Method for producing laminate, method for producing film, film, film with support, and photosensitive transfer material

By forming a hydrophobic and hydrophilic resin layer on the surface of the support body and forming a convex structure and a concave structure at its interface, the problems of insufficient functionality and high manufacturing cost in the prior art are solved, and simple and efficient manufacturing is achieved Excellent functional membrane.

CN118946453APending Publication Date: 2024-11-12FUJIFILM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280094207.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-10-17
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, when using a composition containing resin and particles to produce a water removable film, the functionality such as water removable may be insufficient, and the mold method with a concave structure and a convex structure may be used for a large number of steps and a high manufacturing cost.

Method used

A hydrophobic resin layer and a hydrophilic resin layer are formed on the surface of the support body, and a convex structure and a concave structure are formed at the interface thereof. A laminated body film with excellent functionality is produced by coating and drying of a specific composition.

Benefits of technology

The film with excellent functionality is achieved by simple method, which improves the water repellency and reflection inhibition of the film, and reduces the manufacturing cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005060094570000281
    Figure BDA0005060094570000281
  • Figure BDA0005060094570000301
    Figure BDA0005060094570000301
  • Figure HDA0005060094580000011
    Figure HDA0005060094580000011
Patent Text Reader

Abstract

The invention provides a method for manufacturing a laminate, a method for manufacturing a film, a film, a film with a support, and a photosensitive transfer material. The method for manufacturing a laminate includes: a step of forming a hydrophobic resin layer containing a hydrophobic resin on a surface of a support; a step for forming a hydrophilic resin layer containing a hydrophilic resin on the surface of the hydrophobic resin layer; and a step in which a composition containing an alcohol is applied to the surface of the hydrophilic resin layer and dried, and a convex structure is formed on the hydrophilic resin layer-side surface of the hydrophobic resin layer and a concave structure is formed on the hydrophobic resin layer-side surface of the hydrophilic resin layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a laminate, a method for producing a film, a film, a film with a support, and a photosensitive transfer material. Background Art

[0002] The water-repellent film having at least one of a fine concave structure and a convex structure on the surface is produced by various methods.

[0003] For example, there are known methods of stretching a film obtained by forming a composition containing a resin and particles, and a method of injecting a composition containing a resin into a mold having at least one of a concave structure and a convex structure and curing the composition. Summary of the invention

[0004] Technical issues to be solved by the invention

[0005] However, in the method using the composition containing a resin and particles, the functionality such as water repellency of the produced water repellent film may be insufficient.

[0006] The method using a mold having at least one of a concave structure and a convex structure has problems such as a large number of steps and high manufacturing cost.

[0007] The problem to be solved by one embodiment of the present invention is to provide a method for manufacturing a laminate and a method for manufacturing a film, which can manufacture a film that is simple and has excellent functionality. In addition, the problem to be solved by one embodiment of the present invention is to provide a film, a film with a support, and a photosensitive transfer material, which can be manufactured by a simple method and have excellent functionality.

[0008] Means for solving technical problems

[0009] The specific means for solving the problem are as follows.

[0010] <1> A method for manufacturing a laminate, comprising:

[0011] A step of forming a hydrophobic resin layer containing a hydrophobic resin on the surface of the support;

[0012] A step of forming a hydrophilic resin layer containing a hydrophilic resin on the surface of the hydrophobic resin layer; and

[0013] A step of applying a composition containing an alcohol on the surface of the hydrophilic resin layer and drying the composition to form a convex structure on the hydrophilic resin layer side surface of the hydrophobic resin layer and a concave structure on the hydrophobic resin layer side surface of the hydrophilic resin layer.

[0014] <2> According to the above <1> The method for manufacturing the laminated body, wherein:

[0015] The total light transmittance of the support is 50% or more.

[0016] <3> According to the above <1> or <2> The method for manufacturing the laminated body, wherein:

[0017] The support body contains a polyester resin.

[0018] <4> According to the above <1> to <3> The method for producing a laminate according to any one of the preceding claims, wherein:

[0019] The glass transition temperature of the hydrophobic resin is lower than the glass transition temperature of the hydrophilic resin.

[0020] <5> According to the above <1> to <4> The method for producing a laminate according to any one of the preceding claims, wherein:

[0021] The hydrophobic resin is a polyolefin resin.

[0022] <6> According to the above <1> to <5> The method for producing a laminate according to any one of the preceding claims, wherein:

[0023] The hydrophilic resin is a (meth)acrylic resin.

[0024] <7> According to the above <1> to <6> The method for producing a laminate according to any one of the preceding claims, wherein:

[0025] The above composition also contains water.

[0026] <8> A method for manufacturing a film, comprising:

[0027] Through the above <1> The method for manufacturing a laminated body and the steps for manufacturing a laminated body; and

[0028] A step of performing peeling at an interface between the hydrophobic resin layer and the hydrophilic resin layer included in the laminate.

[0029] <9> A membrane comprising a hydrophobic resin,

[0030] The film has a convex structure with a long diameter of 0.02 μm to 5 μm and an average height of 10 nm to 3000 nm on at least one surface, and

[0031] In every 10 μm 2 The above-mentioned surface is formed with 1 to 1000 of the above-mentioned convex structures.

[0032] <10> According to the above <9> The membrane, wherein

[0033] The water contact angle of the surface having the protruding structures formed thereon is 100° or more at 25°C.

[0034] <11> According to the above <9> or <10> The membrane, wherein

[0035] When the surface on which the convex structure is formed is irradiated with light having a wavelength of 550 nm, the reflectivity is 4% or less.

[0036] <12> A film with a support, comprising a support and the above-mentioned <9> to <11> The film of any one of the above

[0037] The surface of the film opposite to the surface on which the protruding structures are formed is in contact with the support.

[0038] <13> According to the above <12> The film with support, wherein

[0039] The film is disposed on both sides of the support, and

[0040] The transmittance of light with a wavelength of 550 nm is 92% or more.

[0041] <14> A membrane comprising a hydrophilic resin,

[0042] The film has a concave structure with a long diameter of 0.02 μm to 5 μm and an average depth of 10 nm to 3000 nm on at least one surface, and

[0043] In every 10 μm 2 The above-mentioned surface is formed with 1 to 1000 of the above-mentioned concave structures.

[0044] <15> According to the above <14> The membrane, wherein

[0045] At 25° C., the water contact angle of the surface having the concave structures formed thereon is 95° or more.

[0046] <16> A photosensitive transfer material comprises a support, a hydrophobic resin layer, a hydrophilic resin layer, a water-soluble intermediate layer and a photosensitive resin layer in sequence.

[0047] The hydrophobic resin layer contains a polyolefin resin.

[0048] The hydrophilic resin layer contains a (meth)acrylic resin.

[0049] The water-soluble intermediate layer contains a water-soluble resin.

[0050] The hydrophobic resin layer and the hydrophilic resin layer can be peeled off at the interface.

[0051] In the hydrophilic resin layer, 2The surface of the hydrophobic resin layer has 1 to 1000 concave structures formed thereon.

[0052] The long diameter of the concave structure is 0.02 μm to 5 μm, the average depth is 10 nm to 3000 nm, and

[0053] The static friction coefficient of the surface with respect to glass is 1.50 or less.

[0054] Effects of the Invention

[0055] According to one embodiment of the present invention, a method for manufacturing a laminate and a method for manufacturing a film can be provided, which can manufacture a film that is simple and has excellent functionality. In addition, according to one embodiment of the present invention, a film, a film with a support, and a photosensitive transfer material can be provided, which can be manufactured by a simple method and have excellent functionality. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 The SEM image (magnification: 30,000 times) of the surface on which the convex structure of the specific film A produced in Example 1-1 was formed is shown.

[0057] Figure 2 The SEM image (magnification: 30,000 times) of the surface on which the concave structure of the specific film B produced in Example 1-1 was formed is shown.

[0058] Figure 3 The SEM image (magnification: 30,000 times) of the surface on which the convex structure of the specific film A produced in Example 1-4 was formed is shown.

[0059] Figure 4 The SEM image (magnification: 30,000 times) of the surface on which the concave structure of the specific film B produced in Example 1-4 was formed is shown. DETAILED DESCRIPTION

[0060] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. The present invention is not limited to the following embodiments and can be implemented with appropriate additions and changes within the scope of the purpose of the present invention. In each of the drawings, components represented by the same element symbols refer to the same components. Sometimes, the description of components and symbols repeated in each of the drawings can be omitted. The ratio of the dimensions in the drawings does not necessarily represent the ratio of the actual dimensions.

[0061] In the present invention, the numerical range represented by "to" refers to a range including the numerical values ​​recorded before and after "to" as the lower limit and the upper limit. In the numerical range recorded in stages in the present invention, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present invention, the upper limit or lower limit recorded in a certain numerical range can be replaced by the value shown in the embodiment.

[0062] In the present invention, the term "process" includes not only independent processes but also processes that achieve the intended purpose of the process even if they cannot be clearly distinguished from other processes.

[0063] In the present invention, "(meth)acrylic acid" means both or either one of acrylic acid and methacrylic acid.

[0064] In the present invention, when there are plural substances corresponding to each component, the amount of each component in a composition or the like refers to the total amount of the plural substances present in the composition or the like unless otherwise specified.

[0065] In the present invention, a combination of two or more preferred aspects or configurations is a more preferred aspect or configuration.

