaporated material can be deposited evenly;
[0032] Thickness and uniformity control: Use a crystal thickness monitor to monitor the thickness and uniformity of the deposited layer in real time;
[0033] End of evaporation: Once the target thickness is reached and material deposition is complete, turn off the heating source and allow the OLED evaporation equipment to cool naturally; then slowly return to normal pressure.
[0034] Compared with the prior art, the method for manufacturing OLED RGB sub-pixels has the following beneficial effects:
[0035] 1. Realize precise production of ultra-fine pixels: Traditional Fine Metal Mask (FMM) evaporation technology is difficult to achieve smaller OLED RGB pixels due to physical size limitations. The present invention adopts ion implantation technology, which allows precise production of ultra-fine pixels by precisely controlling the position, depth and dose of ion implantation without using FMM. This is particularly important for display devices with high resolution and compact pixel layout.
[0036] 2. Improve display brightness and color saturation: In traditional methods, the use of color filters (CF) will lead to light energy loss, increased costs and reduced display effects. In the method of the present invention, different colors of OLED light-emitting materials are directly evaporated in different areas, and ion implantation technology is used to selectively destroy areas that do not need to emit light, thereby eliminating the need for additional CF layers, which not only reduces production costs, but also significantly improves the brightness and color saturation of the product.
[0037] 3. Reduce pollution during the manufacturing process: The direct connection between the injection equipment and the OLED evaporation equipment forms a completely closed processing environment, which greatly reduces the introduction of potential pollutants during the manufacturing process and helps to improve the stability of OLED and extend its service life.
[0038] 4. Improve production efficiency and reduce costs: By eliminating the traditional CF process, the production process is simplified and the material and operating costs are reduced. In addition, the application of injection technology reduces the complex steps in production and improves the overall production efficiency.
[0039] 5. Enhance product competitiveness: By providing a display effect with higher brightness and better color saturation while reducing costs and improving production efficiency, the OLED RGB sub-pixel manufacturing method of the present invention can provide a more competitive display solution for high-end display devices such as smart phones, high-definition TVs and professional display devices.
[0040] In summary, the present invention not only optimizes the manufacturing process of OLED, but also significantly improves the performance and market competitiveness of the final product, bringing important technological innovation to the development of modern display technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 FIG. 4 is a flow chart of manufacturing OLED RGB sub-pixels in a specific embodiment of the present invention.
[0042] Figure 1 In the figure, Wafer is a silicon wafer substrate;
[0043] Figure 2 It is a schematic diagram of the operation of an ion implantation device used in a specific implementation of the present invention.
[0044] Figure 2 In the invention, Wafer refers to the silicon wafer substrate. DETAILED DESCRIPTION
[0045] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0046] like Figure 1 As shown, the manufacturing method of the OLED RGB sub-pixel comprises the following steps:
[0047] S1 uses a photolithography device to perform photolithography on a silicon wafer substrate to prepare an anode pixel structure, and uses an etching device to remove unnecessary parts to form an anode pixel layer on the silicon wafer substrate;
[0048] S2 applies a layer of hole transport material on the anode pixel layer by evaporation or spin coating to form a hole layer to ensure a good interface between the layers; then uses OLED evaporation equipment to evenly evaporate R color luminescent material on the hole layer to cover the entire silicon wafer substrate to form an R color luminescent layer;
[0049] like Figure 2As shown, S3 uses ion implantation equipment to implant BF2 or PH2 at the GB position, and by implanting B+ or P- ions, the R color luminous area at the GB position is destroyed;
[0050] S4 uses OLED evaporation equipment to evaporate the G color luminescent material on the damaged R color luminescent layer, covering the entire substrate to form a G color luminescent layer;
[0051] like Figure 2 As shown, S5 uses ion implantation equipment to implant BF3 or PH3 at the RB position, and by implanting B+ or P- ions, the G color light emitting area at the RB position is destroyed;
[0052] S6 uses OLED evaporation equipment to evaporate B color luminescent material on the damaged G color luminescent layer, covering the entire substrate to form a B color luminescent layer;
[0053] like Figure 2 As shown, S7 uses ion implantation equipment to implant BF3 or PH3 at the RG position, and by implanting B+ or P- ions, the B color light emitting area at the RG position is destroyed;
[0054] S8 uses OLED coating equipment to evenly coat the cathode material on the damaged B-color light-emitting layer to form a cathode layer; then uses ALD sealing equipment to coat a sealing layer on the cathode layer using atomic layer deposition technology.
