Coating stripping method and coating stripping device
By using a small amount of water-soluble peeling of the water-soluble resin layer on the single side of the substrate film, combined with appropriate tension and angle control, the film peeling efficiency and environmental problems in the prior art are solved, and efficient and environmentally friendly regenerated film production is achieved.
Patent Information
- Application Number
- CN202380029239.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-10
- Filing Date
- 2023-04-05
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the peeling method of the water-soluble resin layer has problems such as the initial peeling capacity and large environmental load, and the use of organic solvents is too large, resulting in high cleaning costs and serious environmental pollution.
A small amount of water is used as the cleaning liquid to peel off the water-soluble resin layer from the single side of the substrate film. By controlling the amount and tension of the cleaning liquid, combined with appropriate angles and contact lengths, efficient film peeling is achieved.
It effectively reduces the use of cleaning liquid, reduces the environmental load, improves the peeling efficiency and stability of the film, and ensures high purity and low-cost production of the regenerated film.
Smart Images

Figure CN118946445A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a peeling method and a peeling device capable of efficiently removing a coating film on the surface of a thermoplastic resin film. Background Art
[0002] Plastics are used in a variety of fields. On the other hand, they are considered to be the cause of marine pollution such as microplastics. Reducing the environmental impact caused by plastics has become a top priority.
[0003] In addition, in recent years, due to the evolution of the Internet of Things (IoT), the number of electronic devices such as the central processing unit (CPU) mounted on computers or smartphones has increased, and the number of stacked ceramic capacitors (multi-layer ceramic capacitors (MLCC)) required to drive electronic devices has also increased dramatically. The general manufacturing method of the MLCC includes the following steps: using a release film having a release layer formed on a plastic substrate film as a carrier, forming a ceramic sheet layer on the release film, and peeling off the ceramic green sheet layer to make a ceramic green sheet. In the process, the release film after the ceramic green sheet is peeled off is discarded as a useless object.
[0004] That is, the increase in the amount of release film waste accompanying the rapid increase in the number of MLCCs in recent years has become an environmental problem, and measures for the recycling of plastic base films have become increasingly active. From the perspective of mold release properties, the components of the release layer contained in the release film are generally different from the components constituting the base film. Therefore, when the release film with the release layer is directly remelted to produce a recycled film, the components of the release layer exist as foreign matter, so stable film production cannot be performed.
[0005] Patent Document 1 discloses a method for removing a release component from a release film. The release film is prepared by immersing the release film in a warm water bath for more than 2 seconds and then brushing the surface of the release film with a brush roller to peel off the release layer.
[0006] In Patent Document 2, as a method for removing a coated film from a base film having a coating formed by coating, the following device is disclosed: it includes a dissolution tank storing an organic solvent, a scraper capable of contacting the surface of the coating is provided at the bottom of the dissolution tank, and the coating is dissolved and removed from the base film having a coating being transported.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2004-363140
[0010] Patent document 2: Japanese Patent Publication No. 2021-146682 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, the film stripping method disclosed in Patent Document 1 has the following problems: since the water-soluble resin layer is eluted into the warm water tank, the resin concentration in the warm water increases with the treatment time, and the initial stripping ability cannot be continued. Even in the case of increasing the water supply amount to suppress the increase in resin concentration, the amount of waste water also increases with the water supply amount, so there is a problem that not only the cleaning cost is greatly increased, but also the environmental load increases.
[0013] In addition, in the film stripping method disclosed in Patent Document 2, an organic solvent is used to dissolve and remove the film. As in Patent Document 1, a large amount of organic solvent is required to continue to show the initial stripping ability, so there is a problem of significantly increasing the environmental load. In addition, the scraper provided at the bottom of the dissolving tank is a device structure that directly contacts the film surface of the substrate film with the film to be transported to scrape the film, but since the substrate film is transported in the liquid, when the film is scraped by the scraper, it is easy to have an organic solvent between the film surface and the scraper, and sometimes it is impossible to obtain sufficient scraping ability. In order to improve the scraping ability, it is conceivable to set the angle between the upstream side and the downstream side of the film surface in the transport direction of the substrate film separated by the scraper to an acute angle, but since it is necessary to deepen the dissolving tank, the volume of the dissolving tank is increased, and the amount of organic solvent used is further increased, which further deteriorates the environmental load.
[0014] Therefore, in order to obtain a base film that can stably produce a regenerated film even if the base film with a coating is remelted after use, the present invention provides a coating stripping method and a coating stripping device that can dissolve a water-soluble resin from the surface of a base film having a coating containing a water-soluble resin on one side of the base film using a small amount of cleaning liquid, thereby efficiently and reliably stripping the coating.
[0015] Technical means of solving problems
[0016] [1] The film peeling method of the present invention for solving the above-mentioned problems is a method for peeling off the film from a substrate film having a film containing a water-soluble resin on at least one side, wherein the film is peeled off at least one side of the substrate film, wherein the film is peeled off at least one side of the substrate film. 2A cleaning liquid containing water as a main component is applied to the film in an amount ranging from 3 ml to 650 ml in terms of surface area, a stripping member is brought into contact with the surface of the film applied with the cleaning liquid, an angle formed by the substrate film across the stripping member is set in a range of 20° to 150°, a tension is applied in a range of 10 N / m to 1000 N / m in at least one direction along the length direction of the substrate film, and the substrate film is relatively moved relative to the stripping member in the length direction of the substrate film, thereby stripping the film from the substrate film.
[0017] [2] The film stripping method of [1] is preferably as follows: within the range where the stripping member contacts the surface of the film, the length of the substrate film in the longitudinal direction is set as a contact length L [m], a plane passing through the center position of the contact length and perpendicular to the surface of the stripping member is set as a vertical plane, a side of the substrate film relatively close to the stripping member is set as an upstream side, and a side of the substrate film relatively far from the stripping member is set as a downstream side, and the contact length L is 1×10 -5 m~1×10 -3 m, so that the angle (acute angle) θ1[°] formed by the vertical plane and the substrate film located upstream of the vertical plane, the angle (acute angle) θ2[°] formed by the vertical plane and the substrate film located downstream of the vertical plane, the tension T1[N / m] applied to the substrate film located upstream of the vertical plane, and the tension T2[N / m] applied to the substrate film located downstream of the vertical plane satisfy the following formula (1).
[0018] Formula (1): 1.0×10 6 ≦{T1×cos(θ1)+T2×cos(θ2)} / L≦2.4×10 8
[0019] [3] The film stripping method of [1] or [2] is preferably: among the two surfaces constituting the stripping member and sandwiching the ridge line at which the stripping member starts to contact the surface of the film, the angle formed by the surface facing the base film before contacting the ridge line and the base film before contacting the ridge line is set to be greater than 5°.
[0020] [4] The film peeling method according to any one of [1] to [3] is preferably characterized in that the film comprises a curable silicone resin.