[0066] In the present invention, "hydrophilic resin" refers to a resin having a polar group. Also, in the present invention, "hydrophobic resin" refers to a resin having no polar group.

[0067] Examples of the polar group include a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphoric acid group, an amide group, and an imide group. From the viewpoint of water repellency, a carboxyl group is preferred.

[0068] In the present invention, when an embodiment is described with reference to drawings, the structure of the embodiment is not limited to the structure shown in the drawings.

[0069] [Method for producing laminated body]

[0070] The method for manufacturing a laminate of the present invention includes: a process of forming a hydrophobic resin layer containing a hydrophobic resin on the surface of a support body (hereinafter referred to as the process of forming a hydrophobic resin layer); a process of forming a hydrophilic resin layer containing a hydrophilic resin on the surface of the hydrophobic resin layer (hereinafter referred to as the process of forming a hydrophilic resin layer); and a process of coating a composition containing an alcohol (hereinafter referred to as a specific composition) on the surface of the hydrophilic resin layer and drying it, thereby forming a convex structure on the hydrophilic resin layer side surface of the hydrophobic resin layer and a concave structure on the hydrophobic resin layer side surface of the hydrophilic resin layer (hereinafter referred to as the process of forming a convex structure and a concave structure).

[0071] The method for producing a laminate of the present invention may include a step of forming a photosensitive resin layer on the surface of the hydrophilic resin layer after applying and drying the specific composition.

[0072] Furthermore, as described later, when the water-soluble intermediate layer is formed using a specific composition, the method for producing a laminate of the present invention may include a step of forming a photosensitive resin layer on the surface of the water-soluble intermediate layer.

[0073] Hereinafter, the above two steps are collectively referred to as a step of forming a photosensitive resin layer.

[0074] (Step of forming a hydrophobic resin layer)

[0075] The method for producing a laminate of the present invention includes the step of forming a hydrophobic resin layer containing a hydrophobic resin on the surface of a support. The hydrophobic resin layer may contain two or more types of hydrophobic resins.

[0076] The hydrophobic resin preferably does not dissolve in water (25° C., pH 7) or methanol (25° C.) at a level of 0.1% by mass or more.

[0077] Examples of the hydrophobic resin include polyolefin resins, polystyrene resins, polyester resins, and (meth)acrylate resins.

[0078] Among the above, from the viewpoints of water repellency, reflection suppression, etc., polyolefin resins are preferred, polyethylene, polypropylene, or ethylene vinyl acetate resins are more preferred, and polyethylene is further preferred.

[0079] Examples of the polyethylene include high-density polyethylene resin (HDPE), medium-density polyethylene resin (MDPE), low-density polyethylene resin (LDPE) and linear low-density polyethylene resin (LLDPE), and LDPE or LLDPE is preferred.

[0080] In the present invention, HDPE refers to polyethylene with a density of 0.945 g / cm3 or more, and MDPE refers to polyethylene with a density of 0.925 g / cm3 or more. 3 Above and less than 0.945g / om 3 Polyethylene, LDPE and LLDPE refer to polyethylene with a density less than 0.925g / om 3 of polyethylene.

[0081] From the viewpoints of water repellency, reflection suppression, etc., the glass transition temperature (Tg) of the hydrophobic resin is preferably lower than the glass transition temperature of the hydrophilic resin contained in the hydrophilic resin layer, more preferably at least 50°C lower than the glass transition temperature of the hydrophilic resin contained in the hydrophilic resin layer, and more preferably at least 100°C lower than the glass transition temperature of the hydrophilic resin contained in the hydrophilic resin layer.

[0082] The glass transition temperature of the hydrophobic resin is preferably -150°C to 70°C, more preferably -100°C to 20°C, and further preferably -100°C to 0°C, from the viewpoints of water repellency, reflection suppression, and the like.

[0083] In the present invention, the glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), more specifically, by the "extrapolated glass transition starting temperature" described in the method for determining the glass transition temperature of JIS K 7121 (1987) "Methods for determining transition temperatures of plastics".

[0084] From the viewpoint of water repellency, reflection suppression, etc., the melt flow rate (MFR) of the hydrophobic resin is preferably 0.1 to 100 g / 10 min, more preferably 0.3 to 30 g / 10 min, further preferably 2 to 20 g / 10 min.

[0085] In the present invention, the melt mass flow rate is obtained by an extrusion plastometer (capillary rheometer), more specifically, by the method described in JIS K7210-1 "Plastics - Method for determining melt mass flow rate (MFR) and melt volume flow rate (MVR) of thermoplastics".

[0086] From the viewpoint of water repellency, reflection suppression, etc., the content of the hydrophobic resin relative to the total mass of the hydrophobic resin layer is preferably 70 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and may be 100 mass %.

[0087] The hydrophobic resin layer may contain additives such as surfactants, pigments, dyes, ultraviolet absorbers, light stabilizers, antioxidants, rust inhibitors, adhesion promoters, thermal inhibitors, and inorganic particles.

[0088] From the viewpoint of water repellency, reflection suppression, and the like, the thickness of the hydrophobic resin is preferably 1 μm to 20 μm, more preferably 3 μm to 15 μm, and even more preferably 5 μm to 10 μm.

[0089] The method for forming the hydrophobic resin layer on the support surface is not particularly limited, and examples thereof include a method of applying a hydrophobic resin composition containing the above-mentioned hydrophobic resin etc. on the support surface and drying the composition. The hydrophobic resin composition may contain an organic solvent.

[0090] The support may contain one or more resins, and examples of the resin include polyester resins, polyolefin resins, (meth)acrylic resins, polyamide resins, polyimide resins, and polyamideimide resins.

[0091] Among the above, from the viewpoint of transparency and mechanical strength, the support preferably contains a polyester resin, and more preferably contains polyethylene terephthalate.

[0092] The content of the resin relative to the total mass of the support is preferably 70% by mass or more, more preferably 80% by mass or more, further preferably 90% by mass or more, and may be 100% by mass.

[0093] The support may contain the above-mentioned additives.

[0094] From the viewpoint of reflection suppression, the total light transmittance of the support is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more.

[0095] In the present invention, the total light transmittance is measured according to the method specified in JIS K 7375 (2008).

[0096] The support is preferably a film containing the above resin, and is more preferably a biaxially stretched film from the viewpoint of mechanical strength and solvent resistance.

[0097] From the viewpoint of retaining the hydrophobic resin layer and the like, the thickness of the support is preferably 1 μm to 50 μm, more preferably 10 μm to 40 μm, and even more preferably 15 μm to 30 μm.

[0098] (Step of forming a hydrophilic resin layer)

[0099] The method for producing a laminate of the present invention includes the step of forming a hydrophilic resin layer containing a hydrophilic resin on the surface of a hydrophobic resin layer. The hydrophilic resin layer may contain two or more hydrophilic resins.

[0100] The hydrophilic resin is preferably soluble in water (25° C., pH 7) or methanol (25° C.) at a concentration of 0.1% by mass or more.

[0101] Examples of the hydrophilic resin include (meth)acrylic resins, styrene (meth)acrylic resins, epoxy resins, polyurethane resins, nylon resins, butyral resins, vinyl alcohol resins, polyvinyl pyrrolidone resins, and cellulose resins.

[0102] Among the above, (meth)acrylic resins are preferred from the viewpoint of water repellency and also preferred from the viewpoint of reducing the static friction coefficient with respect to glass.

[0103] In the case where the laminate manufactured by the manufacturing method of the present invention has a photosensitive resin layer, by reducing the static friction coefficient of the hydrophilic resin layer relative to the glass, the lubricity (hereinafter also referred to as lubricity) of the film on the hydrophilic resin layer side obtained by peeling off the interface between the hydrophobic resin layer and the hydrophilic resin layer relative to the photomask (material of the substrate: glass) can be improved, and the exposure of the photosensitive resin layer can be performed well.

[0104] The hydrophilic resin includes a structural unit having a polar group.

[0105] From the viewpoint of water repellency, lubricity, etc., the content of the structural unit having a polar group is preferably 10 to 40% by mass, more preferably 13 to 37% by mass, and further preferably 15 to 35% by mass based on the total amount of all structural units contained in the hydrophilic resin.

[0106] From the viewpoint of water repellency, lubricity, and the like, the structural unit having a polar group is preferably a structural unit corresponding to (meth)acrylic acid.

[0107] From the viewpoint of water repellency, lubricity, etc., the acid value of the hydrophilic resin is preferably 150 mgKOH / g or more, and more preferably 150 mgKOH / g to 300 mgKOH / g.

[0108] In the present invention, the acid value is measured by the method described in JIS K0070 (1992).

[0109] The glass transition temperature of the hydrophilic resin is preferably 30°C or higher, more preferably 50°C to 180°C, and even more preferably 90°C to 150°C, from the viewpoint of water repellency, lubricity, and the like.

[0110] From the viewpoint of water repellency, lubricity, etc., the weight average molecular weight of the hydrophilic resin is preferably 5,000 or more, more preferably 10,000 to 100,000, and even more preferably 20,000 to 80,000.

[0111] In the present invention, unless otherwise specified, the weight average molecular weight is a molecular weight calculated by a gel permeation chromatography (GPC) analysis apparatus using a column of TSKgel SuperHM-H (trade name manufactured by TOSHO HCORPORATION), using a solvent of PFP (pentafluorophenol) / chloroform = 1 / 2 (mass ratio), a differential refractometer, and using polystyrene as a standard substance.