[0055] In the above method, by combining the deposition of multiple layers of organic light-emitting materials with local destruction technology, the color output of a single pixel can be accurately controlled, thereby achieving high-precision color display. In this process, ion implantation technology is used to accurately adjust the light-emitting characteristics of each pixel on the silicon wafer to ensure that each sub-pixel only displays the predetermined red, green or blue light.
[0056] Preferably, in steps S3, S5 and S7, the specific process of using ion implantation equipment to implant BF3 or PH3 is as follows:
[0057] Preparation phase: Clean and inspect the ion implantation equipment to ensure it is dust-free and operating properly to prevent any potential contamination or mechanical failure;
[0058] Setting parameters: Setting the parameters of the ion implantation equipment according to the production requirements, including the implantation voltage and beam current, to ensure that the implantation depth and dose meet the requirements, thereby achieving precise modification of the predetermined area;
[0059] Directional injection: Directly implant the ion beam into the predetermined area through the opening to achieve ultra-fine pixel manufacturing without FMM preparation; the opening width is 3-5um;
[0060] Perform implantation: activate the ion source, start implanting BF3 or PH3, and control the implantation time to meet the required ion dose and depth; during the implantation process, monitor the implantation depth and distribution in real time, and make adjustments when necessary to ensure overall uniformity and consistency.
[0061] Reasons for setting the openings: Directional injection: The setting of the openings allows the ion beam to be precisely directed to a predetermined area. This directional capability is achieved by physically limiting the propagation area of the ion beam, ensuring that only the predetermined sub-pixel area is modified by ions, thereby controlling the color transition of the light-emitting area;
[0062] Reduced crosstalk: In OLED display technology, precise control of the size and position of the light-emitting area is critical, especially when achieving high-resolution displays. The openings can limit the range of ion implantation and prevent interference between adjacent pixels, thereby improving image clarity and color accuracy.
[0063] Reasons for the opening width of 3-5um: Resolution and fineness: The opening width determines the minimum area that the injected ions can reach, which is directly related to the pixel size of the display. The width of 3-5um allows the manufacture of small pixels, which is suitable for the needs of high-resolution displays without sacrificing display quality.
[0064] Technical limitations and optimization: This width range provides a balance that ensures implant accuracy while taking into account the technical limitations of the manufacturing process (such as equipment accuracy, ion beam diffusion, etc.). Too narrow an opening may lead to technical challenges and increased costs, while too wide an opening may affect implant accuracy and pixel definition.
[0065] Reduce crosstalk and improve color purity: In OLED display technology, crosstalk refers to the unwanted interaction between adjacent pixels, which may cause color mixing or light leakage; using an opening width of 3-5um helps to limit the area of action of the ion beam, thereby reducing crosstalk between adjacent pixels and improving the color purity and quality of the display.
[0066] Preferably, the ion implantation equipment is directly connected to the OLED evaporation equipment to form a completely closed processing environment, thereby reducing the potential damage of pollutants introduced during the manufacturing process and ensuring that the life of the OLED is not affected.
[0067] Preferably, the specific steps of evaporation using OLED evaporation equipment are as follows:
[0068] Preparation and preheating: Before the evaporation begins, the OLED evaporation equipment is preheated to reach the required working temperature to ensure the evaporation rate and stability of the material during the evaporation process;
[0069] Loading materials: Loading materials into the evaporation source of the evaporation equipment;
[0070] Vacuum extraction: Start the vacuum pump in the OLED evaporation equipment to pump the air in the evaporation chamber to a preset pressure to reduce the collision between gas molecules and evaporated material molecules, ensuring that the material can migrate from the source to the substrate without hindrance;
[0071] Evaporation: heating the evaporation source to convert the material directly from solid to gas, controlling the heating temperature and time to adjust the evaporation rate to ensure that the evaporated material can be deposited evenly;
[0072] Thickness and uniformity control: Use a crystal thickness monitor to monitor the thickness and uniformity of the deposited layer in real time;
[0073] End of evaporation: Once the target thickness is reached and material deposition is complete, turn off the heating source and allow the OLED evaporation equipment to cool naturally; then slowly return to normal pressure.
