Hollow fiber membrane, hollow fiber membrane laminate, and filtration module
By using hollow fiber membranes with optimized characteristics, the problem of hollow fiber membrane collapse under high inter-membrane pressure difference is solved, and the combination of high filtration performance and mechanical strength is achieved, which is suitable for filtration operations.
Patent Information
- Application Number
- CN202380029957.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-05
- Filing Date
- 2023-01-17
- Publication Date
- 2024-11-12
AI Technical Summary
During the filtration operation, the high inter-membrane pressure difference of the hollow fiber membrane leads to collapse, reducing the filtration performance.
The hollow fiber membrane with an average outer diameter of 2.10 mm or less and an average thickness of 0.60 mm or modified polytetrafluoroethylene as the main component was used. The orientation degree along the length direction measured by wide-angle X-ray scattering method is The heat of fusion of 72% or more and 85% or less and having an endothermic peak around 328°C is 10.0 J/g or more and 13.4 J/g or less, thereby improving chemical resistance and mechanical strength, and suppressing collapse.
It effectively suppresses collapse under the condition of high pressure difference between membranes during filtration operation, maintains high filtration performance and improves the radial strength and crystallinity of the hollow fiber membrane.
Smart Images

Figure CN118946399A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a hollow fiber membrane, a hollow fiber membrane stack, and a filtration module. This application claims priority to Japanese patent application No. 2022-063137 filed on April 5, 2022. All the contents described in the Japanese patent application are incorporated into this specification by reference. Background Art
[0002] Conventionally, as a solid-liquid separation treatment device in sewage treatment, pharmaceutical manufacturing processes, etc., a filtration device having a filtration module having multiple layers of hollow fiber membranes aligned in the vertical direction is used. Such a filtration device prevents impurities contained in the treated water from penetrating through the surface of the hollow fiber membrane, and allows substances other than the impurities to penetrate into the interior of the hollow fiber membrane, thereby performing filtration treatment.
[0003] As such a filtration module, a filtration module has been proposed that can ensure high particle capture performance and increase the amount of water treated by using a hollow fiber membrane formed of, for example, polytetrafluoroethylene (PTFE) and optimizing the IPA (isopropyl alcohol) bubble point, porosity, etc. of the hollow fiber membrane (see Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2010-42329. Summary of the invention
[0007] The hollow fiber membrane of one embodiment of the present invention contains polytetrafluoroethylene or modified polytetrafluoroethylene as a main component, the average outer diameter of the hollow fiber membrane is less than 2.10 mm, the average thickness is less than 0.60 mm, the isopropanol bubble point is greater than 90 kPa, the orientation degree of the hollow fiber membrane along the length direction measured by wide-angle X-ray scattering method is greater than 72% and less than 85%, and the heat of fusion of the endothermic peak near 328°C is greater than 10.0 J / g and less than 13.4 J / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 This is a schematic cross-sectional view of a hollow fiber membrane according to one embodiment of the present invention.
[0009] Figure 2 This is a schematic cross-sectional view showing a hollow fiber membrane stack according to one embodiment of the present invention.
[0010] Figure 3 It is a schematic cross-sectional view showing a filter module according to one embodiment of the present invention. DETAILED DESCRIPTION
[0011] [Problems to be Solved by the Invention]
[0012] In recent years, in order to improve the filtering performance, the pressure difference between the membranes of the hollow fiber membranes used as filters in the filtering module has been increased during the filtering operation. However, when the pressure difference between the membranes of the hollow fiber membranes during the filtering operation is high, the hollow fiber membranes are prone to collapse, which may reduce the filtering performance.
[0013] The present invention has been made based on the above circumstances, and an object of the present invention is to provide a hollow fiber membrane capable of suppressing collapse when the transmembrane pressure difference is high during filtration operation.
[0014] [Effects of the invention]
[0015] The hollow fiber membrane according to one embodiment of the present invention can suppress collapse when the transmembrane pressure difference is high during filtration operation.
[0016] [Description of Embodiments of the Invention]
[0017] First, embodiments of the present invention are listed and described.
[0018] The hollow fiber membrane of one embodiment of the present invention contains polytetrafluoroethylene or modified polytetrafluoroethylene as a main component, the average outer diameter of the hollow fiber membrane is less than 2.10 mm, the average thickness is less than 0.60 mm, the isopropanol bubble point of the hollow fiber membrane is greater than 90 kPa, the orientation degree of the hollow fiber membrane along the length direction measured by wide-angle X-ray scattering method is greater than 72% and less than 85%, and the heat of fusion of the endothermic peak of the hollow fiber membrane near 328°C is greater than 10.0 J / g and less than 13.4 J / g.