[0021] [5] The film stripping device of the present invention for solving the above-mentioned problem is a device for stripping the film from a base film having a film containing a water-soluble resin on at least one side thereof, comprising: a cleaning liquid applying mechanism for applying a cleaning liquid to the film; a stripping member for stripping the film to which the cleaning liquid has been applied from the base film; a driving device for causing the base film to move relative to the stripping member in the longitudinal direction of the base film; and a tension applying mechanism for applying tension in at least one direction in the longitudinal direction of the base film, the cleaning liquid applying mechanism being adjusted to apply a tension of 100% to the base film per 1 m 2 The cleaning liquid is applied in an amount ranging from 3 ml to 650 ml per surface area, the stripping member is configured to contact the surface of the film applied with the cleaning liquid, and the angle between the substrate films separated by the stripping member is in the range of 20° to 150°, and the tension applying mechanism is adjusted to apply a tension in the range of 10 N / m to 1000 N / m.
[0022] [6] The film peeling device of [5] is preferably such that the length L of the range of the peeling member in contact with the surface of the film in the longitudinal direction of the base film is 1×10 -5 m~1×10 -3 The range of m.
[0023] [7] The film peeling device of [5] or [6] preferably includes: a roll-out device for unwinding the base film having the film that is rolled into a roll; and a winding device for winding the base film after the film is peeled off.
[0024] In addition, the substrate film before the stripping member contacts is referred to as the "substrate film having a coating", and the substrate film after the stripping member contacts is referred to as the "substrate film after the coating is stripped off". In the coating stripping methods [1] to [4] and the coating stripping devices [5] to [7], there is no particular distinction and they are all referred to as the "substrate film".
[0025] Effects of the Invention
[0026] According to the film peeling method and film peeling apparatus of the present invention, a film can be peeled off efficiently and reliably from a base film having a film containing a water-soluble resin on one surface of the base film using a small amount of cleaning liquid. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] [ Figure 1 ] is a schematic diagram of a stripping device according to one embodiment of the present invention.
[0028] [ Figure 2 ] is a schematic diagram of a peeling member of the first embodiment of the peeling device of the present invention.
[0029] [ Figure 3 ] is a schematic diagram of a peeling member of a second embodiment of the peeling device of the present invention.
[0030] [ Figure 4 ] is a schematic diagram of a peeling member of a third embodiment of the peeling device of the present invention.
[0031] [ Figure 5 ] is a graph showing the results of film peeling under the conditions of Example 1.
[0032] [ Figure 6 ] is a graph showing the results of film peeling under the conditions of Example 2.
[0033] [ Figure 7 ] is a graph showing the results of film peeling under the conditions of Example 3. DETAILED DESCRIPTION
[0034] The present inventors have conducted extensive research into a method for efficiently and reliably stripping a coated film from the surface of a film having a coating containing a water-soluble resin on one side of a substrate film using a very small amount of cleaning liquid, and have discovered the following coating stripping method and coating stripping device.
[0035] [Substrate film having a coating film to be targeted]
[0036] The method for peeling a film from a substrate film having a film of the present invention is as follows: a substrate film having a film containing a water-soluble resin on at least one side of the substrate film is used as an object, the film is washed and then peeled off and removed from the substrate film. The film may be on one side or on both sides of the substrate film, and there is no particular limitation.
[0037] Regarding the base film having the coating as the object, not only the coating containing a water-soluble resin in consideration of the load on the environment, but also the base film having a coating containing other water-soluble resins can be the object. Among them, as the water-soluble resin, it is more preferable to use a water-soluble resin having at least one of water-soluble polyester resins, polyester urethane resins, acrylic resins, ethylene ionomer resins, polyvinyl alcohol resins, polyvinyl pyrrolidone resins, ethylene-vinyl alcohol resins, and starch as the main component.
[0038] The coating film containing a water-soluble resin may be a single layer containing a water-soluble resin, a laminate of two or more layers containing a water-soluble resin, or a laminate of a layer containing a water-soluble resin and a layer not containing a water-soluble resin.
[0039] In addition, it is particularly preferred that a release film with a film contains a release component in addition to a water-soluble resin in a part of the film, which can effectively show the film peeling effect. The so-called release component mentioned here refers to a component that increases the contact angle of the film surface with respect to water, that is, reduces the surface energy of the film. For example, a thermosetting silicone resin compound with dimethylsiloxane as the main skeleton as a curable silicone resin, or a UV-curable silicone resin compound that is cured by irradiating ultraviolet (UV) light with a photopolymerization initiator in an organic polysiloxane containing an acryloyl group or a methacryloyl group, and further, a compound having a long-chain alkyl group and a compound having fluorine can be listed. The film can be mixed with a water-soluble resin and a release component, or can be stacked with various layers. In the case of a laminated film, it is preferred that a layer containing a water-soluble resin is formed directly above the base film, and then a layer containing a release component is formed on the outermost surface. The release component is particularly preferably a thermosetting silicone resin compound with a main skeleton of dimethylsiloxane having high water permeability.
[0040] [Method for peeling off a coating from a substrate film having a coating]
[0041] The film stripping method of the present invention is as follows: on the film surface of a substrate film having a film containing the water-soluble resin on at least one side, the film is stripped at a rate of 1 m2 per m3 of the film. 2 A cleaning liquid containing water as a main component is applied in an amount of 3 ml to 650 ml to the surface area, a stripping member is brought into contact with the surface of the film to which the cleaning liquid is applied, and an angle formed by the substrate film across the stripping member is set in the range of 20° to 150°, and a tension is applied in the range of 10 N / m to 1000 N / m in at least one direction in the longitudinal direction of the substrate film, and the substrate film is relatively moved relative to the stripping member in the longitudinal direction thereof, thereby removing the film from the substrate film having the film.
[0042] The method of imparting the cleaning liquid to the film surface in the film stripping method of the present invention may be any method, for example, the cleaning liquid may be imparted in the form of droplets using a spray nozzle, or a high-pressure cleaning machine or a steam generator may be used to impart a high-pressure or high-temperature cleaning liquid. The amount of cleaning liquid imparted is preferably appropriately adjusted according to the properties or thickness of the film to be stripped, and can be properly managed according to the method of imparting the cleaning liquid. For example, the cleaning liquid can be managed by conveying the cleaning liquid using a metering pump, or a flow meter can be set midway in the flow path for conveying the cleaning liquid, or the cleaning liquid imparted to the film surface can be recovered for mass measurement. Alternatively, in the case where the water-soluble resin contains a cleaning liquid and it is difficult to perform mass measurement, the base film with the film and the imparted cleaning liquid, the film after stripping, and all of these can be recovered to calculate the amount of cleaning liquid imparted.