[0112] From the viewpoint of water repellency, lubricity, etc., the content of the hydrophilic resin relative to the total mass of the hydrophilic resin layer is preferably 70 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and may be 100 mass %.

[0113] The hydrophilic resin layer may contain the above-mentioned additives.

[0114] From the viewpoint of water repellency, lubricity, etc., the thickness of the hydrophilic resin is preferably 0.1 μm or more, more preferably 0.5 μm to 10 μm, and further preferably 1 μm to 5 μm.

[0115] The method for forming the hydrophilic resin layer on the surface of the hydrophobic resin layer is not particularly limited, and examples thereof include a method of applying a hydrophilic resin composition containing the above-mentioned hydrophilic resin etc. on the surface of the support and drying the composition. The hydrophilic resin composition may contain an organic solvent.

[0116] (Process of forming convex structure and concave structure)

[0117] The method for producing a laminate of the present invention comprises the steps of applying a specific composition on the surface of a hydrophilic resin layer and drying the composition to form a convex structure on the hydrophilic resin layer side surface of the hydrophobic resin layer and a concave structure on the hydrophobic resin layer side surface of the hydrophilic resin layer.

[0118] The mechanism by which the convex structure is formed on the surface of the hydrophobic resin layer on the hydrophilic resin layer side and the concave structure is formed on the surface of the hydrophilic resin layer on the hydrophobic resin layer side is not yet clear, but is presumed as follows.

[0119] The specific composition applied on the surface of the hydrophilic resin layer permeates from the hydrophilic resin layer to the hydrophobic resin layer. Next, the specific composition is dried by heating to cause foaming of the specific composition.

[0120] The foaming of the specific composition is foamed from the hydrophobic resin layer based on the less plasticization of the specific composition toward the inside of the hydrophilic resin layer based on the plasticization of the specific composition, which is large and fully softened, in a manner as a bubble expansion. In this way, a concave structure is formed on the side surface of the hydrophobic resin layer of the hydrophilic resin layer. Thereafter, it can be inferred that the specific composition that becomes gas is gradually absorbed by the hydrophilic resin layer, and the position of the gas that is foamed becomes a space of a vacuum state, and the specific composition volatilizes outside the system, so that the hydrophobic resin layer is attracted to the space of the hydrophilic resin layer that is sufficiently harder than the hydrophobic resin layer, and therefore a convex structure is formed on the side surface of the hydrophilic resin layer of the hydrophobic resin layer.

[0121] Furthermore, it is presumed that when the hydrophilic resin layer and the hydrophobic resin layer are separated by peeling, the protrusions of the hydrophobic resin layer that have invaded the hydrophilic resin layer are sometimes stretched and sometimes deformed into protrusions with a high aspect ratio.

[0122] It can be inferred that the convex structure imparts excellent functionalities such as water repellency and reflection suppression to the surface of the hydrophobic resin layer, and the concave structure imparts excellent functionalities such as water repellency and lubricity to the surface of the hydrophilic resin layer. In addition, water repellency can be explained as a lotus leaf effect, and reflection suppression can be explained as a moth eye effect.

[0123] The specific composition contains alcohol. The specific composition may contain two or more alcohols. Examples of the alcohol include methanol, ethanol, propanol, butanol, and the like. Methanol is preferred from the viewpoints of water repellency, reflection suppression, lubricity, and the like.

[0124] From the viewpoint of water repellency, antireflection property, lubricity, etc., the content of the alcohol relative to the total mass of the specific composition is preferably 30 to 70 mass %, more preferably 40 to 65 mass %, and even more preferably 45 to 60 mass %.

[0125] From the viewpoint of water repellency, antireflection property, lubricity, and the like, the specific composition preferably contains water.

[0126] When the specific composition contains water, from the viewpoints of water repellency, reflection suppression, lubricity, etc., the ratio of the water content to the alcohol content (water content / alcohol content) is preferably 1 / 9 to 5 / 5, more preferably 2 / 8 to 4 / 6, and further preferably 2 / 8 to 3 / 7.

[0127] The specific composition may contain a water-soluble resin. The specific composition may contain a water-soluble resin, so that the convex structure and the concave structure can be formed, and a water-soluble intermediate layer can be formed on the surface of the hydrophilic resin layer. The specific composition may contain two or more water-soluble resins.

[0128] In the present invention, the water-soluble resin refers to a resin in which 1 g or more is dissolved in 100 g of water at pH 7.0 at 23°C.

[0129] The water-soluble resin preferably has the above-mentioned polar group.

[0130] Examples of the water-soluble resin include polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA), water-soluble polysaccharides (methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, propyl methyl cellulose, etc.), pullulan, starch (hydroxypropyl starch, carboxymethyl starch, etc.), chitosan, cyclodextrin), polyethylene oxide, polyethyloxazoline, hydroxymethyl melamine, polyacrylamide, phenolic resin, etc.

[0131] From the viewpoint of water repellency, antireflection property, lubricity, etc., the content of the water-soluble resin relative to the total mass of the specific composition is preferably 1 to 15 mass %, more preferably 2 to 13 mass %, and even more preferably 3 to 10 mass %.

[0132] The specific composition may contain a water-insoluble resin. The specific composition contains a water-insoluble resin, so that the convex structure and the concave structure can be formed, and a water-soluble intermediate layer can be formed on the surface of the hydrophilic resin layer. The specific composition may contain two or more water-soluble resins.

[0133] In the present invention, the water-insoluble resin refers to a resin of which less than 1 g is dissolved in 100 g of water at pH 7.0 at 23°C.

[0134] Examples of the water-insoluble resin include styrene particle water dispersions, methyl methacrylate water dispersions, acrylic resin water dispersions, polyolefin resin water dispersions, polyester resin water dispersions, polyurethane resin water dispersions, and epoxy resin water dispersions.

[0135] From the viewpoint of water repellency, antireflection property, lubricity, etc., the content of the water-insoluble resin relative to the total mass of the specific composition is preferably 1 to 15 mass %, more preferably 2 to 13 mass %, and even more preferably 3 to 10 mass %.

[0136] The specific composition may contain the above-mentioned additives. Furthermore, the specific composition may contain an organic solvent other than alcohol.

[0137] From the viewpoints of water repellency, antireflection property, lubricity, etc., the coating amount of the specific composition is preferably 10 mL / m 2 ~45mL / m 2 , more preferably 15 mL / m 2 ~40mL / m 2 , more preferably 20mL / m 2 ~30mL / m 2 .

[0138] When the water-soluble intermediate layer is formed from a specific composition, the thickness of the water-soluble intermediate layer is preferably 0.01 μm to 10 μm, more preferably 0.1 μm to 2 μm, from the viewpoint of water repellency, antireflection property, lubricity, and the like.

[0139] The drying temperature of the specific composition is preferably 50°C to 100°C, more preferably 60°C to 90°C, from the viewpoint of water repellency, antireflection property, lubricity, and the like.

[0140] In the present invention, the drying temperature refers to the temperature of the environment in which a specific composition is dried, rather than the temperature of the specific composition.

[0141] (Step of forming a photosensitive resin layer)

[0142] The method for producing a laminate of the present invention may include a step of forming a photosensitive resin layer on the surface of the hydrophilic resin layer after applying and drying the specific composition.

[0143] Furthermore, as described later, when the water-soluble intermediate layer is formed using a specific composition, the method for producing a laminate of the present invention may include a step of forming a photosensitive resin layer on the surface of the hydrophilic resin layer.

[0144] The photosensitive resin layer may be a negative photosensitive resin layer or a positive photosensitive resin layer.

[0145] The photosensitive resin layer may contain one or more polymers having an acid group (hereinafter, also referred to simply as polymers). Examples of the acid group include a carboxyl group, a sulfone group, a phosphoric acid group, and a phosphonic acid group. The acid group is preferably a carboxyl group.

[0146] From the viewpoint of alkali developability, the polymer is preferably an alkali-soluble resin having an acid value of 60 mgKOH / g or more, and more preferably a carboxyl group-containing acrylic resin having an acid value of 60 mgKOH / g or more.

[0147] The polymer may have a reactive group. As the reactive group, a polymerizable group is preferred. As the polymerizable group, ethylenically unsaturated groups, polycondensation groups (hydroxyl groups, carboxyl groups, etc.), polyaddition reactive groups (epoxy groups, isocyanate groups, etc.) and the like can be cited.

[0148] From the viewpoint of alkali developability, the acid value of the polymer is preferably 60 mgKOH / g to 200 mgKOH / g, more preferably 100 mgKOH / g to 200 mgKOH / g, and particularly preferably 150 mgKOH / g to 200 mgKOH / g.

[0149] The weight average molecular weight of the polymer is preferably 1,000 or more, more preferably 10,000 or more, and particularly preferably 20,000 to 100,000.

[0150] The polymer may have a structural unit derived from a non-acidic monomer. Examples of the non-acidic monomer include (meth)acrylic acid esters, ester compounds of vinyl alcohol, (meth)acrylonitrile, and aromatic vinyl compounds.

[0151] Examples of the (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and benzyl (meth)acrylate.

[0152] Examples of the ester compound of vinyl alcohol include vinyl acetate.