[0019] The hollow fiber membrane can improve chemical resistance and mechanical strength by using polytetrafluoroethylene or modified polytetrafluoroethylene as the main component. The average outer diameter of the hollow fiber membrane is less than 2.10 mm, the average thickness is less than 0.60 mm, and the isopropanol bubble point is more than 90 kPa, so that the filtration performance can be well maintained and miniaturization can be achieved. In addition, the orientation degree along the length direction of the hollow fiber membrane measured by the wide-angle X-ray scattering method is more than 72% and less than 85%, which can well maintain the strength of the length direction of the hollow fiber membrane and improve the radial strength of the hollow fiber membrane. Furthermore, the melting heat of the endothermic peak near 328°C of the hollow fiber membrane is more than 10.0 J / g and less than 13.4 J / g, which can improve the crystallinity of the hollow fiber membrane. Therefore, the filtration performance of the hollow fiber membrane is high and the collapse suppression effect is good when the pressure difference between the membranes is high during the filtration operation. Here, the term "main component" refers to a component having the largest content ratio in terms of mass, and refers to a component having a content ratio of, for example, 50 mass % or more, preferably 70 mass % or more, and more preferably 95 mass % or more.
[0020] The "average thickness" of the hollow fiber membrane can be obtained by dividing (average outer diameter - average inner diameter) by 2. The above-mentioned "average outer diameter" refers to the average value of the outer diameters of any two points when the cross section of the hollow fiber membrane is a circle. When the cross section of the hollow fiber membrane is an ellipse, the short diameter and the long diameter are measured at two locations, and the average value is taken as the average outer diameter. In addition, when the cross section of the hollow fiber membrane is an irregular cross section other than a general circle or ellipse, the edge information of the outer diameter of the cross section is extracted to approximate the circle, and the value obtained by dividing the obtained inner circumference by the pi is taken as the average outer diameter. The above-mentioned "average inner diameter" refers to the average value of the inner diameters of any two points. Specifically, the above-mentioned average outer diameter can be measured according to the following steps. First, the hollow fiber membrane is cut into discs on a surface perpendicular to the length direction, and observed with an electron microscope in a manner that the entire cross section enters the field of view. Then, the outer diameters of two locations are measured at approximately diagonal positions of the above-mentioned cross section (positions where the phase shift is approximately 90 degrees), and the average value is taken as the average outer diameter. The above-mentioned "average inner diameter" refers to the average value of the inner diameters of any two points. Specifically, the above-mentioned average outer diameter can be measured according to the following steps. First, the hollow fiber membrane is cut into discs on a surface perpendicular to the length direction, and observed with an electron microscope in a manner that the entire cross section enters the field of view. Then, the outer diameters of two locations are measured at approximately diagonal positions of the above-mentioned cross section (positions where the phase shift is approximately 90 degrees), and the average value is taken as the average outer diameter. The above-mentioned "average inner diameter" refers to the average value of the inner diameters of any two points. The above average inner diameter can be measured according to the following steps. First, the hollow fiber membrane is cut into discs on a surface perpendicular to the length direction, and the whole cross section is observed with an electron microscope in a manner that the cross section is in the field of view. The inner diameter is measured at two locations at approximately diagonal positions of the above cross section (positions where the phase shift is approximately 90 degrees), and the average value is taken as the average inner diameter. "Isopropanol bubble point" refers to the value measured using isopropanol in accordance with JIS-K3832 (1990), which indicates the minimum pressure required to squeeze the liquid out of the hole, and is an indicator corresponding to the average value of the pore size.
[0021] The above-mentioned "degree of orientation" is measured by wide-angle X-ray scattering in the length direction of the hollow fiber membrane. The measurement using the wide-angle X-ray scattering method is performed, for example, as follows. X-rays can use BL16 present in the synchrotron radiation device SAGA-LS. The wavelength can be, for example, 0.056nm (spectrometer: Si 111 twin crystal). First, the hollow fiber membrane is irradiated through an incident slit with a beam diameter of 0.3mm (horizontal) × 0.3mm (vertical). The X-rays scattered by the hollow fiber membrane are detected by a detector (PILATUS100K manufactured by Decotes). The distance from the sample to the detector is 119.65mm. The degree of orientation [%] in the length direction of the hollow fiber membrane is calculated by the Debye-Scherrer method of 100 diffraction lines (plane spacing 0.4902nm) obtained by measurement using the wide-angle X-ray scattering method. The orientation in the length direction is detected as the intensity in the direction offset by 90° in the coordinate with the length direction set to 0°. Therefore, the half-value width x[°] (the width of the peak at half the height of the peak after removing the background) of the peak intensity obtained from the intensity distribution at azimuth angles of 0° to 180° is calculated using the following formula.