[0043] The present inventors have made intensive research and have confirmed that when the film thickness of the water-soluble resin is set to 20×10 -6 In the case of the film thickness between 1.0 mm and 1.0 mm, the amount of cleaning liquid applied is set to 1 m 2 The film peeling effect can be obtained when the surface area is 3ml or more. 2 When the surface area is less than 3 ml, the film stripping effect sometimes becomes low. In particular, when the humidity of the surrounding environment is low, the cleaning liquid is dried before the cleaning liquid dissolves or swells the film containing the water-soluble resin, and the film stripping effect sometimes cannot be obtained. On the other hand, the more the cleaning liquid is applied, the more reliably the film containing the water-soluble resin can be dissolved or swelled, and the film stripping effect is improved. In particular, it was confirmed that when the film thickness of the water-soluble resin is 1.0 mm, by adding 1 m of the film, the film stripping effect is improved. 2 The film peeling effect can also be obtained by applying 650 ml of the cleaning solution to the film surface.
[0044] The cleaning liquid used in the film stripping method of the present invention can show its effect in any solvent as long as it can dissolve the water-soluble resin, but in order to reduce the environmental load, it is preferably water. In addition, by adding a surfactant or the like as a main component to water, the wettability of the cleaning liquid and the film surface can be improved, so that the cleaning liquid can be easily spread over the entire film.
[0045] Regarding the stripping member in the film stripping method of the present invention, a scraper or cloth, a metal plate, a rotating brush roller, etc. are exemplified, but it is not limited to these. As long as it can directly contact the substrate film with the film and physically strip the film, it can be any means. In addition, the stripping member is preferably in direct contact with the surface of the substrate film with the film in a manner of pressing the stripping member, and the substrate film is made to be in a state of bending or curving by the stripping member. While maintaining the state, the substrate film is relatively moved relative to the stripping member in its length direction, thereby stripping the film from the substrate film. The substrate film in the state of bending or curving is preferably set to the angle between the substrate film and the stripping member in the range of 20° to 150°, and a tension is applied in the range of 10N / m to 1000N / m in at least one direction in the length direction. As a result, the stripping member can be strongly pressed against the film surface of the substrate film, so that the film dissolved or swollen by the cleaning liquid can be efficiently and reliably stripped. Therefore, the narrower the range in which the stripping member contacts the base film having the coating, the more locally and strongly the stripping member can be pressed against the coating surface of the base film. Therefore, it is preferred to use a scraper or a corner of a metal plate among the stripping members exemplified above.
[0046] When the angle formed by the base film sandwiching the stripping member is set to less than 20°, the space for installing the stripping member becomes very narrow, which is not realistic. On the other hand, when the angle is set to more than 150°, it is confirmed that although the force pressing the stripping member against the film surface of the base film is weakened, it is possible to strip the film on a part of the film that is easy to strip. However, it is confirmed that when the tension changes when the base film and the stripping member are relatively moved in the longitudinal direction of the base film or when the stripping speed is increased, air is easily included between the base film and the stripping member, and sometimes a part of the film cannot be stripped and drills out, thereby remaining on the base film.
[0047] It was confirmed that the film peeling effect was achieved by setting the tension applied to at least one direction of the length direction of the substrate film to 10 N / m or more. When the substrate film was transported with the tension applied being less than 10 N / m, it was not possible to transport it stably due to the low tension, and sometimes the tension fluctuated greatly, or it meandered during transport, and the film could not be peeled off. On the other hand, when the tension exceeding 1000 N / m was applied, the substrate film was strongly stretched in one direction, so that a plurality of iron sheet wrinkles were generated in the width direction and the length direction of the substrate film, and some of the iron sheet wrinkles became folded wrinkles at the locations where they contacted the peeling member, and sometimes the film could not be peeled off at the folded wrinkles.
[0048] The film stripping method of the present invention is to strip the film from the substrate film having the film by moving the substrate film having the film as the preferred embodiment relative to the stripping member in the longitudinal direction thereof. The means for moving the substrate film relative to the stripping member may be any means, and the stripping member may be fixed and only the substrate film may be transported, or the stripping member may be moved relative to the stationary substrate film. Alternatively, both the stripping member and the substrate film may be moved, and the two may also move in the same direction or in different directions. When the substrate film is transported, it is preferred to keep the tension applied to the substrate film constant, and it is also preferred to keep the tension constant when the transport speed of the substrate film is changed or the transport stop and start are repeated.
[0049] When the base film having the target coating has the coating continuously or intermittently in the longitudinal direction of the base film, it is preferred to convey the base film and perform the coating peeling with the peeling member extended and fixed in the short-side direction of the base film.
[0050] In particular, when the substrate film having a film has a film intermittently in the longitudinal direction of the substrate film, or the amount of the film formed on the substrate film in the longitudinal direction of the substrate film is different, the time for the film to be dissolved or swelled by the cleaning liquid can be changed by making the conveying speed of the substrate film variable, or the time for the portion having the film to contact the stripping member can be changed, thereby appropriately adjusting so that the film stripping can be performed more efficiently. The time for the film to be dissolved or swelled, that is, the time from the application of the cleaning liquid to the stripping of the film by the stripping member is preferably appropriately determined according to the properties of the film, but is preferably 0.05 seconds to 10 seconds in view of the size of the device, etc.
[0051] In addition, in the case where the base film with the film has the film at a certain interval in the longitudinal direction of the base film, the film stripping can be performed by stopping the conveying of the base film for a certain length or changing the conveying speed, and moving the stripping member relative to the portion of the base film with the film. After the film is stripped, the film can be stripped efficiently and reliably by restarting the conveying or restoring the conveying speed. In addition, by stopping the conveying or changing the conveying speed in the middle of the film stripping, the base film after the film stripping can be checked during this period to check whether the film remains. The inspection method can be any means as long as it can detect the remaining film.
[0052] In the film stripping method of the present invention, within the range where the stripping member contacts the film surface of the base film having the film, the contact length in the longitudinal direction of the base film is set to L, the plane passing through the center position of the contact length and perpendicular to the surface of the stripping member is set to the vertical plane, the side of the base film relatively close to the stripping member is set to the upstream side, and the side of the base film relatively far from the stripping member is set to the downstream side, and the contact length L [m] is 1×10 -5 m~1×10 -3 m, the angle (acute angle) θ1[°] formed by the vertical plane and the substrate film located upstream of the vertical plane, the angle (acute angle) θ2[°] formed by the vertical plane and the substrate film located downstream of the vertical plane, the tension T1[N / m] applied to the substrate film located upstream of the vertical plane, and the tension T2[N / m] applied to the substrate film located downstream of the vertical plane are preferably such that the film is peeled off as in the following formula (1).
[0053] Formula (1): 1.0×10 6 ≦{T1×cos(θ1)+T2×cos(θ2)} / L≦2.4×10 8
[0054] The shorter the contact length L, the stronger the contact between the peeling member and the film surface of the base film can be. The inventors have made intensive research and found that the shortest contact length L is 5×10 -6 m is the limit of machining. -6 m, burrs will appear during processing, or even if the burrs are removed by abrasive paper or abrasive cloth, there will be residual grinding marks, and it is impossible to reduce the size of the burrs to less than 5×10 -6 On the other hand, when the contact length L is larger than 1×10 -3 m, in order to satisfy the above formula (1), it is necessary to set the tension T1 and the tension T2 to be large, and then make the angle θ1 and the angle θ2 formed by the vertical plane and the base film as small as possible. In this case, even if the film stripping conditions are adjusted according to the properties of the film to be stripped, the adjustable range in the above formula (1) is narrowed, so only the film with properties that are relatively easy to strip can be stripped.