[0074] The specific embodiments described herein are merely examples of the spirit of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but will not deviate from the spirit of the present invention or exceed the defined scope. Although the present invention is described and described in detail in the drawings and the foregoing description, such descriptions and descriptions are considered to be illustrative or exemplary rather than restrictive. It should be understood that within the scope of the following claims, changes and modifications may be made by a person of ordinary skill. Specifically, the present invention encompasses additional embodiments having any combination of features from the above-mentioned different embodiments. With respect to the use of the expression "generally" or "substantially", this patent application should be understood to disclose that these features and values are also fully satisfied, i.e., there is no aforementioned characterization as "generally" or "substantially".
[0075] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
Claims
1. A method for manufacturing an OLED RGB sub-pixel, characterized in that: The method for manufacturing the OLED RGB sub-pixel comprises the following steps: S1 uses a photolithography device to perform photolithography on a silicon wafer substrate to prepare an anode pixel structure, and uses an etching device to remove unnecessary parts to form an anode pixel layer on the silicon wafer substrate; S2 applies a layer of hole transport material on the anode pixel layer by evaporation or spin coating to form a hole layer to ensure a good interface between the layers; then uses OLED evaporation equipment to evenly evaporate R color luminescent material on the hole layer to cover the entire silicon wafer substrate to form an R color luminescent layer; S3 uses ion implantation equipment to implant BF3 or PH2 at the GB position, and by implanting B+ or P- ions, destroys the R color luminous area at the GB position; S4 uses OLED evaporation equipment to evaporate the G color luminescent material on the damaged R color luminescent layer, covering the entire substrate to form a G color luminescent layer; S5 uses ion implantation equipment to implant BF3 or PH3 at the RB position, and destroys the G color luminescent area at the RB position by implanting B+ or P- ions; S6 uses OLED evaporation equipment to evaporate B color luminescent material on the damaged G color luminescent layer, covering the entire substrate to form a B color luminescent layer; S7 uses ion implantation equipment to implant BF3 or PH3 at the RG position, and by implanting B+ or P- ions, destroys the B color luminescent area at the RG position; S8 uses OLED coating equipment to evenly coat the cathode material on the damaged B-color light-emitting layer to form a cathode layer; then uses ALD sealing equipment to coat a sealing layer on the cathode layer using atomic layer deposition technology.
2. The method for manufacturing an OLED RGB sub-pixel as claimed in claim 1, characterized in that: In steps S3, S5 and S7, the specific process of using ion implantation equipment to implant BF3 or PH3 is as follows: Preparation phase: Clean and inspect the ion implantation equipment to ensure it is dust-free and operating properly to prevent any potential contamination or mechanical failure; Setting parameters: Setting the parameters of the ion implantation equipment according to the production requirements, including the implantation voltage and beam current, to ensure that the implantation depth and dose meet the requirements, thereby achieving precise modification of the predetermined area; Directional implantation: Directed implantation of ion beams into a predetermined area through an opening to achieve ultra-fine pixel fabrication without FMM preparation; The opening width is 3-5um; Perform implantation: activate the ion source, start implanting BF3 or PH3, and control the implantation time to meet the required ion dose and depth; during the implantation process, monitor the implantation depth and distribution in real time, and make adjustments when necessary to ensure overall uniformity and consistency.
3. The method for manufacturing an OLED RGB sub-pixel as claimed in claim 1, characterized in that: The ion implantation equipment is directly connected to the OLED evaporation equipment to form a completely closed processing environment, reducing the potential damage of pollutants introduced during the manufacturing process and ensuring that the life of the OLED is not affected.
4. The method for manufacturing an OLED RGB sub-pixel as claimed in claim 1, characterized in that: Using OLED evaporation equipment, the specific steps for evaporation are as follows: Preparation and preheating: Before the evaporation begins, the OLED evaporation equipment is preheated to reach the required working temperature to ensure the evaporation rate and stability of the material during the evaporation process; Loading materials: Loading materials into the evaporation source of the evaporation equipment; Vacuum extraction: Start the vacuum pump in the OLED evaporation equipment to pump the air in the evaporation chamber to a preset pressure to reduce the collision between gas molecules and evaporated material molecules, ensuring that the material can migrate from the source to the substrate without hindrance; Evaporation: heating the evaporation source to convert the material directly from solid to gas, controlling the heating temperature and time to adjust the evaporation rate to ensure that the evaporated material can be deposited evenly; Thickness and uniformity control: Use a crystal thickness monitor to monitor the thickness and uniformity of the deposited layer in real time; End of evaporation: Once the target thickness is reached and the material deposition is complete, turn off the heating source and let the OLED evaporation equipment cool naturally; Then slowly return to normal pressure.