[0153] Examples of the aromatic vinyl compound include styrene and styrene derivatives.

[0154] The non-acidic monomer is preferably one or more monomers selected from the group consisting of methyl (meth)acrylate, n-butyl (meth)acrylate, styrene, a styrene derivative, and benzyl (meth)acrylate.

[0155] From the viewpoint of photosensitivity, the content of the polymer is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, and further preferably 30 to 70% by mass, based on the total mass of the photosensitive resin layer.

[0156] The photosensitive resin layer may contain one or more polymerizable compounds.

[0157] The polymerizable compound is not limited, and a known polymerizable compound can be used. The polymerizable compound is preferably an ethylenically unsaturated compound. The ethylenically unsaturated compound is a compound having one or more ethylenically unsaturated groups.

[0158] The ethylenically unsaturated group is preferably a (meth)acryloyl group. The ethylenically unsaturated compound is preferably a (meth)acrylate compound.

[0159] As the ethylenically unsaturated compound, an ethylenically unsaturated compound having a bisphenol structure is also preferably used.

[0160] Examples of the ethylenically unsaturated compound having a bisphenol structure include alkylene oxide-modified bisphenol A di(meth)acrylates. Examples of the alkylene oxide-modified bisphenol A di(meth)acrylates include ethylene glycol dimethacrylates to which an average of 5 mol of ethylene oxide is added to both ends of bisphenol A, ethylene glycol dimethacrylates to which an average of 2 mol of ethylene oxide is added to both ends of bisphenol A, ethylene glycol dimethacrylates to which an average of 5 mol of ethylene oxide is added to both ends of bisphenol A, alkylene glycol dimethacrylates to which an average of 6 mol of ethylene oxide and an average of 2 mol of propylene oxide are added to both ends of bisphenol A, and alkylene glycol dimethacrylates to which an average of 15 mol of ethylene oxide and an average of 2 mol of propylene oxide are added to both ends of bisphenol A.

[0161] Specific examples of the alkylene oxide-modified bisphenol A di(meth)acrylate include 2,2-bis(4-(methacryloyloxydiethoxy)phenyl)propane and 2,2-bis(4-(methacryloyloxyethoxypropoxy)phenyl)propane.

[0162] The molecular weight of the polymerizable compound is preferably 200 to 3,000, more preferably 280 to 2,200, and particularly preferably 300 to 2,200. When the polymerizable compound is a compound having a molecular weight distribution (e.g., a polymer), the weight average molecular weight of the polymerizable compound is preferably 200 to 3,000, more preferably 280 to 2,200, and particularly preferably 300 to 2,200.

[0163] The content of the polymerizable compound is preferably 10 to 70% by mass, more preferably 20 to 60% by mass, and particularly preferably 20 to 50% by mass, based on the total mass of the photosensitive resin layer.

[0164] The photosensitive resin layer may contain a polymerization initiator. As the polymerization initiator, a conventionally known photoradical polymerization initiator may be used.

[0165] The content of the polymerization initiator with respect to the total mass of the photosensitive resin layer is not particularly limited, but can be 0.01% by mass to 1% by mass.

[0166] The photosensitive resin layer may contain the above-mentioned additives.

[0167] The thickness of the photosensitive resin layer is not particularly limited, and can be 0.5 μm to 5 μm.

[0168] The method for forming the photosensitive resin layer is not particularly limited, and examples thereof include a method in which a photosensitive resin layer-forming composition containing the above-mentioned photosensitive resin is applied to the surface of the hydrophilic resin layer or the surface of the water-soluble intermediate layer and then dried.

[0169] The composition for forming a photosensitive resin layer may contain an organic solvent.

[0170] From the viewpoint of water repellency, antireflection property, lubricity and the like, the content of alcohol relative to the total mass of the photosensitive resin layer-forming composition is preferably 50% by mass or less, more preferably 10% by mass or less.

[0171] From the viewpoint of water repellency, antireflection property, lubricity and the like, the water content relative to the total mass of the photosensitive resin layer-forming composition is preferably 5 mass % or less, more preferably 1 mass % or less, and particularly preferably no water is contained.

[0172] [Method for producing film]

[0173] The method for producing a film of the present invention comprises: a step of producing a laminate by the above-mentioned method for producing a laminate (hereinafter referred to as a step of producing a laminate); and a step of peeling off the interface between a hydrophobic resin layer and a hydrophilic resin layer of the laminate (hereinafter referred to as a peeling off step).

[0174] According to the above-mentioned film manufacturing method, a film composed of a hydrophobic resin layer on the surface of a support body and having a convex structure on the surface (hereinafter referred to as specific film A), and a film composed of a hydrophilic resin layer and having a concave structure on the surface (hereinafter referred to as specific film B) can be manufactured.

[0175] In addition, description of the process of manufacturing the laminated body is omitted.

[0176] [Peeling process]

[0177] The method for producing a film of the present invention includes a step of performing peeling at the interface between a hydrophobic resin layer and a hydrophilic resin layer included in a laminate.

[0178] The peeling method is not particularly limited, and the peeling may be performed manually or by using a peeling device.

[0179] From the viewpoint of peeling without destroying the convex structure formed on the specific film A and the concave structure formed on the specific film B, the peeling force of the hydrophobic resin layer and the hydrophilic resin layer is preferably 0.5 g / cm to 50 g / cm, more preferably 0.5 g / cm to 10 g / cm.

[0180] In the present invention, the peeling force is measured by a tester when the hydrophobic resin layer is peeled off from the hydrophilic resin layer in a 180° direction at a speed of 300 mm / min in an environment of 25°C.

[0181] From the viewpoint of water repellency, reflection suppression, etc., the major diameter of the protruding structures on the surface of the specific film A is preferably 0.02 μm to 5 μm, more preferably 0.02 μm to 1 μm, and even more preferably 0.02 μm to 0.4 μm.

[0182] In the present invention, the major diameter of the convex structure is determined as follows.

[0183] First, a SEM image of the surface of the film on which the convex structures are formed is acquired by a scanning electron microscope (SEM).

[0184] On the convex structure in the SEM image, the distance between the two points with the largest distance was measured and the distance was taken as the major axis of the convex structure.

[0185] From the viewpoint of water repellency, reflection suppression, and the like, the average height of the protruding structures on the surface of the specific film A is preferably 10 nm to 3000 nm, more preferably 30 nm to 1000 nm, and even more preferably 100 nm to 500 nm.

[0186] In the present invention, the average height of the convex structures is determined in the following manner.

[0187] First, a test piece of the film was prepared using an ultramicrotome, and a SEM image of the cross section was obtained using a scanning electron microscope.

[0188] Three convex structures in the SEM images were randomly selected, and the maximum height difference was measured as the height. The average of the height differences was calculated as the average height of the convex structures.

[0189] From the viewpoint of water repellency, reflection suppression, etc., it is preferred that the surface of the specific film A has a 2 The surface of the film has 1 to 1000 convex structures, more preferably 10 to 900 convex structures, and further preferably 30 to 850 convex structures.

[0190] In the present invention, the number of convex structures is measured from a SEM image of the surface of the film on which the convex structures are formed.

[0191] From the viewpoint of water repellency, the water contact angle of the surface on which the protruding structures of the specific film A are formed at 25° C. is preferably 100° or more, more preferably 105° or more, and even more preferably 110° or more.

[0192] In the present invention, the water contact angle is measured in accordance with the sessile drop method of JIS R 3257 (1999).

[0193] From the viewpoint of reflection suppression, the reflectance when the surface of the specific film A having the convex structure formed thereon is irradiated with light having a wavelength of 550 nm is preferably 4% or less, and more preferably 3% or less.

[0194] In addition, the incident angle of light is set to 0°.

[0195] From the viewpoint of water repellency, lubricity, etc., the major diameter of the concave structures in the specific film B is preferably 0.02 μm to 5 μm, more preferably 0.02 μm to 1 μm, and even more preferably 0.02 μm to 0.4 μm.

[0196] In the present invention, the major diameter of the concave structure is determined in the following manner.

[0197] First, a scanning electron microscope (SEM) image of the surface of the film on which the concave structure is formed is obtained.

[0198] On the concave structure of the SEM image, the distance between the two points with the largest distance was measured and taken as the major axis of the convex structure.

[0199] From the viewpoint of water repellency, lubricity, etc., the average depth of the concave structures in the specific film B is preferably 10 nm to 3000 nm, more preferably 30 nm to 1000 nm, and further preferably 100 nm to 500 nm.

[0200] In the present invention, the average depth of the concave structures is determined in the following manner.

[0201] First, a test piece of the film was prepared using an ultramicrotome, and a SEM image of the cross section was obtained using a scanning electron microscope.

[0202] The concave structures of three SEM images were randomly selected, the maximum height difference was measured as the depth, and the average was calculated as the average depth of the concave structures.

[0203] From the viewpoint of water repellency, lubricity, etc., it is preferred that the surface of the specific film B has a 2 The surface of the film has 1 to 1000 concave structures, more preferably 10 to 900 concave structures, and even more preferably 30 to 850 concave structures.

[0204] In the present invention, the number of concave structures is measured from a SEM image of the surface of the film on which the concave structures are formed.

[0205] From the viewpoint of water repellency, the water contact angle of the surface having the concave structure formed in the specific film B at 25° C. is preferably 95° or more, more preferably 105° or more, and further preferably 110° or more.