[0022] Orientation degree [%] (180X80}×
[0023] The heat of fusion of the endothermic peak near 328°C of the hollow fiber membrane was measured using a differential scanning calorimeter, and is the endothermic value near 328°C measured using a differential scanning calorimeter. "Near 328°C" means between 323°C and 333°C. Specifically, the heat of fusion of the hollow fiber membrane is the heat of fusion when heated from 50°C to 400°C at a rate of 10°C / min. The sample amount in the above measurement is 8 mg to 12 mg, and the sampling time is 1 second / time.
[0024] The hollow fiber membrane stack of another embodiment of the present invention comprises the hollow fiber membrane and one or more layers of porous membranes, wherein the one or more layers of porous membranes are mainly composed of polytetrafluoroethylene or modified polytetrafluoroethylene and are stacked on the outer peripheral surface of the hollow fiber membrane. The hollow fiber membrane stack comprises the hollow fiber membrane and one or more layers of the porous membranes stacked on the outer peripheral surface of the hollow fiber membrane, so that the hollow fiber membrane functions as a protective material of the porous membrane, and therefore, the hollow fiber membrane stack can maintain good filtering performance and can improve the mechanical strength and life of the hollow fiber membrane stack.
[0025] A filtration module according to another aspect of the present invention comprises a plurality of the hollow fiber membrane stacks. The filtration module can maintain good filtration performance and increase life by comprising a plurality of the hollow fiber membrane stacks.
[0026] [Details of the embodiments of the present invention]
[0027] Hereinafter, a hollow fiber membrane, a hollow fiber membrane stack, and a filtration module according to each embodiment of the present invention will be described in detail with reference to the drawings.
[0028] <Hollow fiber membrane>
[0029] Figure 1 The hollow fiber membrane 1 is mainly composed of polytetrafluoroethylene or modified polytetrafluoroethylene. Polytetrafluoroethylene and modified polytetrafluoroethylene are fluororesins with excellent chemical resistance and solvent resistance, so the selectivity of the types of liquid and gas supplied to the filter module is improved. In addition, polytetrafluoroethylene and modified polytetrafluoroethylene are fluororesins with high hydrophobicity, so they can suppress the leakage of liquid from the hollow fiber membrane 1 and improve the permeability of gas.
[0030] Modified polytetrafluoroethylene refers to polytetrafluoroethylene obtained by copolymerizing hexafluoropropylene (HFP), alkyl vinyl ether (AVE), chlorotrifluoroethylene (CTFE) or the like in a small amount, preferably in a range of 1 / 50 (molar ratio) or less relative to tetrafluoroethylene.
[0031] The lower limit of the average outer diameter of the hollow fiber membrane 1 is not particularly limited, but is preferably 1.8 mm, more preferably 1.9 mm. On the other hand, the upper limit of the average outer diameter of the hollow fiber membrane 1 is 2.1 mm, more preferably 1.95 mm. When the above-mentioned average outer diameter does not meet the above-mentioned lower limit, it is possible to cause an increase in pressure loss. On the other hand, when the above-mentioned average outer diameter is greater than the above-mentioned upper limit, it is possible that the membrane area contained in the shell becomes smaller or the distance between the membranes becomes closer, thereby causing the permeability of each membrane to decrease.
[0032] The lower limit of the average inner diameter of the hollow fiber membrane 1 is not particularly limited, but is preferably 0.9 mm, more preferably 0.95 mm. On the other hand, the upper limit of the average inner diameter of the hollow fiber membrane is preferably 1.15 mm, more preferably 1.10 mm. When the average inner diameter does not meet the lower limit, it is possible to increase the pressure loss. On the other hand, when the average inner diameter is greater than the upper limit, it is possible to reduce the compressive strength, resulting in rupture caused by internal pressure and buckling caused by external pressure.
[0033] The lower limit of the average thickness of the hollow fiber membrane 1 is preferably 0.38 mm, and more preferably 0.4 mm. On the other hand, the upper limit of the average thickness of the hollow fiber membrane 1 is 0.60 mm, and preferably 0.45 mm. When the above average thickness does not meet the above lower limit, it is possible to cause the compressive strength to decrease, resulting in rupture caused by internal pressure and buckling caused by external pressure. On the other hand, when the above average thickness is greater than the above upper limit, it is possible to cause the filtering performance to become insufficient.
[0034] The lower limit of the isopropanol bubble point of the hollow fiber membrane 1 is 90 kPa, preferably 95 kPa. On the other hand, the upper limit of the isopropanol bubble point of the hollow fiber membrane 1 is preferably 125 kPa, more preferably 120 kPa. In the case where the isopropanol bubble point of the hollow fiber membrane 1 does not meet the above lower limit, it is possible that impurities cannot be fully separated. In the case where the isopropanol bubble point of the hollow fiber membrane 1 is greater than the above upper limit, it is possible that the water permeability of the hollow fiber membrane 1 becomes insufficient, and the filtration efficiency of the hollow fiber membrane 1 is reduced.