[0055] In the film stripping method of the present invention, when using Figure 2 When a rigid body such as a scraper or a metal plate having a front end shape shown in FIG. 1 is used as a stripping member, it is preferred to set the angle θ3 formed by the surface of the stripping member and the surface of the substrate film before contacting the ridgeline (hereinafter, sometimes referred to as the upstream side surface r1 of the stripping member) and the substrate film before contacting the ridgeline to be 5° or more to strip the film. When the angle is set to less than 5°, it is confirmed that the film (hereinafter referred to as the stripping material) after stripping is accumulated between the substrate film relatively close to the stripping member and the upstream side surface r1 of the stripping member. It is rare that when the film is continuously stripped, a part of the accumulated stripping material flows out in a manner that overflows to the end of the short side direction of the substrate film and adheres to the side of the end of the short side direction of the substrate film or the back of the substrate film. On the other hand, it is confirmed that the accumulated stripping material is significantly reduced by setting the angle θ3 to be 5° or more. When the angle is 5° or more, the peeling material does not flow along the upstream side surface r1 of the peeling member and overflow in the short-side direction of the base film, and the film can be peeled stably and continuously.
[0056] [Device for peeling off a film from a base film having a film]
[0057] The preferred embodiment of the film peeling device of the present invention will be described based on the drawings. In addition, the following description exemplifies one embodiment of the present invention, and is not limited thereto, and various changes can be made within the scope of the gist of the present invention.
[0058] Figure 11 is a schematic diagram of a film stripping device 101 according to an embodiment of the present invention. The film stripping device 101 includes a winding device 4 for winding out a base film 2 having a film, and a winding device 5 for winding up a base film 3 after the film is stripped. The film stripping device 101 includes a driving device 9 for conveying the base film 2 having a film, a spray head 6 as a cleaning liquid imparting mechanism for imparting a cleaning liquid 11 to the film of the base film 2 having a film, a peeling member 7 for stripping the film of the base film 2 having a film together with the cleaning liquid 11, and a driving device 10 for conveying the base film 3 after the film is stripped. In addition, the cleaning liquid imparting mechanism includes, in addition to the spray head 6, a liquid feeding pump 12 for conveying the cleaning liquid 11 to the spray head 6, and a tank (not shown) for storing the cleaning liquid.
[0059] The substrate film is transported by the drive device 9 and the drive device 10, and the substrate film moves in the longitudinal direction relative to the stripping member 7. In addition, in order to stably transport the substrate film, the drive device 9 and the drive device 10 are preferably a structure that can cut off the tension. In the case of tension cutting using a suction roller, sometimes a part of the film of the substrate film 2 with a film is sucked and becomes a cause of failure, so it is more preferred to use a structure clamped by a metal drive roller and a rubber roller. The drive device 9 and the drive device 10 also function as a tension imparting mechanism. Furthermore, the drive rollers of the drive devices 9 and the drive devices 10 are preferably equipped with the following mechanism (tension control mechanism): the rotation speed can be set separately, and the tension imparted to the substrate film between the drive device 9 and the drive device 10 in the longitudinal direction of the substrate film can be controlled by controlling the rotation speed. As long as a mechanism that can control the tension imparted to the substrate film in the longitudinal direction of the substrate film is included, it is not limited to this. In order to control the tension, a tension meter (not shown) may be provided between the drive device 9 and the stripping member 7, or between the stripping member 7 and the drive device 10, or both, to feed back the rotation speed of the drive rollers of the drive device 9 and the drive device 10 so as to achieve a predetermined tension. In addition, an accumulator (not shown) may be provided at the side of the unwinding device 4 closer to the stripping member 7 so that the speed at which the base film 2 with the film is unwound from the unwinding device 4 can be varied, so that even if the base film 2 with the film is transported intermittently due to replacement of the base film 2 with the film rolled up in the unwinding device 4, handling of a fault in operation occurring in the film stripping device 101, or inspection before the film is stripped, the film can be stripped at a constant speed. In addition, a dancer roller (not shown) may be provided between the drive device 9 and the drive device 10 to reduce the tension fluctuation generated when the transport speed is changed, but the present invention is not limited to these as long as the transport speed is varied and the tension fluctuation can be reduced.
[0060] In addition, in the present embodiment, the base film is transported by the driving devices 9 and 10, so the base film moves in the longitudinal direction relative to the peeling member 7, but as long as the base film can move in the longitudinal direction relative to the peeling member 7, it is not necessary to be limited to a mechanism that transports the base film by the driving devices 9 and 10. It may include a mechanism that moves the peeling member 7 relative to the stationary base film, or a mechanism that moves both the peeling member 7 and the base film, or a mechanism that moves both in the same direction or in different directions.
[0061] In addition, the spray head 6 and the peeling member 7 as part of the cleaning liquid applying mechanism are surrounded by the small chamber 8. The spray head 6 only needs to spray the cleaning liquid 11 and apply it to the film surface of the base film 2 having the film, and examples thereof include a slit nozzle or a spray nozzle, but are not limited thereto. The amount of the cleaning liquid 11 applied to the film surface of the base film 2 having the film is preferably 3 ml / m 2 ~650ml / m 2 range, so that the film containing the water-soluble resin is fully dissolved. In order to apply the cleaning liquid 11 in the amount required for peeling the film to the film surface of the substrate film 2 having the film, the specifications of the spray head 6 and the liquid feeding pump 12 can be determined and adjusted. The amount of cleaning liquid 11 applied can be controlled by using a metering pump in the liquid feeding pump 12, or by providing a flow meter (not shown) between the liquid feeding pump 12 and the spray nozzle 6, and feeding back the indicated value of the flow meter for control. Alternatively, the sprayed cleaning liquid 11 can be recovered, the amount applied can be determined based on its quality, and the amount applied can be fed back to the liquid feeding pump to control the amount applied.
[0062] The ejection head 6 and the peeling device 7 only need to be arranged facing the film surface of the base film 2 having the film. Figure 1 In the embodiment, the coating is stacked on the lower surface side of the substrate film 2, and the spray head 6 and the stripping device 7 are arranged in a manner facing the lower surface side of the substrate film 2 stacked with the coating, but are not limited to being arranged toward the lower surface side of the substrate film 2. In addition, in order to allow the coating of the substrate film 2 rolled into a roll to be handled on either the inner side or the outer side of the roller, the unwinding device is more preferably a mechanism that can handle either the upper unwinding or the lower unwinding, so as to switch the unwinding direction of the substrate film 2 with the coating, and the coating surface of the substrate film 2 with the coating can be transported facing the spray head 6 and the stripping device 7.