[0206] From the viewpoint of lubricity, the static friction coefficient of the surface with the concave structure formed on the specific film B with respect to glass is preferably 1.50 or less, more preferably 1.00 or less, and further preferably 0.85 or less. The lower limit of the static friction coefficient is not particularly limited, and can be 0.1 or more.

[0207] In the present invention, the static friction coefficient is measured in accordance with JIS K 7125 (1999) under an environment of 25° C. and a relative humidity of 50%.

[0208] [Film with convex structure]

[0209] The film of the present invention contains a hydrophobic resin and has a convex structure with a long diameter of 0.02 μm to 5 μm and an average height of 10 nm to 3000 nm on at least one surface, and a convex structure with a long diameter of 0.02 μm to 5 μm and an average height of 10 nm to 3000 nm per 10 μm. 2 The surface is formed with 1 to 1000 convex structures.

[0210] As for the hydrophobic resin, since it is mentioned above, description is omitted here.

[0211] From the viewpoint of water repellency, reflection suppression, etc., the content of the hydrophobic resin relative to the total mass of the film is preferably 70 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and may be 100 mass %.

[0212] The film may contain a surfactant, the above-mentioned additives.

[0213] From the viewpoint of water repellency, reflection suppression, etc., the major diameter of the protruding structure is preferably 0.02 to 5 μm, more preferably 0.02 to 1 μm, and even more preferably 0.02 to 0.4 μm. The major diameter of the protruding structure is measured by the same method as described above.

[0214] The average height of the convex structures is preferably 30 nm to 1000 nm, more preferably 100 nm to 500 nm, from the viewpoint of water repellency, reflection suppression, etc. The average height of the convex structures is measured by the same method as above.

[0215] From the viewpoint of water repellency, reflection suppression, etc., it is preferable that the convex structure has a width of 10 μm. 2 10 to 900, more preferably 30 to 850, are formed on the surface of the coating.

[0216] From the viewpoint of water repellency, the water contact angle of the surface of the film having the convex structures is preferably 100° or more, more preferably 105° or more, and further preferably 110° or more at 25° C. The number of convex structures is measured by the same method as described above.

[0217] From the viewpoint of reflection suppression, the reflectance when the surface of the film having the convex structure formed thereon is irradiated with light having a wavelength of 550 nm is preferably 4% or less, and more preferably 3% or less.

[0218] In addition, the incident angle of light is set to 0°.

[0219] From the viewpoint of water repellency, reflection suppression, and the like, the thickness of the film is preferably 1 μm to 20 μm, more preferably 3 μm to 15 μm, and even more preferably 5 μm to 10 μm.

[0220] Examples of uses of the film of the present invention include water-repellent films, antifouling films, high-transparency films, and antireflection films.

[0221] The film of the present invention can be produced by the above-mentioned film production method.

[0222] [Film with support]

[0223] The film with a support of the present invention comprises a support and a film having the above-mentioned convex structure provided on one surface of the support.

[0224] The surface of the film having the protruding structures opposite to the surface on which the protruding structures are formed is in contact with the support.

[0225] The film having the convex structure and the support body are as described above, and therefore description thereof is omitted here.

[0226] From the viewpoint of film transparency, in the support-attached film of the present invention, it is preferred that films having a convex structure are provided on both surfaces of the support and that the transmittance of light at a wavelength of 550 nm is 92% or more.

[0227] When the convex structure is only on one side, the transparency improvement effect of the anti-reflection film is only half obtained, and the transmittance improvement effect is halved due to reflection from the non-anti-reflection surface without the convex structure. Therefore, it is preferred that the film with the convex structure is arranged on both sides of the support body.

[0228] The light transmittance is more preferably 94% or more.

[0229] In addition, the incident angle of light is set to 0°.

[0230] Examples of uses of the support-attached film of the present invention include water-repellent films, antifouling films, high-transparency films, and antireflection films.

[0231] [Film with concave structure]

[0232] The film of the present invention contains a hydrophilic resin and has a concave structure with a long diameter of 0.02 μm to 5 μm and an average depth of 10 nm to 3000 nm on at least one surface, and a concave structure with a long diameter of 0.02 μm to 5 μm and an average depth of 10 nm to 3000 nm every 10 μm. 2 The surface is formed with 1 to 1000 concave structures.

[0233] As for the hydrophilic resin, since it is mentioned above, description is omitted here.

[0234] From the viewpoint of water repellency, lubricity, etc., the content of the hydrophilic resin relative to the total mass of the film is preferably 70 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and may be 100 mass %.

[0235] The film may contain the above-mentioned additives.

[0236] From the viewpoint of water repellency, lubricity, etc., the major diameter of the concave structure is preferably 0.02 μm to 5 μm, more preferably 0.02 μm to 1 μm, and even more preferably 0.02 μm to 0.4 μm.

[0237] The measurement of the major diameter of the concave structure is performed by the same method as described above.

[0238] From the viewpoint of water repellency, lubricity, and the like, the average depth of the concave structures is preferably 30 nm to 1000 nm, and more preferably 100 nm to 500 nm.

[0239] The average depth of the concave structures was measured by the same method as above.

[0240] From the viewpoint of water repellency, lubricity, etc., it is preferred that the concave structure has a width of 10 μm. 2 10 to 900, more preferably 30 to 850, are formed on the surface of the coating.

[0241] The number of concave structures was measured by the same method as above.

[0242] From the viewpoint of water repellency, the water contact angle of the surface of the film having the concave structure formed thereon at 25° C. is preferably 95° or more, more preferably 105° or more, and even more preferably 110° or more.

[0243] The water contact angle was measured by the same method as above.

[0244] From the viewpoint of lubricity, the static friction coefficient of the surface of the film of the present invention having the concave structures formed thereon to glass is preferably 1.50 or less, more preferably 1.00 or less, and still more preferably 0.85 or less. The lower limit of the static friction coefficient is not particularly limited and can be 0.1 or more.

[0245] The static friction coefficient was measured by the same method as above.

[0246] Examples of uses of the film of the present invention include water-repellent films, antifouling films, slippery films, and surface films of photosensitive transfer materials.

[0247] The film of the present invention can be produced by the above-mentioned film production method.

[0248] [Photosensitive transfer material]

[0249] The photosensitive transfer material of the present invention comprises a support, a hydrophobic resin layer, a hydrophilic resin layer, a water-soluble intermediate layer and a photosensitive resin layer in this order.

[0250] The hydrophobic resin layer contains a polyolefin resin,

[0251] The hydrophilic resin layer contains a (meth)acrylic resin.

[0252] The water-soluble intermediate layer contains a water-soluble resin.

[0253] The interface between the hydrophobic resin layer and the hydrophilic resin layer can be peeled off.

[0254] In the hydrophilic resin layer, every 10 μm 2 The surface of the hydrophobic resin layer has 1 to 1000 concave structures formed thereon.

[0255] The long diameter of the concave structure is 0.02 μm to 5 μm, the average depth is 10 nm to 3000 nm, and

[0256] The static friction coefficient of the surface with respect to glass is 1.50 or less.

[0257] The support, the hydrophobic resin layer, the hydrophilic resin layer, the water-soluble intermediate layer, and the photosensitive resin layer included in the photosensitive transfer material of the present invention are already described above, and the description thereof is omitted here.

[0258] Furthermore, the preferred numerical ranges for the number, major axis, and average depth of the concave structures of the hydrophilic resin layer are as described above, and are therefore omitted here.

[0259] Furthermore, the preferred numerical range of the static friction coefficient of the surface of the hydrophilic resin layer on which the concave structures are formed with respect to glass is also as described above, and description thereof is omitted here.

[0260] The hydrophobic resin layer may have a convex structure formed on the surface on the hydrophilic resin layer side.

[0261] The preferred numerical ranges for the number, major axis, and average depth of the convex structures are also as described above, and are omitted here.

[0262] The preferred numerical ranges of the water contact angle of the surface of the hydrophobic resin layer on which the protruding structures are formed and the reflectance when irradiated with light of a wavelength of 550 nm are as described above, and description thereof is omitted here.

[0263] The photosensitive transfer material of the present invention can be peeled off at the interface between the hydrophobic resin layer and the hydrophilic resin layer, thereby enabling the transfer layer including the hydrophilic resin layer, the water-soluble intermediate layer and the photosensitive resin layer in sequence to be transferred to the surface of the transfer target.

[0264] The preferred numerical ranges of the peeling force of the hydrophobic resin layer and the hydrophilic resin layer are also as described above, and the description thereof is omitted here.

[0265] The film of the present invention can be produced by the above-mentioned method for producing a laminate.

[0266] Example

[0267] Hereinafter, the above-mentioned embodiment will be described in more detail by way of examples, but the above-mentioned embodiment is not limited to these examples.

[0268] <Example 1-1>

[0269] As a support, a polyethylene terephthalate (PET) film (total light transmittance: 91%, biaxially stretched film) having a thickness of 25 μm was prepared.

[0270] On one surface of the support, a hydrophobic resin composition having the following composition was melt-extruded to form a hydrophobic resin layer having a thickness of 5 μm.