[0035] The lower limit of the orientation degree along the length direction of the hollow fiber membrane 1 measured by the wide-angle X-ray scattering method is 72%, preferably 73%. On the other hand, the upper limit of the orientation degree along the length direction of the hollow fiber membrane 1 is 85%, preferably 75%. When the orientation degree along the length direction is less than 72%, the strength of the hollow fiber membrane 1 in the length direction may be reduced, and sufficient tensile strength cannot be obtained. On the other hand, when the average thickness is greater than the upper limit, sufficient radial strength may not be obtained, and collapse under high pressure difference between membranes during filtration operation cannot be suppressed. When the orientation degree along the length direction of the hollow fiber membrane 1 measured by the wide-angle X-ray scattering method is within the above range, the strength of the hollow fiber membrane 1 in the length direction can be well maintained and the radial strength of the hollow fiber membrane can be improved.
[0036] The upper limit of the heat of fusion of the endothermic peak near 328°C of the hollow fiber membrane 1 is 13.4 J / g, and more preferably 13.3 J / g. The lower limit of the heat of fusion of the endothermic peak near 328°C of the hollow fiber membrane 1 is 10.0 J / g, and more preferably 11.0 J / g. When the heat of fusion of the hollow fiber membrane 1 is greater than the upper limit, the pore size may become larger. On the other hand, when the heat of fusion of the hollow fiber membrane 1 does not meet the lower limit, the porosity may decrease. By setting the heat of fusion of the hollow fiber membrane 1 to the above range, a hollow fiber membrane 1 having a high degree of crystallinity and a pore size in a better range can be obtained. Therefore, even if the average outer diameter of the hollow fiber membrane 1 is within the range of 2.0 mm or less and the average thickness is within the range of 0.45 mm or less, the collapse suppression effect of the hollow fiber membrane 1 when the pressure difference between the membranes is high during the filtration operation is good.
[0037] The hollow fiber membrane 1 may contain other fluororesins and additives in addition to polytetrafluoroethylene and modified polytetrafluoroethylene within the range that does not impair the desired effect of the present invention. Examples of the additives include inorganic fillers for improving wear resistance and facilitating pore formation, metal powders, metal oxide powders, metal sulfide powders, etc.
[0038] [Method for producing hollow fiber membrane]
[0039] Next, an example of a method for manufacturing the hollow fiber membrane is described. The method for manufacturing the hollow fiber membrane includes: a step of molding particles of polytetrafluoroethylene or modified polytetrafluoroethylene into a cylindrical primary molded body (primary molded body molding step), a step of extruding the primary molded body into a cylindrical body (extrusion molding step), a step of stretching the cylindrical body in a longitudinal direction while heating the cylindrical body (stretching step), and heat-treating the stretched cylindrical body to a temperature above the melting point of PTFE (heat treatment step).
[0040] (Primary molded body forming process)
[0041] In the primary molded body molding process, a raw material prepared by mixing a liquid lubricant with a powder of polytetrafluoroethylene or modified polytetrafluoroethylene is compression molded. The powder of polytetrafluoroethylene or modified polytetrafluoroethylene as a raw material is composed of, for example, fine particles of polytetrafluoroethylene or modified polytetrafluoroethylene. Specifically, fine powder of polytetrafluoroethylene or modified polytetrafluoroethylene produced by emulsion polymerization and molding powder of polytetrafluoroethylene or modified polytetrafluoroethylene produced by suspension polymerization can be cited.
[0042] As the liquid lubricant to be mixed with the powder (raw material powder) of polytetrafluoroethylene or modified polytetrafluoroethylene, various lubricants used in the paste extrusion method in the past can be used. For example, petroleum solvents such as naphtha and white oil, hydrocarbon oils such as undecane, aromatic hydrocarbons such as toluene and xylene, alcohols, ketones, esters, silicone oils, chlorofluorocarbon oils, solutions of polymers such as polyisobutylene and polyisoprene dissolved in these solvents, mixtures of two or more of these, aqueous solutions containing surfactants, etc. As the liquid lubricant, it is preferable to use a single-component liquid lubricant because it is easy to mix evenly.