[0063] In order to accelerate the dissolution of the water-soluble resin contained in the film, the spray head 6 is preferably capable of spraying the heated cleaning liquid 11. Regarding the heating of the cleaning liquid 11, a heat source such as a cartridge heater may be included in the spray head 6, or a tank (not shown) storing the cleaning liquid may be heated, but any means may be used as long as the cleaning liquid 11 can be heated, and it is not limited to these. In order to dissolve the water-soluble resin contained in the film more quickly, the cleaning liquid 11 may be sprayed from the spray head 6 in the form of steam. Generally speaking, it is difficult to measure the amount of steam sprayed accurately, so the amount of liquid reduced from the tank storing the cleaning liquid 11 within a certain period of time can be measured as the amount of cleaning liquid 11 applied.
[0064] In order to eject the heated cleaning liquid 11 , the material of the ejection head 6 is preferably heat-resistant, and preferably metal or heat-resistant resin is used.
[0065] Figure 2 1 is a schematic cross-sectional view of a stripping member 7 of a first embodiment in a film stripping device 101. The stripping member 7 is in direct contact with the film surface of the base film 2 having the film, and is arranged so that the angle formed by the base film through the stripping member 7, that is, the angle (θ1+θ2) formed by the base film 3 after the film stripping and the base film 2 before the film stripping, is in the range of 20° to 150°. When the angle is less than 20°, the stripping member 7 bends or vibrates when the film is stripped from the base film 2, or deforms or breaks when the tension applied to the base film 2 is high, and the stripping member 7 may cause a defect in the film stripping. In addition, when the angle is greater than 150°, the force pressing the stripping member 7 against the base film 2 becomes weak. When the base film 2 is conveyed in the above state and the film stripping is performed, the force pressing the stripping member 7 against the base film 2 is insufficient due to only a slight change in the tension applied to the base film 2, and the film stripping may not be able to be stripped, and a part of the film may remain on the base film.
[0066] In addition, the tension (T1, T2) in the length direction of the substrate film applied to the substrate film is controlled by the tension control mechanism, and the tension is preferably adjustable within the range of 10N / m to 1000N / m. As long as the applied tension and the angle formed by the substrate film across the stripping member 7 are adjusted according to the properties of the substrate film 2 having the film to be stripped, the higher the tension, the smaller the angle between the substrate films, and the more strongly the substrate film 2 with the film can be pressed to the stripping member 7, so the film can be more reliably stripped. However, when the pressing force is too strong, it will exceed the breaking strength of the substrate film, and sometimes the substrate film will break. In the case of the substrate film breaking, the film cannot be continuously stripped, which significantly deteriorates the operating efficiency of the film stripping device 101. The inventors and others have repeatedly conducted multiple studies, and it has been confirmed that by setting the tension to less than 1000N / m, the film can be continuously stripped without breaking the substrate film even when the angle formed by the substrate film is reduced. It was also confirmed that when the tension exceeded 1000 N / m, the base film was rarely broken based on foreign matter attached to the front end of the stripping member 7 or a tiny burr generated during the processing when the stripping member 7 was manufactured. On the other hand, the lower the tension, the smaller the force pressing the stripping member 7 against the base film, so although it is difficult to peel off the film, as long as the film is easy to peel off, the film can be peeled off even with a small tension. However, when the tension is reduced, the conveying state of the base film is significantly deteriorated. When the base film is conveyed at a low tension of less than 10 N / m, the base film meanders during conveyance, or wrinkles are generated in the base film, and a portion that is not in direct contact with the stripping member 7 is generated in the width direction of the base film, and the film cannot be peeled off. The lower limit of the tension is preferably 50 N / m or more, and more preferably 100 N / m or more.
[0067] like Figure 2 As shown in FIG. 1 , the peeling member 7 in the peeling device 101 of the present invention is arranged to directly contact the film surface of the base film 2 having the film, and the angle (θ1+θ2) formed by the base film across the peeling member 7 is adjusted to a range of 20° to 150°. In this state, the contact length L in the longitudinal direction of the base film of the range where the peeling member 7 contacts the film surface is preferably 1×10 -5 m~1×10 -3 At this time, in order to further increase the force pressing the peeling member 7 against the base film, the contact length L is as short as possible. Therefore, the inventors want to make the contact portion of the peeling member 7 with the film surface as sharp as possible. As a result, the contact length L is limited to 5×10 -6 m. When the contact length L is set to 5×10 -6m, under the condition that the force pressing the peeling member 7 against the base film is strong, a strong force is locally applied, so the tip of the peeling member 7 may be deformed. Therefore, it is known that in order to prevent the tip of the peeling member 7 from deforming under various conditions, the contact length L is more preferably set to 1×10 -5 m or more. When the contact length L is long, the force pressing the peeling member 7 against the base film is widely dispersed by the contact length L, so that the film is difficult to peel off. The inventors have made intensive research and found that by setting the contact length L to 1×10 -3 m or less, even if the properties of the target film change, the film can be peeled off by adjusting the amount of cleaning liquid 11 applied, the tension applied to the base film, and the angle between the base films sandwiched by the peeling member 7. -3 In the case of 0.1% to 0.2%, the force pressing the peeling member 7 against the base film is dispersed and reduced, so that it is difficult to peel the coating film stably, and a part of the coating film remains.
[0068] Figure 3 1 is a schematic diagram of the second peeling member 13 in the film peeling device 101 of the present invention. Figure 3 As shown, the contact length L in the longitudinal direction of the base film of the range where the peeling member 13 contacts the film surface also includes the case where the front end of the peeling member 13 is an arc. Figure 4 1 is a schematic diagram of the third peeling member 14 in the film peeling device 101 of the present invention. Figure 4 As shown in FIG. 1 , when the range of the peeling member 14 in contact with the film surface covers multiple surfaces, the contact length L corresponds to the sum of L1, L2, and L3. In the peeling member 14, the sum of L1, L2, and L3 as the contact length L is preferably 1×10 -5 m~1×10 -3 The range of m.
[0069] In order to prevent the cleaning liquid 11 from scattering around and to prevent the temperature of the cleaning liquid 11 from decreasing when the cleaning liquid 11 is heated, the chamber 8 of the stripping device 101 is provided so as to surround the ejection head 6 to the stripping device 7. Since the interior of the chamber 8 becomes high temperature, the material of the chamber 8 is preferably heat-resistant, and metal or glass is preferably used.
[0070] In order to stably produce a regenerated film after remelting, the base film 3 wound by the winding device 5 is preferably completely dehydrated, and a drying device (not shown) may be provided between the peeling device 7 and the winding device 5. The drying device can be provided before winding, either before or after the driving device 10.