[0271] -Hydrophobic resin composition-

[0272] Polyethylene A (LLDPE, Tg-70°C or less, MFR 8 g / 10 min to 10 g / 10 min, manufactured by Prime Polymer Co., Ltd., Evolue (registered trademark) SP1071C) 100 parts by mass

[0273] A hydrophilic resin composition having the following composition was applied to the surface of the hydrophobic resin layer and then dried in an oven at 80° for 1 minute to form a hydrophilic resin layer having a thickness of 2.4 μm.

[0274] The (meth)acrylic resin A is a 1:1 mixed solution (solid content concentration: 30.0 mass%) of a copolymer of styrene, methacrylic acid and methyl methacrylate (content of each monomer: 52 mass% / 29 mass% / 19 mass%, Mw: 70,000, Tg 130°C, acid value 189 mgKOH / g), propylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether.

[0275] -Hydrophilic resin composition A-1-

[0276] (Meth) acrylic resin A-1 59.4 parts by mass

[0277] · Surfactant (DIC Corporation, MEGAFACE (registered trademark) F552) 0.03 parts by mass · Propylene glycol monomethyl ether acetate 10.6 parts by mass

[0278] ·Methyl ethyl ketone 94.2 parts by mass

[0279] Propylene glycol monomethyl ether 15.7 parts by mass

[0280] The specific composition of the following composition was applied to the surface of the hydrophilic resin layer and dried in an oven at 80° for 1 minute to form a water-soluble intermediate layer with a thickness of 1.0 μm, thereby obtaining a specific laminate. The coating amount was set to 27 mL / m 2 .

[0281] -Specific Composition-

[0282] Methanol 57.0 parts by mass

[0283] · Water 38.0 parts by mass

[0284] Polyvinyl alcohol A (PVA, manufactured by Mitsubishi Chemical Corporation, GOHSENX (registered trademark) CSK-50) 1.67 parts by mass

[0285] Polyvinyl alcohol B (PVA, manufactured by JAPAN VAM & POVAL CO., LTD., JMR-3H) 1.67 parts by mass

[0286] Polyvinyl pyrrolidone (PVP, manufactured by Ashland, PVP-K30) 1.67 parts by mass

[0287] Surfactant (DIC Corporation, MEGAFACE (registered trademark) F444) 0.005 parts by mass

[0288] After the specific composition was applied and dried, a photosensitive resin layer-forming composition having the following composition was applied on the surface of the water-soluble intermediate layer and dried in an oven at 80° for 1 minute to form a photosensitive resin layer having a thickness of 2.2 μm.

[0289] -Photosensitive resin layer forming composition B-1-

[0290] · Polymerizable compound (ARONIX (registered trademark) M270 manufactured by TOAGOSEI CO., LTD.) 0.92 parts by mass

[0291] · Polymerizable compound (2,2-bis[4-(methacryloyloxypentaethoxy)phenyl]propane, manufactured by SHIN-NAKAMURA CHEMICAL CO, LTD., BPE500) 8.78 parts by mass

[0292] Acid group-containing polymer: (meth)acrylic resin A 39.43 parts by mass

[0293] · Photoradical polymerization initiator (4,4'-bis(diethylamino)benzophenone, manufactured by Tokyo Chemical Industry Co., Ltd., EAB-F) 0.070 parts by mass

[0294] Photopolymerization initiator ("B-CIM": 2-(2-chlorophenyl)-4,5-diphenylimidazole dimer (manufactured by Hampford Research)) 1.61 parts by mass

[0295] Chain transfer agent (N-phenylcarbamoylmethyl-N-carboxymethylaniline (manufactured by FUJIFILM Wako Pure Chemical Corporation)) 0.032 parts by mass

[0296] ·Polymerization inhibitor ("1-phenyl-3-pyrazolidone": manufactured by FUJIFILM Wako Pure Chemical Corporation, 1% by mass MEK solution) 0.24 parts by mass

[0297] ·Polymerization inhibitor ("phenothiazine": manufactured by FUJIFILM Wako Pure Chemical Corporation) 0.063 parts by mass

[0298] Rust inhibitor (carboxybenzotriazole, manufactured by JOHOKU CHEMICAL CO., LTD., CBT-1) 0.023 parts by mass

[0299] Surfactant (DIC Corporation, F-552) 0.25 parts by mass

[0300] 82.5 parts by mass of methyl ethyl ketone

[0301] 1-Methoxy-2-propyl acetate 37.9 parts by mass

[0302] ·Methanol 4.7 parts by mass

[0303] Propylene glycol monomethyl ether (MFG, manufactured by Wako Pure Chemical Industries, Ltd.) 3.5 parts by mass

[0304] The photosensitive resin layer of the specific laminate was laminated on the copper foil side surface of a polyethylene terephthalate film with copper foil (hereinafter referred to as a copper-coated PET film). The lamination conditions were a roll temperature of 100° C. and a lamination speed of 4 m / min.

[0305] After laminating on the copper-bearing PET film, peeling is performed at the interface between the hydrophilic resin layer and the hydrophobic resin layer of the specific stack to obtain a specific film A (hydrophobic resin layer) having a convex structure formed on the surface of the support body and a specific film B (hydrophilic resin layer) having a concave portion formed on the surface of the copper-bearing PET film.

[0306] A SEM image of the surface of the specific film A on which the protruding structure was formed was acquired using a scanning electron microscope (manufactured by Hitachi High-Tech Corporation, S-4800, magnification 30,000 times). Figure 1 The SEM image is shown in .

[0307] The results of measuring the major diameter of the protrusion structure from the SEM image showed that the major diameter ranged from 0.18 μm to 0.53 μm, and it was confirmed that the major diameter of the protrusion structure increased with each 10 μm increase. 2 There are 122 convex structures formed on the surface.

[0308] A test piece of the specific film A was prepared using an ultramicrotome, and an SEM image of the cross section was obtained using the scanning electron microscope. The average height of the convex structures was measured and found to be 62 nm.

[0309] The long diameter of the concave structures on the surface of the specific film B on which the concave structures were formed was measured in the same manner as the convex structures, and the result was that it was in the range of 0.12 μm to 0.74 μm. 2 There are 72 concave structures formed on the surface. Figure 2 The SEM image is shown in .

[0310] A SEM image of the cross section of the specific film B was obtained in the same manner as the specific film A, and the average depth of the concave structures was measured to be 72 nm.

[0311] <Example 1-2>

[0312] A specific laminate, a specific film A, and a specific film B were produced in the same manner as in Example 1-1 except that the thickness of the hydrophilic resin layer was changed to 1.6 μm.

[0313] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1 and the result was that it was in the range of 0.08 μm to 0.18 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was 0.08 μm to 0.18 μm. 2 There are 837 convex structures formed on the surface.

[0314] The average height of the protruding structures was measured in the same manner as in Example 1-1 and was found to be 31 nm.

[0315] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1 and the result was that it was in the range of 0.04 μm to 0.14 μm, and it was confirmed that the long diameter of the concave structure of the specific film B was 0.04 μm to 0.14 μm. 2There are 826 concave structures formed on the surface.

[0316] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 45 nm.

[0317] <Examples 1-3>

[0318] A specific laminate, a specific film A, and a specific film B were produced in the same manner as in Example 1-2 except that the ratio of the water content to the methanol content (water content / methanol content) in the specific composition was changed to 3 / 7.

[0319] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.13 μm to 0.26 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was in the range of 0.13 μm to 0.26 μm. 2 There are 566 convex structures formed on the surface.

[0320] The average height of the protruding structures was measured in the same manner as in Example 1-1 and found to be 54 nm.

[0321] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1 and the result was that it was in the range of 0.06 μm to 0.19 μm, and it was confirmed that the long diameter of the concave structure of the specific film B was 0.06 μm to 0.19 μm. 2 The surface is formed with 525 concave structures.

[0322] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 56 nm.

[0323] <Examples 1-4>

[0324] A specific laminate, a specific film A, and a specific film B were produced in the same manner as in Example 1-2 except that the ratio of the water content to the methanol content (water content / methanol content) in the specific composition was changed to 2 / 8.

[0325] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.08 μm to 0.24 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was in the range of 0.08 μm to 0.24 μm. 2 There are 269 convex structures formed on the surface. Figure 3 The SEM image is shown in .

[0326] The average height of the protruding structures was measured in the same manner as in Example 1-1 and found to be 355 nm.

[0327] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.08 μm to 0.29 μm, and it was confirmed that the concave structure of the specific film B was 0.08 μm to 0.29 μm. 2 The surface is formed with 400 concave structures. Figure 4The SEM image is shown in .

[0328] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 126 nm.

[0329] <Examples 1-5>

[0330] A specific laminate, a specific film A, and a specific film B were produced in the same manner as in Example 1-2 except that the hydrophobic resin composition was changed to the following composition and the thickness of the hydrophobic resin layer was changed to 10 μm.

[0331] -Hydrophobic resin composition-

[0332] Polyethylene B (LDPE, Tg-70°C or less, MFR 8 g / 10 min to 10 g / 10 min, manufactured by TOSOH CORPORATION, Petrosen DLZ19A) 100 parts by mass

[0333] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.16 μm to 0.82 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was in the range of 0.16 μm to 0.82 μm. 2 There are 115 convex structures formed on the surface.

[0334] The average height of the protruding structures was measured in the same manner as in Example 1-1 and was found to be 65 nm.