[0043] As the lower limit of the amount of the liquid lubricant, it is preferably 20 parts by mass relative to 100 parts by mass of the raw material powder, and more preferably 22 parts by mass relative to 100 parts by mass of the raw material powder. On the other hand, as the upper limit of the amount of the liquid lubricant, it is preferably 28 parts by mass relative to 100 parts by mass of the raw material powder, and more preferably 25 parts by mass relative to 100 parts by mass of the raw material powder. When the amount of the liquid lubricant does not meet the above lower limit, it is possible to cause insufficient lubricity and extrusion molding in the subsequent cylindrical body molding process becomes difficult. On the contrary, when the amount of the liquid lubricant is greater than the above upper limit, it is possible to cause the cylindrical body to break easily in the subsequent stretching process.
[0044] The length of the primary molded body to be formed in the longitudinal direction can be selected within the range of the stroke of the cylinder of the extrusion molding machine used in the subsequent cylindrical body molding step.
[0045] (Extrusion molding process)
[0046] In the extrusion molding process, the primary molded body is molded into a tube shape by an extrusion molding machine equipped with a die head having a circular opening and a center pin arranged at the center of the opening of the die head. The extrusion molding is performed at a temperature lower than the melting point of polytetrafluoroethylene or modified polytetrafluoroethylene, generally at room temperature.
[0047] Furthermore, in the extrusion molding step, it is preferred that the cylindrical body extruded from the die head is heated to volatilize the liquid lubricant. By removing the liquid lubricant in this way, the cylindrical body can be stably stretched in the subsequent stretching step.
[0048] In the extrusion molding step, the cylindrical body extruded from the die may be wound at a speed faster than the extrusion speed from the die to perform primary stretching on the cylindrical body. The stretching ratio of the primary stretching may be, for example, 150% to 170%.
[0049] In this extrusion molding, the larger the reduction rate (the ratio of the cross-sectional area of the primary molded body to the area of the gap between the die head and the center pin), the more the molecular chains of polytetrafluoroethylene or modified polytetrafluoroethylene are oriented along the length direction of the cylinder, the greater the strength of the cylinder in the length direction, and on the other hand, the radial strength decreases.
[0050] The lower limit of the reduction ratio in the extrusion molding process is preferably 800, and more preferably 850. On the other hand, the upper limit of the reduction ratio in the extrusion molding is preferably 1200, and more preferably 1150. When the reduction ratio in the extrusion molding does not meet the above lower limit, it is possible that the formation efficiency of the cylinder becomes insufficient, and it is possible that the strength of the cylinder in the longitudinal direction becomes insufficient, and the cylinder becomes easy to break in the subsequent stretching process. On the contrary, when the reduction ratio in the extrusion molding is greater than the above upper limit, it is possible that the radial strength of the cylinder is reduced, and the strength of the obtained hollow fiber membrane becomes insufficient.
[0051] (Stretching process)
[0052] In the stretching process, the cylinder is stretched in the longitudinal direction while being heated, so as to be stretched in a manner of reducing the diameter to a desired diameter. Therefore, the stretching ratio in the stretching process is set in a manner such that the total stretching ratio including the primary stretching in the extrusion molding process is an appropriate value. In the stretching process, the molecular chains of polytetrafluoroethylene or modified polytetrafluoroethylene are also further oriented in the longitudinal direction of the cylinder.
[0053] The lower limit of the heating temperature during stretching is preferably 200°C, more preferably 220°C. On the other hand, the upper limit of the heating temperature during stretching is preferably 300°C, more preferably 280°C. When the heating temperature during stretching does not meet the above lower limit, it is possible that the stretching speed of the cylinder cannot be sufficiently increased. On the contrary, when the heating temperature during stretching is greater than the above upper limit, it is possible that the melting point of polytetrafluoroethylene or modified polytetrafluoroethylene is exceeded due to uneven temperature, thereby causing the cylinder to break.
[0054] (Heat treatment process)
[0055] In the heat treatment process, the stretched cylinder is heat treated to a temperature above the melting point of polytetrafluoroethylene or modified polytetrafluoroethylene. As a result, the orientation degree of the hollow fiber membrane along the length direction can be relaxed and adjusted to a good range. Specifically, through the heat treatment process, the orientation degree of the hollow fiber membrane along the length direction is adjusted to 72% or more and 85% or less. As the heating temperature of the heat treatment process, it is preferably 330°C or more and 370°C or less, and as the heating time, it is preferably 15 minutes or more and 60 minutes or less.
[0056] According to this hollow fiber membrane, collapse can be suppressed when the transmembrane pressure difference is high during filtration operation.
[0057] <Hollow fiber membrane stack>
[0058] The hollow fiber membrane stack comprises the hollow fiber membrane and one or more porous membranes mainly composed of polytetrafluoroethylene or modified polytetrafluoroethylene and stacked on the outer peripheral surface of the hollow fiber membrane. The porous membrane can improve heat resistance, chemical stability, etc. by mainly composed of polytetrafluoroethylene or modified polytetrafluoroethylene.