[0071] In addition, in order to confirm the quality of the base film 3 after the film is peeled off, an inspection machine (not shown) for detecting the residue of the film or environmental foreign matter attached during the process may be provided before the winding device 5. The inspection machine can be selected according to the properties of the base film 3, and it is preferred to use an inspection machine that uses transmitted light or reflected light. In addition, a marking device (not shown) for recording the position of the residue of the film or environmental foreign matter attached during the process detected by the inspection machine may be provided between the inspection machine and the winding device 5. As long as the position of the detection object can be marked, the marking method using the marking device may be any method such as a pen, a sticker, or a laser. By marking the residue of the film or the environmental foreign matter attached during the process, the said part can be removed before remelting, so that the regenerated film can be produced more stably, and the quality of the regenerated film can be prevented from deteriorating.
[0072] In the film stripping device of the present invention, the substrate film with the film may be in the form of a cut single sheet, and is particularly preferably a substrate film with the film rolled up. The film stripping process can be continuously and efficiently performed by unwinding the rolled substrate film with the film, stripping the film using the film stripping device of the present invention, and winding up the substrate film after the film is stripped.
[0073] In addition, in order to dissolve and swell the film more efficiently by applying the cleaning liquid 11 to the film surface of the base film with the film, a device for exposing the layer containing a large amount of water-soluble resin in the film of the base film 2 with the film may be provided between the unwinding device 4 and the driving device 9. In particular, when the film of the base film with the film is a thermosetting silicone resin compound with dimethylsiloxane as the main skeleton, the base film with the film is preferably used as a process release film in terms of its surface free energy characteristics, specifically, as a release film for extracting the release object in a desired shape after setting the release object on the film of the base film with the film. Since the base film with the film used as the process release film may have the release object remaining on the film surface, it is preferable to provide a device for exposing the film surface of the base film with the film between the unwinding device 4 and the driving device 9 to expose the film surface of the base film with the film. The device for exposing the film surface may be a contact type or a non-contact type, and is appropriately selected according to the remaining state of the object to be demolded.
[0074] The mold release object can be appropriately selected according to the characteristics of the film, and examples thereof include an adhesive containing inorganic substances such as metals formed by vapor deposition or organic substances such as acrylic acid formed by coating, and a ceramic green sheet containing barium titanate as a main component.
[0075] According to the above, by using the film stripping method and the film stripping device of the present invention, a small amount of cleaning liquid can be used to dissolve the water-soluble resin from the surface of the film having the film, and the film can be stripped efficiently and reliably. In addition, according to the film stripping method and the film stripping device of the present invention, a high-purity resin sheet without foreign matter can be obtained at a low cost without significantly increasing the environmental load, so that the regenerated film can be stably produced.
[0076] Example
[0077] Hereinafter, the present invention will be described with reference to Examples, but the present invention is not necessarily limited thereto.
[0078] <Base film with coating>
[0079] The following coated films were produced.
[0080] <Coated membrane>
[0081] A coating film of a polyvinyl alcohol resin as a water-soluble resin was formed with a film thickness of 0.1 μm on one surface of a polyethylene terephthalate substrate film having a thickness of 30 μm and a width of 100 mm.
[0082] Furthermore, a coating film of a curable silicone resin as a release component was formed thereon in the following manner so as to have a film thickness of 0.1 μm with reference to the coating material described in Japanese Patent Application Laid-Open No. 2015-189226.
[0083] By
[0084] Thermosetting silicone, manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KS-847T": 100 parts by mass,
[0085] · Platinum catalyst, manufactured by Shin-Etsu Chemical Co., Ltd., trade name "CAT-PL-50T": 3 parts by mass was prepared by dissolving in a mixed solution of toluene and methyl ethyl ketone (MEK) as a solvent (the mass ratio of toluene:MEK was 1:1) so that the solid content was 1.8% by mass. Then, it was applied on the film of the polyvinyl alcohol resin using a bar coater, and dried in an oven at 90°C for 20 seconds to form a film of the release component, thereby obtaining a film with a film.
[0086] <Peeling evaluation method>
[0087] (1) Peelability of the film
[0088] The evaluation of peeling is measured by the following method using a commercially available Dyne Pen (surface energy: 30mN / m, 70mN / m). Under a room temperature of 23°C, the sample surface is drawn using a Dyne Pen. When the state is maintained for more than 4 seconds, it is judged that the surface energy of the sample surface is higher than the surface energy of the Dyne Pen. If the film of the release component of the film with a film remains on the surface, the surface energy of these is less than 30mN / m, so any Dyne Pen will bounce off the reagent on the sample surface and cannot maintain the drawing. On the other hand, when the film of the release component is peeled off and the water-soluble polyvinyl alcohol resin is exposed, the surface energy is more than 70mN / m, so any Dyne Pen can maintain the drawing. When both the film of the release component and the film of the water-soluble polyvinyl alcohol resin are peeled off to expose the polyethylene terephthalate, the surface energy is 43.8 mN / m, so the drawing of the dyne pen of 30 mN / m is maintained, but the drawing of the dyne pen of 70 mN / m cannot be maintained. The above evaluation method is used to determine whether the film with a film is peelable.
[0089] If the film of the release component of the film with a film remains on the surface, the release component will be mixed into the recycled resin sheet, so the recycled resin sheet will be colored (yellowing) or foreign matter will be generated, so the quality of the recycled resin sheet will deteriorate and it will not be practical. In the case where the film of the release component is peeled off, but a part of the film of the water-soluble polyvinyl alcohol resin remains, the recycled resin sheet will be slightly colored (yellowing), and although the quality is slightly inferior to the quality of the raw material, it is within the practical range. If both the film of the release component and the film of the water-soluble polyvinyl alcohol resin are peeled off, it will become a good quality as a recycled resin sheet.
[0090] (2) Quality of recycled resin sheets
[0091] (i) Melt film forming properties
[0092] After the coated film is peeled off from the film with the film, the base film is recovered. After the recovered base film is crushed by a crusher, the recycled resin sheet granulated by a granulator is dried at 180°C for 2 hours, put into an extruder, melt-extruded at 280°C, and formed into a sheet on a casting drum cooled to 25°C to confirm whether the polyethylene terephthalate film can be produced without any problem.
[0093] (ii) Intrinsic viscosity
[0094] The intrinsic viscosity IV(R) of the sheet obtained in (i) is measured. Regarding the intrinsic viscosity IV(R), a polyethylene terephthalate film is dissolved in 100 ml of o-chlorophenol (solution concentration C = 1.2 g / dl), and the viscosity of the solution at 25°C is measured using an Ostwald viscometer. In addition, the viscosity of the solvent is measured in the same manner. Using the obtained solution viscosity and solvent viscosity, [η] (dl / g) is calculated by the following formula (a), and the obtained value is used as the intrinsic viscosity.
[0095] (a) ηsp / C=[η]+K[η] 2 ·C
[0096] (Here, ηsp=(solution viscosity (dl / g) / solvent viscosity (dl / g))-1, and K is the Huggins constant (set to 0.343)).
[0097] Next, before the film with a coating is produced, the intrinsic viscosity IV(I) of the base film before the coating is formed, which is sampled in advance, is measured in the same manner.
[0098] Since the quality reduction of the resin sheet caused by the mixing of foreign matter is expressed as the difference between IV(R) and IV(I), ΔIV is calculated according to the following formula (b), and the determination is performed as follows using the obtained value.