[0335] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1 and the result was that it was in the range of 0.21 μm to 0.80 μm, and it was confirmed that the long diameter of the concave structure of the specific film B was 0.21 μm to 0.80 μm. 2 There are 49 concave structures formed on the surface.

[0336] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 163 nm.

[0337] <Examples 1-6>

[0338] A specific laminate, a specific film A, and a specific film B were produced in the same manner as in Example 1-2 except that the hydrophobic resin composition was changed to the following composition.

[0339] -Hydrophobic resin composition-

[0340] 100 parts by mass of ethylene vinyl acetate resin (Tg -30°C to -25°C, MFR 8 g / 10 min to 10 g / 10 min, EVA, manufactured by DOW-MITSUIPOLYCHEMICALS CO., LTD., EVAFLEX (registered trademark) P1007)

[0341] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.49 μm to 1.27 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was in the range of 0.49 μm to 1.27 μm. 2 There are 18 convex structures formed on the surface.

[0342] The average height of the protruding structures was measured in the same manner as in Example 1-1 and found to be 128 nm.

[0343] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.46 μm to 1.22 μm, and it was confirmed that the concave structure of the specific film B was 0.46 μm to 1.22 μm. 2 There are 23 concave structures formed on the surface.

[0344] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 189 nm.

[0345] <Examples 1-7>

[0346] Except having changed the (meth)acrylic resin A in the hydrophilic resin composition into the (meth)acrylic resin B, it carried out similarly to Example 1-5, and produced the specific laminated body, the specific film A, and the specific film B.

[0347] The (meth)acrylic resin B is a propylene glycol monomethyl ether solution (solid content concentration: 30.0 mass%) of a copolymer of styrene and acrylic acid (content of each monomer: 71 mass % / 29 mass %, Mw: 8000, Tg 102° C., acid value 225 mgKOH / g).

[0348] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.53 μm to 1.25 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was in the range of 0.53 μm to 1.25 μm. 2 There are 1.8 convex structures formed on the surface.

[0349] The average height of the protruding structures was measured in the same manner as in Example 1-1 and found to be 469 nm.

[0350] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.26 μm to 1.38 μm, and it was confirmed that the concave structure of the specific film B was 0.26 μm to 1.38 μm. 2 There are 1.9 concave structures formed on the surface.

[0351] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 688 nm.

[0352] <Example 1-8>

[0353] A specific laminate, a specific film A, and a specific film B were produced in the same manner as in Example 1-5 except that the (meth)acrylic resin A in the hydrophilic resin composition was changed to the (meth)acrylic resin C.

[0354] The (meth)acrylic resin C is a propylene glycol monomethyl ether solution (solid content concentration: 30.0 mass%) of a copolymer of styrene and acrylic acid (content of each monomer: 71 mass % / 29 mass %, Mw: 13000, Tg 102° C., acid value 225 mgKOH / g).

[0355] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1 and the result was that it was in the range of 0.26 μm to 0.30 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was 0.26 μm to 0.30 μm. 2 There are 44 convex structures formed on the surface.

[0356] The average height of the protruding structures was measured in the same manner as in Example 1-1 and found to be 198 nm.

[0357] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1 and the result was that it was in the range of 0.32 μm to 0.85 μm, and it was confirmed that the long diameter of the concave structure of the specific film B was 0.32 μm to 0.85 μm. 2 There are 45 concave structures formed on the surface.

[0358] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 251 nm.

[0359] <Example 1-9>

[0360] A specific laminate, specific film A, and specific film B were produced in the same manner as in Example 1-5 except that the thickness of the hydrophilic resin layer was changed to 2.4 μm, the copper-attached PET film was changed to a tape (polyester tape No. 31B manufactured by NITTO DENKO CORPORATION), and no photosensitive resin layer was formed.

[0361] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.42 μm to 1.72 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was in the range of 0.42 μm to 1.72 μm. 2 There are 15 convex structures formed on the surface.

[0362] The average height of the protruding structures was measured in the same manner as in Example 1-1 and found to be 106 nm.

[0363] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.44 μm to 1.15 μm, and it was confirmed that the concave structure of the specific film B was 0.44 μm to 1.15 μm. 2 There are 16 concave structures formed on the surface.

[0364] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 133 μm.

[0365] <Example 1-10>

[0366] A specific laminate, a specific film A, and a specific film B were produced in the same manner as in Example 1-5, except that the thickness of the hydrophilic resin layer was changed to 2.4 μm, the specific composition was changed to the following composition, and no photosensitive resin layer was formed. In addition, since the specific composition contained only water and methanol, no water-soluble intermediate layer was formed.

[0367] -Specific Composition-

[0368] Methanol 60.0 parts by mass

[0369] · Water 40.0 parts by weight

[0370] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.37 μm to 1.12 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was in the range of 0.37 μm to 1.12 μm. 2 There are 28 convex structures formed on the surface.

[0371] The average height of the protruding structures was measured in the same manner as in Example 1-1 and found to be 168 nm.

[0372] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.14 μm to 1.12 μm, and it was confirmed that the concave structure of the specific film B was 0.14 μm to 1.12 μm. 2 There are 26 concave structures formed on the surface.

[0373] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 226 nm.

[0374] <Example 1-11>

[0375] A specific laminate, a specific film A, and a specific film B were produced in the same manner as in Example 1-10 except that the specific composition was changed to the following composition. In addition, since the specific composition contained only methanol, a water-soluble intermediate layer was not formed.

[0376] -Specific Composition-

[0377] Methanol 100.0 parts by mass

[0378] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 2.51 μm to 4.11 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was in the range of 2.51 μm to 4.11 μm. 2 There are 1.4 convex structures formed on the surface.

[0379] The average height of the protruding structures was measured in the same manner as in Example 1-1 and found to be 20 nm.

[0380] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 2.01 μm to 4.19 μm, and it was confirmed that the concave structure of the specific film B was 2.01 μm to 4.19 μm. 2 There are 1.9 concave structures formed on the surface.

[0381] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 2035 nm.

[0382] <Comparative Example 1-1>

[0383] In the same manner as in Example 1-1, a hydrophobic resin layer having a thickness of 5 μm was formed on one surface of the PET film.

[0384] The surface of the hydrophobic resin layer was observed in the same manner as in Example 1-1, but no convex structure or concave structure was formed.

[0385] <Comparative Example 1-2>

[0386] A laminated body was produced in the same manner as in Example 1-1 except that the hydrophobic resin layer was not formed.

[0387] The photosensitive resin layer of the laminate was laminated on the copper foil side of the copper-attached PET film. The lamination conditions were a roll temperature of 100° C. and a lamination speed of 4 m / min.

[0388] After lamination on the copper-attached PET film, at the interface between the hydrophilic resin layer of the specific laminate and the support, the support and the film (hydrophilic resin layer) formed on the surface of the copper-attached PET film are peeled off.

[0389] The surface of the film was observed in the same manner as in Example 1-1, but no convex structure or concave structure was formed.

[0390] <Comparative Examples 1-3>

[0391] A laminate, a film A, and a film B were produced in the same manner as in Example 1-5 except that the specific composition was not used.

[0392] The surfaces of the films A and B were observed in the same manner as in Example 1-1, but no convex structure or concave structure was formed.

[0393] 《Water repellency evaluation》

[0394] The water contact angle of the surface on which the protruding structures of the specific film A obtained in the above example were formed was measured at 25° C. according to the sessile drop method of JIS R 3257 (1999), and the results are summarized in Table 1.

[0395] Likewise, the water contact angle of the surface having the concave structure formed thereon of the specific film B obtained in the above-mentioned example was measured and summarized in Table 1.

[0396] For Comparative Example 1-1, the water contact angle of the surface of the hydrophobic resin layer was measured and the results are shown in Table 1.

[0397] For Comparative Example 1-2, the water contact angle of the surface of the film was measured and the results are shown in Table 1.

[0398] For Comparative Examples 1-3, the water contact angles on the surfaces of Film A and Film B were measured and the results are shown in Table 1.

[0399] In this evaluation, a water contact angle of 95° or more was considered to be good in water repellency.

[0400] 《Measurement of reflectivity》

[0401] The reflectance when the surface of the specific film A obtained in Example 1-4 having the convex structure formed thereon was irradiated with light of a wavelength of 550 nm at an incident angle of 0° was measured by a spectrophotometer V-570 manufactured by JASCO Corporation, and is recorded in Table 1. At this time, a black PET film with an adhesive layer for antireflection (trade name "KUKKIRI MIERU" manufactured by TOMOEGAWA CO., LTD.) was attached to the surface of the PET support body on the opposite side to the surface of the specific film A having the convex structure formed thereon, and the measurement was performed.

[0402] The reflectance of the surface of the hydrophobic resin layer of Comparative Example 1-1 was measured in the same manner as above and the reflectance is shown in Table 1.

[0403] 《Determination of static friction coefficient》

[0404] The static friction coefficient of the surface having the concave structure of the specific film B obtained in Examples 1-1 to 1-8 with respect to a glass substrate (Aoita (soda) glass 200 mm×200 mm×5 mm thickness) was measured at 25°C and a relative humidity of 50% according to JIS K 7125 (1999) and is shown in Table 1.

[0405] Regarding Comparative Example 1-2, the static friction coefficient of the film was measured and the results are shown in Table 1.

[0406] Regarding Comparative Example 1-3, the static friction coefficient of Film B was measured and the results are shown in Table 1.