[0059] Figure 2 This is a schematic cross-sectional view showing a hollow fiber membrane stack according to one embodiment of the present invention. Figure 2 The hollow fiber membrane stack 40 shown has the hollow fiber membrane 1 and one or more layers of porous membrane 2 stacked on the outer peripheral surface of the hollow fiber membrane 1. In the hollow fiber membrane stack 40, the hollow fiber membrane 1 functions as a supporting membrane, and the porous membrane 2 functions as a filtration layer. The hollow fiber membrane stack 40 has the hollow fiber membrane 1 and one or more layers of the porous membrane 2 stacked on the outer peripheral surface of the hollow fiber membrane 1, so that the hollow fiber membrane 1 functions as a protective material for the porous membrane 2. Therefore, the hollow fiber membrane stack 40 can maintain good filtering performance and can improve the mechanical strength and life of the hollow fiber membrane stack 40.
[0060] The upper limit of the average thickness of one layer of the porous membrane 2 is preferably 20 μm, and more preferably 18 μm. On the other hand, the lower limit of the above average thickness of the porous membrane 2 is preferably 8 μm, and more preferably 10 μm. In the case where the above average thickness of the porous membrane 2 is greater than the above upper limit, the pressure loss of the hollow fiber membrane stack 40 may increase. On the other hand, in the case where the average thickness of the porous membrane 2 is less than the above lower limit, the strength of the hollow fiber membrane stack 40 may become insufficient.
[0061] The hollow fiber membrane stack may have a three-layer structure, for example, two layers of porous membranes may be stacked on the hollow fiber membrane as the supporting membrane disposed in the innermost layer. Alternatively, the hollow fiber membrane stack may have a structure of four or more layers.
[0062] [Method for producing hollow fiber membrane stack]
[0063] An embodiment of a method for manufacturing a hollow fiber membrane stack is described in which the hollow fiber membrane stack has a porous membrane and the hollow fiber membrane as a supporting membrane. The method for manufacturing the hollow fiber membrane stack includes: a step of spirally winding a porous strip-shaped body around the outer peripheral surface of the hollow fiber membrane in a manner that its two edge portions overlap (winding step), and a step of bonding the hollow fiber membrane to the strip-shaped body by heating (bonding step).
[0064] (Winding process)
[0065] The porous membranes are laminated by spirally winding a porous belt-shaped body containing PTFE as a main component around the outer peripheral surface of the hollow fiber membrane.
[0066] As the belt-shaped body wound around the hollow fiber membrane, it is preferable to use a belt-shaped body made porous by forming slits by stretching a PTFE sheet.
[0067] The lower limit of the average width of the strip-shaped body wound around the hollow fiber membrane is 6.0 mm, preferably 6.5 mm. On the other hand, the upper limit of the average width of the strip-shaped body wound around the hollow fiber membrane is 12.0 mm, preferably 11.5 mm. In the case where the average width of the strip-shaped body wound around the hollow fiber membrane does not meet the above lower limit, the area of the region where the strips overlap becomes larger, and therefore, the filtration performance of the obtained hollow fiber membrane laminate may be unnecessarily reduced. On the contrary, in the case where the average width of the strip-shaped body wound around the hollow fiber membrane is greater than the above upper limit, the angle of the strip-shaped body wound radially relative to the hollow fiber membrane becomes larger, and therefore, it may be difficult to wind the strip-shaped body.
[0068] (Gluing process)
[0069] In the bonding process, the material formed by winding the strip-shaped body to form the porous membrane on the outer peripheral surface of the hollow fiber membrane is heated to a temperature above the melting point of PTFE. Thus, the overlapping side edges of the strip-shaped body are bonded to each other to form a continuous porous membrane, and the porous membrane is integrated with the hollow fiber membrane.
[0070] The heating temperature in the bonding step can be, for example, 350° C. or higher and 400° C. or lower, and the heating time can be, for example, 1 minute or longer and 10 minutes or shorter.
[0071] According to the hollow fiber membrane stack, the hollow fiber membrane functions as a protective material of the porous membrane, so the hollow fiber membrane stack can maintain good filtering performance and can improve the mechanical strength and life of the hollow fiber membrane stack. Therefore, the hollow fiber membrane stack has excellent filtering performance and mechanical strength and is suitable as a filter.
[0072] <Filter module>
[0073] The filtration module has a plurality of hollow fiber membrane stacks. The filtration module is used in a membrane separation device for removing impurities from raw water and discharging filtered water. The filtration module is used, for example, in a precision filtration device, an ultrafiltration device, a reverse osmosis device, and the like.