[0099] (b) ΔIV=IV(R)-IV(I)
[0100] The difference in intrinsic viscosity is 0.05 or less: This is within the range where there is no problem in the quality of the recycled resin sheet.
[0101] The difference in intrinsic viscosity is more than 0.05 and less than 0.2: Although the quality as a recycled resin sheet is slightly inferior, it is within the practical range.
[0102] The difference in intrinsic viscosity exceeds 0.2: The quality of the recycled resin sheet is not practical.
[0103] <Example 1>
[0104] Place the membrane with the membrane on Figure 1 The unwinding device 4 of the stripping device 101 is shown.
[0105] A spray nozzle (two-fluid method) was used as the spray head 6 for spraying the cleaning liquid 11. The cleaning liquid was set to 60°C warm water, and the spraying amount was adjusted to 100% per 1m of the film using a diaphragm pump. 2 The surface area is 3ml to 650ml and is directly applied to the membrane.
[0106] The peeling member 7 is used as Figure 2The width of the front end of the stainless steel plate in the substrate conveying direction is set to 1.0×10 -5 m. The peeling member 7 was arranged so that the angle (θ1+θ2) between the substrate films was 90° (θ1: 45°, θ2: 45°). It was confirmed that the length L of the substrate film and the front end of the plate in direct contact in the conveying direction was 1.0×10 -5 The ejection head 6 and the peeling member 7 were arranged so that the base film reached the peeling member 7 1 second after the warm water was supplied from the ejection head 6 .
[0107] The film was peeled off by conveying the base film while applying a tension of 10 N / m from two directions in the longitudinal direction of the base film. In addition, the film was peeled off by setting the tension to 500 N / m and 1000 N / m in the same device configuration.
[0108] The film was taken up by the winding device 5, and the peeled film was collected. The peeled state of the film was confirmed by a dyne pen. The result showed that under the condition of tension of 1000 N / m, if the moisture content was adjusted to 3 ml / m 2 ~650ml / m 2 If the moisture content is adjusted to 10 ml / m under the condition of 500 N / m tension, the film of the hardened silicone resin and the water-soluble polyvinyl alcohol resin of the release component can be peeled off. 2 ~650ml / m 2 On the other hand, under the condition of tension of 10N / m, by setting the amount of water given to 100ml / m 2 As described above, it was confirmed that both the films of the curable silicone resin as the release component and the water-soluble polyvinyl alcohol resin can be peeled off.
[0109] Then, the base film 3, which can be confirmed to have been peeled off, was recovered and formed into a sheet by the method described in (2) (i) to produce a polyethylene terephthalate film. No bubbles or gels were found in the molten polymer, and no abnormalities such as pressure rise occurred, and a polyethylene terephthalate film was obtained. The difference in intrinsic viscosity at each level is shown in Figure 5 The difference in intrinsic viscosity at any level was less than 0.2, which was not a practical problem. It was confirmed that the greater the amount of water imparted, the higher the tension imparted, and the smaller the difference in intrinsic viscosity, that is, the better the quality of the recycled resin sheet.
[0110] <Example 2>
[0111] Place the membrane with the membrane on Figure 1The unwinding device 4 of the stripping device 101 is shown.
[0112] The amount of water imparted to the film was set to 100 ml / m 2 Furthermore, the angle (θ1+θ2) formed by the base film via the peeling member 7 was set to 20°, and the tension was set to 500 N / m. The film was peeled off in the same manner as in Example 1 otherwise. In addition, the same device was used to construct the apparatus, but the angle (θ1+θ2) was modified to be changeable, and the angle (θ1+θ2) was changed to 45° (θ1: 22.5°, θ2: 22.5°), 60° (θ1: 30°, θ2: 30°), 90° (θ1: 45°, θ2: 45°), 120° (θ1: 60°, θ2: 60°), 150° (θ1: 75°, θ2: 75°), 170° (θ1: 45°, θ2: 45°), or the tension was changed to 10 N / m, 50 N / m, 100 N / m, 250 N / m, 500 N / m, 750 N / m, 1000 N / m in both directions, and the film was peeled off in the same manner. The distance between the ejection head 6 and the peeling member 7 was adjusted so that the ejection head 6 reached the peeling member 7 1 second after the warm water was applied to the substrate film.
[0113] The film was wound up by the winding device 5, and the base film 3 after the film was peeled off was collected, and the peeling state of the film was confirmed by a dyne pen. Figure 6 The film can be peeled off at each level. The "○" in the figure indicates the condition under which the film of the hardened silicone resin and the water-soluble polyvinyl alcohol resin, which are the demolding components, can be peeled off. The "△" in the figure indicates the condition under which the hardened silicone resin can be peeled off, but a part of the polyvinyl alcohol resin remains on the surface of the substrate film. The "×" in the figure indicates the condition under which a part of the hardened silicone resin and the polyvinyl alcohol resin remain on the surface of the substrate film. According to the results, it was confirmed that the more obtuse the angle between the film and the substrate film is when the film is peeled off, or the lower the tension applied, the more the film will have peeling residue.
[0114] Then, the base film 3 was recovered, crushed by a crusher, and made into a resin sheet by a granulator. Thereafter, it was put into an extruder, melt-extruded at 280°C, and formed into a sheet on a casting drum cooled to 25°C to produce a polyethylene terephthalate film. Figure 6In the resin sheet recovered under the condition of "×", gel was generated in the molten polymer, and the device was abnormal due to the pressure increase, so the polyethylene terephthalate film could not be obtained. On the other hand, in the resin sheet recovered under the condition of "△", no bubbles or gels were confirmed in the molten polymer, and no abnormalities such as pressure increase occurred, and a polyethylene terephthalate film could be obtained. Thereafter, the difference in inherent viscosity was confirmed, and the result confirmed that it was in the range of more than 0.05 and less than 0.2 under any condition. Although the quality as a recycled resin sheet is slightly poor, it is within the practical range. In the resin sheet recovered under the condition of "○", it was confirmed that a polyethylene terephthalate film can be stably obtained, and the difference in inherent viscosity is also less than 0.05, which is within the range where there is no problem with the quality as a recycled resin sheet.
[0115] <Example 3>
[0116] Place the membrane with the membrane on Figure 1 The unwinding device 4 of the stripping device 101 is shown.
[0117] As the peeling member 7, various Figure 2 The stainless steel plate with the tip shape shown in the figure was changed in length L of the tip portion in direct contact with the base film in the conveying direction. Specifically, L was set to 1.0×10 -5 m, 2.5×10 -5 m, 5.0×10 -5 m, 1.0×10 -4 m, 2.0×10 -4 m, 5.0×10 -4 m, 7.5×10 -4 m, 1.0×10 -3 Each plate was prepared in the manner of m. The angle (θ1+θ2) formed by the base film across the peeling member 7 was changed in the range of 20° to 150°, and the tension was also changed in the range of 10N / m to 1000N / m. The distance between the ejection head 6 and the peeling member 7 was adjusted each time so that it reached the peeling member 7 1 second after the warm water was applied to the base film. In addition, the film was peeled off in the same manner as in Example 1.