[0407]

[0408] (Example 2-1)

[0409] As a support, a polyethylene terephthalate (PET) film having a thickness of 25 μm was prepared.

[0410] The hydrophobic resin composition used in Example 1-1 was melt-extruded on both surfaces of the support to form a hydrophobic resin layer having a thickness of 5 μm.

[0411] Thereafter, 16 μm polyethylene terephthalate (PET) films were bonded to both surfaces of the surface of the hydrophobic resin layer as protective films.

[0412] The protective film on one side was peeled off, and the hydrophilic resin composition used in Example 1-1 was applied to the surface of the exposed hydrophobic resin layer, followed by drying in an oven at 80° for 1 minute to form a hydrophilic resin layer having a thickness of 1.6 μm.

[0413] The specific composition used in Example 1-4 was applied to the surface of the hydrophilic resin layer and dried in an oven at 80° for 1 minute to obtain a specific laminate. The coating amount was set to 27 mL / m 2 .

[0414] After applying and drying the specific composition, the photosensitive resin layer-forming composition used in Example 1-1 was applied to the surface of the hydrophilic resin layer and dried in an oven at 80° for 1 minute to form a photosensitive resin layer having a thickness of 2.2 μm.

[0415] The photosensitive resin layer of the specific laminate was laminated on the copper foil side surface of the copper-attached PET film. The lamination conditions were set to a roll temperature of 100° C. and a lamination speed of 4 m / min.

[0416] The protective film on the other side was peeled off, and the hydrophilic resin composition used in Example 1-1 was applied to the surface of the exposed hydrophobic resin layer, followed by drying in an oven at 80° for 1 minute to form a hydrophilic resin layer having a thickness of 1.6 μm.

[0417] The specific composition used in Example 1-4 was applied to the surface of the hydrophilic resin layer and dried in an oven at 80° for 1 minute to obtain a specific laminate. The coating amount was set to 27 mL / m 2 .

[0418] After applying and drying the specific composition, the photosensitive resin layer-forming composition used in Example 1-1 was applied to the surface of the hydrophilic resin layer and dried in an oven at 80° for 1 minute to form a photosensitive resin layer having a thickness of 2.2 μm.

[0419] The photosensitive resin layer of the obtained specific laminate was laminated on the copper foil side surface of the copper-attached PET film. The lamination conditions were set to a roll temperature of 100° C. and a lamination speed of 4 m / min.

[0420] After laminating on the copper-bearing PET film, peeling is performed at the interface between the hydrophilic resin layer and the hydrophobic resin layer of the specific stack to obtain a specific film A (hydrophobic resin layer) having a convex structure formed on both sides of the support body and a specific film B (hydrophilic resin layer) having a concave portion formed on the surface of the copper-bearing PET film.

[0421] Hereinafter, a laminate of a support and the specific film A formed on both surfaces of the support is referred to as a film with a support.

[0422] The long diameter of the protrusion structure of the specific film A was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.08 μm to 0.24 μm, and it was confirmed that the long diameter of the protrusion structure of the specific film A was in the range of 0.08 μm to 0.24 μm. 2 There are 269 convex structures formed on the surface.

[0423] The average height of the protruding structures was measured in the same manner as in Example 1-1 and was found to be 355 μm.

[0424] The water contact angle of the surface on which the convex structures of the specific film A were formed was measured in the same manner as in Example 1-1 and was found to be 140°.

[0425] The long diameter of the concave structure of the specific film B was measured in the same manner as in Example 1-1. The result was that the long diameter was in the range of 0.08 μm to 0.29 μm, and it was confirmed that the concave structure of the specific film B was 0.08 μm to 0.29 μm. 2 The surface is formed with 400 concave structures.

[0426] The average depth of the concave structures was measured in the same manner as in Example 1-1 and found to be 126 μm.

[0427] The water contact angle of the surface on which the concave structures of the specific film B were formed was measured in the same manner as in Example 1-1 and was found to be 120°.

[0428] 《Measurement of transmittance》

[0429] The transmittance of the support-attached film composed of the support obtained in Example 2-1 and the specific film A having convex structures formed on both surfaces thereof when irradiated with light of a wavelength of 550 nm at an incident angle of 0° was measured using an ultraviolet visible spectrophotometer UV-1800 manufactured by SHIMADZU CORPORATION and is reported in Table 2.

[0430] The transmittance of the hydrophobic resin layer surface of Comparative Example 1-1 was also measured in the same manner as above, and the transmittance is shown in Table 1.

[0431] [Table 2]

[0432]

[0433] As can be seen from Tables 1 and 2, the specific films A and B obtained from the laminates produced in Examples have higher water contact angles and are superior in water repellency than the films obtained in Comparative Examples.

[0434] As can be seen from Table 1, the specific film A obtained from the laminate produced in Example 1-4 is superior in reflection suppression property compared with the hydrophobic resin layer produced in Comparative Example 1-1.

[0435] As can be seen from Table 1, the specific film B obtained from the laminated bodies produced in Examples 1-1 to 1-8 has a lower static friction coefficient with respect to glass and is excellent in lubricity than the films obtained in Comparative Examples 1-2 and 1-3.

[0436] As can be seen from Table 2, the support-attached film obtained from the laminate produced in Example 2-1 has superior reflection suppressing properties compared to the hydrophobic resin layer produced in Comparative Example 1-1.

[0437] The disclosure of Japanese Patent Application No. 2022-061220 filed on March 31, 2022 is incorporated by reference in its entirety into this specification. All documents, patent applications, and technical standards described in this specification are incorporated by reference into this specification to the same extent as if each document, patent application, and technical standard were specifically and individually described as being incorporated by reference.

Claims

1. A method for manufacturing a laminate, comprising: A step of forming a hydrophobic resin layer containing a hydrophobic resin on the surface of the support; A step of forming a hydrophilic resin layer containing a hydrophilic resin on the surface of the hydrophobic resin layer; and A step of applying a composition containing an alcohol on the surface of the hydrophilic resin layer and drying the composition to form a convex structure on the hydrophilic resin layer side surface of the hydrophobic resin layer and a concave structure on the hydrophobic resin layer side surface of the hydrophilic resin layer.

2. The method for producing a laminate according to claim 1, wherein: The total light transmittance of the support is greater than 50%.

3. The method for producing a laminate according to claim 1 or 2, wherein: The support contains a polyester resin.

4. The method for producing a laminate according to any one of claims 1 to 3, wherein: The glass transition temperature of the hydrophobic resin is lower than the glass transition temperature of the hydrophilic resin.

5. The method for producing a laminate according to any one of claims 1 to 4, wherein: The hydrophobic resin is a polyolefin resin.

6. The method for producing a laminate according to any one of claims 1 to 5, wherein: The hydrophilic resin is a (meth)acrylic resin.

7. The method for producing a laminate according to any one of claims 1 to 6, wherein: The composition also contains water.

8. A method for producing a film, comprising: A step of manufacturing a laminate by the method for manufacturing a laminate according to claim 1; and A step of performing peeling at an interface between the hydrophobic resin layer and the hydrophilic resin layer included in the laminate.

9. A membrane comprising a hydrophobic resin, The film has a convex structure with a long diameter of 0.02 μm to 5 μm and an average height of 10 nm to 3000 nm on at least one surface, and In every 10 μm 2 The surface of the device has 1 to 1000 convex structures formed thereon.

10. The film according to claim 9, wherein At 25° C., a water contact angle of the surface on which the protruding structures are formed is 100° or more.

11. The film according to claim 9 or 10, wherein When the surface having the convex structure formed thereon is irradiated with light having a wavelength of 550 nm, the reflectivity is 4% or less.

12. A film with a support, comprising a support and the film according to any one of claims 9 to 11 provided on one surface of the support, A surface of the film opposite to the surface on which the protruding structures are formed is in contact with the support.

13. The support-attached film according to claim 12, wherein: The film is disposed on both sides of the support, and The transmittance of light with a wavelength of 550 nm is 92% or more.

14. A membrane comprising a hydrophilic resin, The film has a concave structure with a long diameter of 0.02 μm to 5 μm and an average depth of 10 nm to 3000 nm on at least one surface, and In every 10 μm 2 The surface of the device has 1 to 1000 concave structures formed thereon.

15. The film according to claim 14, wherein At 25° C., the water contact angle of the surface having the concave structures formed thereon is 95° or more.

16. A photosensitive transfer material comprising, in order, a support, a hydrophobic resin layer, a hydrophilic resin layer, a water-soluble intermediate layer and a photosensitive resin layer, The hydrophobic resin layer contains a polyolefin resin, The hydrophilic resin layer contains a (meth)acrylic resin. The water-soluble intermediate layer contains a water-soluble resin. The hydrophobic resin layer and the hydrophilic resin layer can be peeled off at the interface. In the hydrophilic resin layer, every 10 μm 2 The surface of the hydrophobic resin layer has 1 to 1000 concave structures formed thereon. The long diameter of the concave structure is 0.02 μm to 5 μm, the average depth is 10 nm to 3000 nm, and The static friction coefficient of the surface with respect to glass is 1.50 or less.

Citation Information

Patent Citations

  • Synthetic polymer film and manufacturing method for the synthetic polymer film

    CN110183694A

  • Method for producing polymeric gel and the resultant polymeric gel

    JP2004263081A