[0074] Figure 3 A filter module 50 according to an embodiment of the present invention is shown. The filter module 50 is an external pressure filter module, and includes a membrane member 20 and a cylindrical housing 30, wherein the membrane member 20 includes a plurality of hollow fiber membrane stacks 40 aligned in one direction, and the cylindrical housing 30 accommodates the membrane member 20. In addition, the filter module 50 includes a first holding member 4, a second holding member 5, and a support member 6, wherein the first holding member 4 fixes one end of the plurality of hollow fiber membrane stacks 40 in the housing 30, the second holding member 5 fixes the other end of the plurality of hollow fiber membrane stacks 40 in the housing 30, and the support member 6 maintains the interval between the first holding member 4 and the second holding member 5. The support member 6 is composed of, for example, a metal support pipe that is spanned between the first holding member 4 and the second holding member 5.
[0075] The plurality of hollow fiber membrane stacks 40, the first holding member 4, and the second holding member 5 are configured as a cartridge that can be loaded and unloaded relative to the housing 30. That is, the first holding member 4 and the second holding member 5 are not bonded to the inner peripheral surface of the housing 30. Even in the case where the plurality of hollow fiber membrane stacks 40, the first holding member 4, and the second holding member 5 are configured as a cartridge, the filtration module 50 can appropriately suppress entanglement of the hollow fiber membrane stacks 40, because the interval between the first holding member 4 and the second holding member 5 is maintained by the support member 6.
[0076] As the shell 30, a shell of existing specifications can be used. The shell 30 has a main body 11 whose inner diameter is approximately uniform in the entire axial direction, a cover 13 connected to one end side of the main body 11, and a bottom 15 connected to the other end side of the main body 11. The main body 11 is, for example, cylindrical. In the present embodiment, the central axis of the main body 11 is arranged in the up-down direction. A first retaining member 4 is detachably connected to the inner peripheral surface of the main body 11. In other words, the first retaining member 4 is detachably connected to the smooth surface of the shell 30. The main body 11 has a sewage discharge port 10 at the upper part of the peripheral wall. The cover 13 is detachably connected to the main body 11. The cover 13 has a filtered water discharge port 8 that can discharge the filtered water B that has passed through the plurality of hollow fiber membrane stacks 40. The bottom 15 is funnel-shaped with a diameter that decreases downward, and has a raw water inlet 7 at the top end that can introduce raw water A into the shell 30. A sewage discharge port 10 that can discharge sewage C is provided on the side of the shell 30. It should be noted that the arrangement positions and orientations of the raw water inlet 7, the filtered water outlet 8, and the sewage outlet 10 are not particularly limited, and can be configured according to the state in which the filter module 50 is installed. In addition, "the inner diameter is substantially uniform" means that, for example, the ratio of the maximum value to the minimum value of the inner diameter in the entire axial direction is greater than 1.00 and less than 1.10, preferably greater than 1.00 and less than 1.05.
[0077] The filtration module 50 introduces raw water A from the raw water inlet 7 into the housing 30, suppresses the penetration of impurities on the outer peripheral surface of the plurality of hollow fiber membrane stacks 40, and discharges the filtered water B that has passed through the plurality of hollow fiber membrane stacks 40 from the filtered water outlet 8, thereby performing a filtration process. In addition, the filtration module 50 is configured so that the sewage C containing impurities that have not penetrated the plurality of hollow fiber membrane stacks 40 is discharged from the sewage outlet 10.
[0078] According to this filtration module, by including a plurality of the hollow fiber membrane stacks, it is possible to maintain good filtration performance and to extend the life.
[0079] [Other embodiments]
[0080] The embodiments disclosed herein are illustrative in all aspects and should not be construed as restrictive. The scope of the present invention is not limited to the configuration of the above-described embodiments but is indicated by the scope of the claims, and is intended to include all modifications within the meaning and scope equivalent to the scope of the claims.
[0081] Example
[0082] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.
[0083] <Hollow fiber membrane: Test No. 1 to No. 6>
[0084] PTFE fine powder ("F104" manufactured by Daikin Co., Ltd.) as raw material powder was used as raw material. 25 parts by mass of liquid lubricant ("FP-25" manufactured by Idemitsu Co., Ltd.) was mixed with the raw material powder relative to 100 parts by mass of the raw material powder, and pressed into a cylindrical shape using a preforming machine. Then, an extruder was used to form a cylindrical body. The barrel and die head temperature were set to 50°C.
[0085] Next, the cylindrical body was stretched at 200° C. The average outer diameter and average thickness of the stretched cylindrical body are shown in Table 1. The average outer diameter and average thickness were obtained by averaging the values at arbitrary points.