[0118] The film was wound up by the winding device 5, and the base film 3 after the film was peeled off was collected, and the peeling state of the film was confirmed by a dyne pen. Figure 7 The correlation between the film availability at each level and {T1×cos(θ1)+T2×cos(θ2)} / L is shown in FIG. In addition, the meanings of the symbols in the figure are the same as those in Example 2. It was confirmed that when the contact length L was 1×10 -5 m~1×10 -3 m, in the range of satisfying formula (1): 1.0×10 6≦{T1×cos(θ1)+T2×cos(θ2)} / L≦2.4×10 8 In particular, it was confirmed that the smaller the contact length L, the more easily the film can be peeled off.
[0119] Then, the base film 3 was recovered, crushed by a crusher, and made into a resin sheet by a granulator. Then, it was put into an extruder, melt-extruded at 280°C, and formed into a sheet on a casting drum cooled to 25°C to make a polyethylene terephthalate film. The difference in intrinsic viscosity was confirmed for the level at which a polyethylene terephthalate film can be made. The result was Figure 7 The same results as those in Example 2 can be obtained at the levels of "△" and "○".
[0120] <Comparative Example 1>
[0121] Place the membrane with the membrane on Figure 1 The unwinding device 4 of the peeling device 101 shown in the figure is adjusted to the spraying amount of the cleaning liquid 11 per 1m of the film. 2 The film was peeled off in the same manner as in Example 1 except that the surface area was changed to 2 ml.
[0122] The substrate film 3 after film peeling was collected by winding up using a winding device 5, and the peeling state of the film was confirmed using a dyne pen. As a result, it was confirmed that the films of the curing silicone resin and the water-soluble polyvinyl alcohol resin of the release component both remained. Since it was confirmed that any of the films remained, the subsequent evaluation was not carried out.
[0123] <Comparative Example 2>
[0124] Place the membrane with the membrane on Figure 1 The unwinding device 4 of the stripping device 101 shown in the figure. A tension of 1100 N / m was applied from two directions in the longitudinal direction of the base film. In addition, the film was stripped in the same manner as in Example 1. By applying high tension, iron-like wrinkles were generated in the base film in the conveying direction. Since the generated wrinkles directly passed through the stripping member 7, it was possible to visually confirm that the film remained at the same position as the wrinkle generation position in the film width direction.
[0125] The base film 3 after the film was peeled off was taken up by the winding device 5, and the peeling state of the film was confirmed by the dyne pen. As a result, it was confirmed that the film of the hardened silicone resin of the mold release component and the water-soluble polyvinyl alcohol resin remained at the same position as the wrinkle generation position in the film width direction. On the other hand, it was confirmed that the film of the hardened silicone resin of the mold release component and the water-soluble polyvinyl alcohol resin could be peeled off at the position where the wrinkle did not generate. Since it is difficult to extract only the part where any film can be peeled off from the recovered base film 3, the subsequent evaluation was not carried out.
[0126] Industrial Applicability
[0127] The base film having a coating that can be applied to the method and device for stripping a coating from a base film having a coating of the present invention is not limited to a film having a coating containing a water-soluble resin on one side of the base film, but any regenerable resin film, paper film, or metal film having a coating containing a readily soluble resin layer will suffice.
[0128] Explanation of symbols
[0129] 2: Base film with coating
[0130] 3: Base film
[0131] 4: Roll-out device
[0132] 5: Winding device
[0133] 6: Spray head
[0134] 7, 13, 14: Stripping equipment
[0135] 8: Small room
[0136] 9, 10: Driving device
[0137] 11: Cleaning fluid
[0138] 12: Liquid delivery pump
Claims
1. A method for peeling a film, which is a method for peeling a film from a base film having a film containing a water-soluble resin on at least one surface, wherein: For every 1m of the membrane 2 A cleaning liquid containing water as a main component is applied to the film in an amount ranging from 3 ml to 650 ml on the surface area. A stripping member is brought into contact with the surface of the coating film to which the cleaning liquid is applied, an angle formed by the substrate film across the stripping member is set in the range of 20° to 150°, a tension is applied in the range of 10 N / m to 1000 N / m in at least one direction along the length direction of the substrate film, and the substrate film is relatively moved relative to the stripping member in the length direction of the substrate film to strip the coating film from the substrate film.
2. The film stripping method according to claim 1, wherein: In the range where the stripping member contacts the surface of the film, the length of the substrate film in the longitudinal direction is defined as the contact length, the plane passing through the center position of the contact length and perpendicular to the surface of the stripping member is defined as the vertical plane, the side of the substrate film relatively close to the stripping member is defined as the upstream side, and the side of the substrate film relatively far from the stripping member is defined as the downstream side, The contact length L[m] is 1×10 -5 m~1×10 -3 The range of m, The angle (acute angle) θ1 [°] formed between the vertical plane and the substrate film located on the upstream side of the vertical plane, the angle (acute angle) θ2 [°] formed between the vertical plane and the substrate film located on the downstream side of the vertical plane, the tension T1 [N / m] applied to the substrate film located on the upstream side of the vertical plane, and the tension T2 [N / m] applied to the substrate film located on the downstream side of the vertical plane satisfy the following formula (1), Equation (1): 1.0×10 6 ≦{T1×cos(θ1)+T2×cos(θ2)} / L≦2.4×10 8 .
3. The film stripping method according to claim 1, wherein: Of the two surfaces constituting the peeling member and sandwiching the ridgeline where the peeling member starts to contact the surface of the film, the angle formed by the surface facing the base film before contacting the ridgeline and the base film before contacting the ridgeline is set to be 5° or more.
4. The film peeling method according to any one of claims 1 to 3, wherein The coating film includes a curable silicone resin.
5. A film peeling device for peeling off a film from a base film having a film containing a water-soluble resin on at least one side thereof, comprising: A cleaning liquid imparting mechanism, used for imparting cleaning liquid to the film; a peeling member for peeling the film to which the cleaning liquid has been applied from the base film; a driving device for moving the substrate film relative to the peeling member in the longitudinal direction of the substrate film; as well as A tension imparting mechanism for imparting tension to at least one direction of the length direction of the substrate film, The cleaning liquid applying mechanism is adjusted to apply the cleaning liquid to the film at a rate of 1 m 2 The cleaning solution is applied in an amount ranging from 3 ml to 650 ml per surface area, The peeling member is arranged to contact the surface of the film to which the cleaning liquid is applied, and the angle formed by the base film through the peeling member is in the range of 20° to 150°. The tension applying mechanism is adjusted to apply a tension in the range of 10 N / m to 1000 N / m.
6. The film peeling device according to claim 5, wherein: The length of the range of the peeling member in contact with the surface of the film in the longitudinal direction of the base film is 1×10 -5 m~1×10 -3 The range of m.