[0086] Next, the stretched cylindrical bodies of Test Nos. 2 to 6 were subjected to heat treatment under the heating conditions described in Table 1. The stretched cylindrical body of Test No. 1 was not subjected to the heat treatment step.
[0087] [Determination of physical property values]
[0088] (Determination of heat of fusion)
[0089] About 10 mg of each hollow fiber membrane sample was measured for the heat of fusion [J / g] of the endothermic peak near 328° C. under the following conditions using a heat flux differential scanning calorimeter (“DSC60-A” manufactured by Shimadzu Corporation).
[0090] (Orientation Degree)
[0091] For the hollow fiber membranes of Test Nos. 1 to 6, the degree of orientation [%] in the longitudinal direction was measured by the above-mentioned measuring method.
[0092] (Isopropyl alcohol (IPA) bubble point)
[0093] The IPA bubble point [kPa] was measured using isopropyl alcohol as a test liquid in accordance with JIS-K3832 (1990).
[0094] (Isopropyl alcohol (IPA) flow rate)
[0095] Regarding the IPA flow rate [mL / min], the pressure difference was set to 0.1 MPa and the membrane length was set to 10 cm, and the flow rate of isopropyl alcohol permeating the hollow fiber membrane was measured.
[0096] [Evaluation of hollow fiber membranes]
[0097] (External pressure strength)
[0098] With respect to the hollow fiber membranes of Test Nos. 1 to 6, water pressure was applied from the outside of the hollow fiber membrane, and the pressure [kPa] at the time when the membrane collapsed was visually measured.
[0099] (Tensile Strength)
[0100] The hollow fiber membranes of Test Nos. 1 to 6 were measured for tensile strength (maximum tensile stress) [MPa] at a line spacing of 100 mm and a test speed of 100 mm / min in accordance with JIS-K7161 (2014).
[0101] Table 1 shows the measurement results of the orientation degree, isopropyl alcohol flow rate, isopropyl alcohol bubble point, heat of fusion, external pressure strength, and tensile strength of the hollow fiber membranes of Test No. 1 to No. 6.
[0102] [Table 1]
[0103]
[0104] As shown in Table 1, the hollow fiber membranes of Test No. 2 to Test No. 5, which have an average outer diameter of less than 2.10 mm, an average thickness of less than 0.60 mm, an isopropanol bubble point of more than 90 kPa, an orientation degree in the length direction of more than 72% and less than 85%, and a heat of fusion of the endothermic peak near 328°C of more than 10.0 J / g and less than 13.4 J / g, have high external pressure strength and tensile strength. It can be seen from this that the strength in the length direction and the radial strength of the hollow fiber membranes of No. 2 to No. 5 are both good. On the other hand, it can be considered that the hollow fiber membrane of Test No. 1, which has an orientation degree in the length direction of more than 85%, has poor external pressure strength and poor collapse suppression effect when the pressure difference between membranes during filtration operation is high. The hollow fiber membrane of Test No. 6, which has an orientation degree in the length direction of less than 72% and a heat of fusion of the endothermic peak near 328°C of more than 13.4 J / g, broke in the external pressure strength test and the tensile strength test.
[0105] As described above, the hollow fiber membrane has an excellent collapse suppression effect when the transmembrane pressure difference during filtration operation is high. Therefore, the hollow fiber membrane is suitable for use in filtration devices such as wastewater treatment.
[0106] Description of Reference Numerals
[0107] 1 hollow fiber membrane, 2 porous membrane, 4 first retaining member, 5 second retaining member, 6 supporting member, 7 raw water inlet, 8 filtered water outlet, 10 sewage outlet, 11 main body, 13 cover, 15 bottom, 20 membrane member, 30 shell, 40 hollow fiber membrane stack, 50 filtration module, A raw water, B filtered water, C sewage.
Claims
1. A hollow fiber membrane, which is mainly composed of polytetrafluoroethylene or modified polytetrafluoroethylene, The hollow fiber membrane has an average outer diameter of 2.10 mm or less, an average thickness of 0.60 mm or less, and an isopropanol bubble point of 90 kPa or more. The hollow fiber membrane has an orientation degree in the longitudinal direction of 72% to 85% as measured by wide-angle X-ray scattering, and a heat of fusion at an endothermic peak near 328° C. of 10.0 J / g to 13.4 J / g.
2. A hollow fiber membrane stack comprising the hollow fiber membrane according to claim 1 and one or more layers of porous membranes, The one or more porous membranes contain polytetrafluoroethylene or modified polytetrafluoroethylene as a main component and are laminated on the outer peripheral surface of the hollow fiber membrane. 3 . A filtration module comprising a plurality of the hollow fiber membrane stacks according to claim 2 .